A silicon-based negative electrode aqueous binder and its preparation method and application
By using polymer polymers with hydroxyl and carboxyl groups and small molecule organic acids in silicon-based anode materials to construct a crosslinking network structure, the problem of electrode instability caused by volume expansion during circulation of silicon-based anode materials is solved, and lithium is significantly improved Electrochemical properties of ion batteries.
Patent Information
- Application Number
- CN202410246067.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-05
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-03-05
AI Technical Summary
The existing silicon-based anode materials have unstable electrodes due to volume expansion during circulation, and cannot effectively interact with silicon particles, resulting in a degradation of electrochemical performance.
Using polymer polymers containing hydroxyl and carboxyl groups and small molecular organic acids as raw materials, a crosslinking network structure is constructed through covalent ester bonds and non-covalent hydrogen bonds to form a crosslinking network binder with multi-gradient energy dissipation. Preparation of silicon-based negative electrode material.
It effectively suppresses the volume expansion of the silicon negative electrode, improves the electrochemical performance of lithium-ion batteries, and improves the cycle stability and capacity retention rate of the negative electrode sheet and secondary batteries.
Smart Images

Figure CN117894990B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery materials, and more specifically relates to a silicon-based negative electrode aqueous binder and a preparation method and application thereof. Background Art
[0002] Silicon (Si) has a very high theoretical capacity (4200mAHg -1) , is the graphite negative electrode (372mAHg -1 ) and has a lower electrochemical window (~0.4 V vs Li / Li +) , so it is considered to be a very promising negative electrode material.
[0003] However, during long-term cycling, the huge density change between silicon and its discharge products leads to a huge volume expansion (~300%), which further leads to irreversible pulverization of the electrode, unstable solid electrolyte interface (SEI) and electrical contact failure between electrode materials. These negative effects ultimately lead to degradation of the negative electrode and rapid capacity loss. At present, most of the research on solving the silicon expansion problem focuses on the nano-sizing of silicon particles and the composite with carbon-based materials, and the use of efficient binders is also an effective solution.
[0004] Effective binders hold electrode particles together and support electrochemical processes in small amounts. Polyvinylidene fluoride (PVDF), a conventionally used binder, exhibits poor performance on silicon anodes due to its weak interaction with active materials and relatively high expansion rate in organic electrolytes. Therefore, many new binders have been explored.
[0005] Synthetic polymer binders represented by polyacrylic acid (PAA), polyvinyl alcohol (PVA), and polyacrylonitrile (PAN) are used in silicon anodes because of their controllable and modifiable structures. In addition, biomass polymer binders have also received great attention due to their biodegradability and natural abundance, such as sodium alginate (SA), carboxymethyl cellulose (CMC), chitosan (CS), guar gum (GG), carrageenan (KG), etc. Compared with synthetic polymer binders, biomass materials with abundant polar groups (hydroxyl, carboxyl, amino) are more likely to form a strong interaction with the Si-OH of the SiO2 layer on silicon particles, improving the structural stability of the electrode. However, the above polymers are not sufficient to accommodate huge volume changes due to their linear or branched structures, resulting in electrical isolation of silicon and the resulting unstable SEI formation. Therefore, it is necessary to find a new binder with strong interchain connections to form a robust binder network. Summary of the invention
[0006] The purpose of the present invention is to provide a silicon-based negative electrode aqueous binder and a preparation method and application thereof, to form a mutually cross-linked network structure through in-situ esterification polymerization, to provide more active sites for the silicon negative electrode and the binder, to solve the technical problem that the linear polymer binder of the existing negative electrode material cannot effectively interact with the silicon particles, to effectively inhibit the volume expansion of the silicon negative electrode during the charge and discharge cycle, and to further improve the electrochemical performance of the lithium-ion battery.
[0007] To achieve the above object, the present invention provides the following solutions:
[0008] One of the technical solutions of the present invention is to provide a silicon-based negative electrode aqueous binder, the raw materials of which include: a high molecular polymer containing hydroxyl and carboxyl groups and a small molecule organic acid.
[0009] Furthermore, the mass ratio of the high molecular weight polymer to the low molecular weight organic acid is 1-9:1-9.
[0010] Furthermore, the high molecular polymer includes at least one of guar gum, xanthan gum, sodium alginate, sodium hyaluronate and carrageenan.
[0011] Furthermore, the small molecule organic acid includes at least one of malic acid, citric acid, tartaric acid and acetic acid.
[0012] In the present invention, small molecule organic acid is used as a cross-linking agent to bridge the flexible high molecular polymer molecular chains through covalent ester bonds and non-covalent hydrogen bonds, thereby constructing a cross-linking network structure with multi-gradient energy dissipation.
[0013] The second technical solution of the present invention is to provide a method for preparing the above-mentioned silicon-based negative electrode aqueous binder, the steps comprising:
[0014] The high molecular polymer and the low molecular organic acid are uniformly dispersed in water, and then heated and stirred for reaction to obtain the silicon-based negative electrode aqueous binder.
[0015] Furthermore, the mass ratio of the total mass of the high molecular weight polymer and the small molecular weight organic acid to water is 1:9 to 1:4, preferably 1:9.
[0016] Furthermore, the temperature of the heating and stirring reaction is 60-100° C., the rotation speed is 300-800 rpm, and the time is 6-12 hours.
[0017] In the present invention, water is used as solvent, high molecular polymer and small molecular organic acid are used as solutes, and a binder is prepared by heating and stirring reaction, wherein the carboxyl group in the crosslinking agent molecule and the hydroxyl group of the water-soluble high molecular polymer are caused to form a strong covalent ester bond through heating and stirring, thereby crosslinking to the water-soluble high molecular polymer molecular chain.
[0018] The third technical solution of the present invention is to provide an application of the above-mentioned silicon-based negative electrode aqueous binder in the preparation of lithium-ion batteries.
[0019] A fourth technical solution of the present invention is to provide a negative electrode sheet, wherein the negative electrode sheet is made of a current collector and a negative electrode slurry loaded on the current collector;
[0020] The negative electrode slurry is formed by mixing the negative electrode active material, the conductive additive and the above-mentioned silicon-based negative electrode aqueous binder.
[0021] Furthermore, the negative electrode active material includes one of nano silicon particles, silicon carbon particles and silicon dioxide particles, preferably nano silicon particles.
[0022] Furthermore, the conductive additive includes one of Super P, graphene and Ketjen black, preferably Super P.
[0023] Furthermore, the mass ratio of the negative electrode active material, the conductive additive and the silicon-based negative electrode aqueous binder in the negative electrode slurry is 60-80:5-30:5-20.
[0024] A fifth technical solution of the present invention is to provide a method for preparing the above-mentioned negative electrode sheet, the steps comprising:
[0025] The negative electrode active material, the conductive additive and the silicon-based negative electrode aqueous binder are mixed uniformly, coated on the surface of the current collector, and then dried and rolled and cut to obtain the negative electrode sheet.
[0026] Furthermore, the drying temperature is 60-120° C. and the drying time is 8-16 hours.
[0027] Technical solution six of the present invention: Provide a secondary battery, including a positive electrode, a separator, an electrolyte and the above-mentioned negative electrode plate.
[0028] The present invention discloses the following technical effects:
[0029] The binder of the present invention uses a high-viscosity water-soluble high-molecular polymer and a small-molecule organic acid with high reactivity as main raw materials, provides more active sites with silicon particles through strong covalent ester bonds and reversible non-covalent hydrogen bonds, and realizes effective combination of different functional components at the molecular level. The preparation process of the cross-linked network structure binder is simple, easy to operate, low in cost, and can be mass-produced. By introducing hydroxyl, carboxyl, and esterification groups into the composite binder, stronger hydrogen bonds can be formed with the silicon oxide thin layer on the silicon surface. The hydrogen bonds are tightly combined with silicon nanoparticles to form a current collector, which can effectively reduce the volume expansion of silicon, while improving the electrochemical properties of nano-silicon, and improving the electrochemical properties of the negative electrode plate and secondary battery prepared thereby. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0031] Figure 1 The cycle stability comparison of the secondary batteries prepared in Example 1 and Comparative Example 1 is shown;
[0032] Figure 2 The cyclic voltammogram of the secondary battery prepared in Example 1;
[0033] Figure 3 XRD diagram of the negative electrode material and pure silicon prepared in Example 1;
[0034] Figure 4 The figure shows the cycle stability comparison of the secondary batteries prepared in Comparative Example 3 and Comparative Example 4. DETAILED DESCRIPTION
[0035] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0036] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0037] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0038] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0039] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0040] Example 1
[0041] Preparation of silicon-based negative electrode aqueous binder:
[0042] 0.6 g of sodium hyaluronate and 0.4 g of malic acid were added to a weighing bottle, and 9 g of water was added, and stirred at 80° C. (600 rpm) for 12 hours to allow it to fully dissolve and react, thereby obtaining a silicon-based negative electrode aqueous binder with a mass concentration of 10%.
[0043] Preparation of negative electrode sheet:
[0044] Nano silicon particles, Super P and the above-mentioned silicon-based negative electrode aqueous binder with a mass concentration of 10% are homogenized in a mass ratio of 60:30:10, the homogenized slurry is evenly applied on the copper foil, dried at 80°C for 12h under vacuum conditions, and rolled and cut to obtain the negative electrode sheet.
[0045] Preparation of secondary batteries:
[0046] The dried negative electrode sheet was moved into a glove box, and a lithium sheet was used as a counter electrode to assemble a 2016 button cell, wherein the separator was Celgard 2500, the electrolyte was composed of LiPF6 as an electrolytic salt and an EC / DMC / DEC solution with a volume ratio of 1:1:1 (the concentration of LiPF6 was 1M), and 5% by mass of FEC was added as an additive. The assembled battery was sealed and left to stand for 10 hours to obtain a secondary battery.
[0047] Example 2
[0048] Preparation of silicon-based negative electrode aqueous binder:
[0049] 0.8 g of sodium hyaluronate and 0.2 g of malic acid were added to a weighing bottle, and 9 g of water was added. The mixture was stirred at 80° C. (600 rpm) for 12 hours to allow the mixture to fully dissolve and react, thereby obtaining a silicon-based negative electrode aqueous binder with a mass concentration of 10%.
[0050] The preparation of the negative electrode is the same as in Example 1.
[0051] The preparation of the secondary battery is the same as in Example 1.
[0052] Example 3
[0053] Preparation of silicon-based negative electrode aqueous binder:
[0054] 0.2 g of sodium hyaluronate and 0.8 g of malic acid were added to a weighing bottle, and 9 g of water was added, and stirred at 80° C. (600 rpm) for 12 hours to allow it to fully dissolve and react, thereby obtaining a silicon-based negative electrode aqueous binder with a mass concentration of 10%.
[0055] The preparation of the negative electrode sheet is the same as in Example 1.
[0056] The preparation of the secondary battery is the same as in Example 1.
[0057] Example 4
[0058] Preparation of silicon-based negative electrode aqueous binder:
[0059] 0.6 g guar gum and 0.4 g citric acid were added to a weighing bottle, and 9 g water was added, and stirred at 80° C. (600 rpm) for 12 hours to allow it to fully dissolve and react, thereby obtaining a silicon-based negative electrode aqueous binder with a mass concentration of 10%.
[0060] The preparation of the negative electrode is the same as in Example 1.
[0061] The preparation of the secondary battery is the same as in Example 1.
[0062] Example 5
[0063] Preparation of silicon-based negative electrode aqueous binder:
[0064] 0.5 g of sodium hyaluronate and 0.5 g of malic acid were added to a weighing bottle, and 9 g of water was added. The mixture was stirred at 80° C. (600 rpm) for 12 hours to allow the mixture to fully dissolve and react, thereby obtaining a silicon-based negative electrode aqueous binder with a mass concentration of 10%.
[0065] The preparation of the negative electrode sheet is the same as in Example 1.
[0066] The preparation of the secondary battery is the same as in Example 1.
[0067] Example 6
[0068] Preparation of silicon-based negative electrode aqueous binder:
[0069] 0.5 g of carrageenan and 0.5 g of tartaric acid were added to a weighing bottle, and 9 g of water was added, and stirred at 80° C. (600 rpm) for 12 hours to fully dissolve and react, thereby obtaining a silicon-based negative electrode aqueous binder with a mass concentration of 10%.
[0070] The preparation of the negative electrode sheet is the same as in Example 1.
[0071] The preparation of the secondary battery is the same as in Example 1.
[0072] Example 7
[0073] Preparation of silicon-based negative electrode aqueous binder:
[0074] 0.6 g of xanthan gum and 0.4 g of acetic acid were added to a weighing bottle, and 9 g of water was added, and stirred at 80° C. (600 rpm) for 12 hours to allow it to fully dissolve and react, thereby obtaining a silicon-based negative electrode aqueous binder with a mass concentration of 10%.
[0075] The preparation of the negative electrode is the same as in Example 1.
[0076] The preparation of the secondary battery is the same as in Example 1.
[0077] Comparative Example 1
[0078] Preparation of binder:
[0079] 0.5 g of carboxymethyl cellulose and 0.5 g of styrene-butadiene rubber were added into a weighing bottle, and 9 g of water was added, and the mixture was stirred at 80° C. (600 rpm) for 12 hours to allow the mixture to fully dissolve and react, thereby obtaining a binder.
[0080] The preparation of the negative electrode is the same as in Example 1.
[0081] The preparation of the secondary battery is the same as in Example 1.
[0082] Comparative Example 2
[0083] The binder is: polyvinylidene fluoride.
[0084] The preparation of the negative electrode is the same as in Example 1.
[0085] The preparation of the secondary battery is the same as in Example 1.
[0086] Comparative Example 3
[0087] Preparation of silicon-based negative electrode aqueous binder:
[0088] 1 g of sodium hyaluronate was added to a weighing bottle, and 9 g of water was added, and stirred (600 rpm) at 80° C. for 12 hours to fully dissolve it, thereby obtaining a silicon-based negative electrode aqueous binder with a mass concentration of 10%.
[0089] The preparation of the negative electrode is the same as in Example 1.
[0090] The preparation of the secondary battery is the same as in Example 1.
[0091] Comparative Example 4
[0092] Preparation of silicon-based negative electrode aqueous binder:
[0093] 1 g of malic acid was added to a weighing bottle, and 9 g of water was added, and stirred (600 rpm) at 80° C. for 12 hours to fully dissolve the malic acid, thereby obtaining a silicon-based negative electrode aqueous binder with a mass concentration of 10%.
[0094] The preparation of the negative electrode is the same as in Example 1.
[0095] The preparation of the secondary battery is the same as in Example 1.
[0096] Test example
[0097] The secondary batteries prepared in Examples 1 to 7 and Comparative Examples 1 to 4 were subjected to constant current electrochemical performance tests on a charge and discharge tester, wherein the charge and discharge rate was 0.1C and the voltage range was 0.01 to 2V. The results are shown in Table 1.
[0098] Table 1
[0099]
[0100] From the data comparison in Table 1, it can be seen that the secondary battery prepared by the adhesive prepared by the method of the present invention has a higher initial capacity and capacity retention rate than the comparative example, especially the capacity retention rate. Among them, the secondary battery prepared by the adhesive in which sodium hyaluronate and malic acid are mixed in a ratio of 6:4 in Example 1 has the best performance.
[0101] Figure 1 The cycle stability of the secondary battery prepared in Example 1 is compared with that in Comparative Example 1. Figure 1 It can be seen that the secondary battery prepared in Example 1 has an initial discharge capacity of 3982 mAh / g, and after 100 cycles, the discharge capacity is 1949 mAh / g. The cross-linked network structure binder formed by cross-linking copolymerization of sodium hyaluronate and malic acid has a cycle performance that is significantly better than sodium carboxymethyl cellulose and styrene-butadiene rubber as silicon negative electrode binders.
[0102] The secondary battery prepared in Example 1 was subjected to a cyclic voltammetry test at a potential window of 0.01 to 2.0 V and a scan rate of 0.1 mV / s. The results are as follows: Figure 2 As shown, it has obvious redox characteristic peaks of Si lithiation and delithiation, indicating that the electrode reaction kinetics of the material is good.
[0103] Figure 3 The XRD diagram of the negative electrode material and pure silicon prepared in Example 1; Figure 3 It can be seen that the small broad peak near 22° of Si corresponds to the amorphous native oxide SiO2, and this peak of the negative electrode material prepared in Example 1 at 80°C is significantly enhanced, which is attributed to the supramolecular interaction between HM and the hydroxylated Si surface.
[0104] Figure 4 The cycle stability of the secondary batteries prepared in Comparative Example 3 and Comparative Example 4 is compared. Figure 4It can be seen that the first discharge capacities of the secondary batteries prepared in Comparative Examples 3 and 4 are 3459 mAh / g and 3544 mAh / g, respectively. After 100 cycles, the capacities are 805 mAh / g and 894 mAh / g, respectively. It can be seen that when sodium hyaluronate or malic acid is used alone as a binder, the cycle performance is lower than the effect of the combination of the two.
[0105] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0106] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A silicon-based negative electrode aqueous binder, characterized in that: The silicon-based negative electrode aqueous binder is composed of a high molecular polymer containing hydroxyl and carboxyl groups, a small molecular organic acid and water; The mass ratio of the high molecular weight polymer to the small molecular weight organic acid is 6:4; The mass ratio of the sum of the mass of the high molecular weight polymer and the small molecular weight organic acid to the mass of water is 1:9; The preparation steps of the silicon-based negative electrode aqueous binder are: After the high molecular polymer and the small molecular organic acid are uniformly dispersed in water, the silicon-based negative electrode aqueous binder is obtained after heating and stirring for reaction; The heating and stirring reaction was performed at a temperature of 80°C, a rotation speed of 600 rpm, and a time of 12 h; The high molecular polymer is sodium hyaluronate; the low molecular organic acid is malic acid.
2. A method for preparing a silicon-based negative electrode aqueous binder as claimed in claim 1, characterized in that the steps include: After the high molecular polymer and the small molecular organic acid are uniformly dispersed in water, the silicon-based negative electrode aqueous binder is obtained after heating and stirring for reaction; The mass ratio of the total mass of the high molecular polymer and the small molecular organic acid to water is 1:9; the temperature of the heating and stirring reaction is 80° C., the rotation speed is 600 rpm, and the time is 12 hours.
3. Use of the silicon-based negative electrode aqueous binder as claimed in claim 1 in the preparation of lithium-ion batteries.
4. A negative electrode plate, characterized in that: The negative electrode sheet is made of a current collector and a negative electrode slurry loaded on the current collector; The negative electrode slurry is formed by mixing a negative electrode active material, a conductive additive and the silicon-based negative electrode aqueous binder according to claim 1; The negative electrode active material comprises one of nano silicon particles, silicon carbon particles and silicon dioxide particles; The conductive additive includes one of Super P, graphene and Ketjen black.
5. The negative electrode sheet according to claim 4, characterized in that: The mass ratio of the negative electrode active material, the conductive additive and the silicon-based negative electrode aqueous binder in the negative electrode slurry is 60-80:5-30:5-20.
6. A method for preparing a negative electrode sheet as claimed in claim 4 or 5, characterized in that the steps include: The negative electrode active material, the conductive additive and the silicon-based negative electrode aqueous binder are mixed uniformly, coated on the surface of the current collector, dried, rolled and cut to obtain the negative electrode sheet.
7. The preparation method according to claim 6, characterized in that: The drying temperature is 60-120° C. and the drying time is 8-16 hours.
8. A secondary battery, characterized in that: It comprises a positive electrode, a separator, an electrolyte and the negative electrode sheet as claimed in claim 4 or 5.
Citation Information
Patent Citations
Compound binding agent and application thereof as well as lithium-ion battery negative electrode material prepared based on compound binding agent and preparation method
CN108461728A
Aqueous binder, lithium ion battery silicon-based negative electrode and preparation method of lithium ion battery silicon-based negative electrode
CN114665094A
Silicon negative electrode binder as well as preparation method and application thereof
CN116470054A