Negative pole piece with artificially constructed SEI film and preparation method and application of negative pole piece

The phospholipid vesicles coated with organic solid electrolyte coating combined with anionic polymer complex, which solves the problem of unstable SEI film of silicon-based anode, forms a solid electrode protective layer, and improves the interface of lithium batteries Stability and cycle efficiency extend battery life.

CN119050272APending Publication Date: 2024-11-29LIONGO (CHANGZHOU) NEW ENERGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411148036.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The unstable SEI film of silicon-based anode in lithium-ion batteries causes the electrode surface to rupture, reducing the service life and efficiency of the battery. The existing methods for building high-performance SEI films have problems such as high cost or difficulty in industrialization.

Method used

The organic solid electrolyte coating layer is used to combine silicon anode material coated by phospholipid vesicles and anionic polymer complex to form a stable SEI film, through the multiple forces of phospholipid vesicles and silicon oxide particles and anionic polymer. The combination of polar groups and Li+ creates a solid electrode protective layer.

Benefits of technology

It improves the interface stability and cycling efficiency of lithium batteries, extends the battery life, reduces the volume expansion and side reactions of lithium electrodes, and enhances the thermal stability and mechanical strength of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005003060180000231
    Figure BDA0005003060180000231
Patent Text Reader

Abstract

The invention provides a negative pole piece with an artificially constructed SEI film. The negative pole piece comprises a negative current collector; the first coating is compounded on the surface of the negative electrode current collector and comprises a silicon negative electrode material coated by phospholipid vesicles; a second coating composited to the first coating, the second coating comprising an anionic polymer complex; and the organic solid electrolyte coating layer is compounded on the second coating. The silicon substrate with the artificially constructed SEI film provided by the invention is applied as a negative pole piece, a protective layer can be formed outside silicon negative pole material particles, and the effects of buffering volume expansion and preventing an active material from being in contact with an electrolyte are achieved, so that the stability of silicon monoxide can be ensured, and meanwhile, more active lithium is ensured to be removed, and more reversible capacity is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to an artificially constructed SEI film and a preparation method and application thereof. Background Art

[0002] With the rapid development of electric vehicles, portable devices, and various flexible wearable devices, the demand for battery energy with lighter weight, smaller size, higher output voltage and energy density continues to expand. The energy density of commercial lithium-ion batteries with graphite as negative electrodes cannot fully meet the emerging market demand. Lithium metal batteries (LMBs), which were once hindered by the limitations of liquid electrolytes, have turned around with the breakthrough of solid electrolytes. Silicon-based negative electrode materials have high theoretical specific capacity (4200mAh / g at high temperature, 3580mAh / g at room temperature), low delithiation potential (<0.5V), environmental friendliness, and abundant reserves. Therefore, high-voltage LMBs with high energy density positive electrode materials have extremely high theoretical energy density and are ideal power devices for current electronic devices.

[0003] However, as the negative electrode of the battery, the unstable SEI film during the charge and discharge process of silicon leads to a series of domino effects: the huge changes in the surface and surface stress during the deintercalation of the silicon-based negative electrode cause the SEI film formed on the negative electrode surface to break continuously, while the exposed surface continuously forms a new SEI film, and the SEI film breaks and regenerates continuously, resulting in the continuous increase in the thickness of the SEI film. The lithium source in the electrolyte and the positive electrode is constantly reduced, resulting in low first coulomb efficiency, low conductivity and high Li + Transmission resistance. Therefore, the service life of lithium batteries can be improved by constructing a stable SEI film. At present, there are two main ways to construct high-performance SEI: (1) adding functional additives; carbonate additives are easy to produce gas, and S-containing additives are expensive and difficult to industrialize. (2) Constructing artificial SEI membranes, such as inorganic conductive composites, thin films, and carbon materials, to isolate the side reactions between the electrode and the electrolyte. Although the artificial SEI layer has good electronic conductivity and good chemical stability, it is easily broken by the expansion of the silicon base during the cycle. By constructing a higher specific surface area to buffer the volume expansion of the silicon-based negative electrode and effectively avoid structural collapse, it is an effective means to establish a stable artificial SEI membrane. At the same time, as the cycle progresses, the repeated rupture and formation of the SEI membrane consumes a large amount of active lithium ions, which will reduce the charge and discharge efficiency of the electrode material. In addition, the SEI membrane is unstable and easy to decompose during high-temperature storage, and rupture and growth will occur. It is necessary to develop a stable artificial SEI membrane to improve the interface stability of the silicon negative electrode. Summary of the invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide a negative electrode plate with an artificially constructed SEI film, a preparation method thereof and an application thereof. The negative electrode plate with an artificially constructed SEI film provided by the present invention has excellent interface stability.

[0005] The present invention provides a negative electrode sheet with an artificially constructed SEI film, comprising:

[0006] Anode current collector;

[0007] A first coating layer composited on the surface of the negative electrode current collector, wherein the first coating layer comprises a silicon negative electrode material coated with phospholipid vesicles;

[0008] A second coating layer composited with the first coating layer, wherein the second coating layer comprises an anionic polymer complex;

[0009] An organic solid electrolyte coating layer is compounded on the second coating layer.

[0010] Preferably, the method for preparing the phospholipid vesicles comprises the following steps:

[0011] 1) preparing an organic solution containing phospholipids;

[0012] 2) After removing the organic solvent in the organic solution, a layer of phospholipid dry film is obtained;

[0013] 3) The phospholipid dry film is hydrated to obtain phospholipid vesicles.

[0014] Preferably, the phospholipid is selected from one or more of phosphatidylcholine, phospholipid glyceride, dioleylphosphatidylcholine, and dioleylphosphatidylglycerol;

[0015] The mass percentage of the phospholipid in the silicon negative electrode material is 20% to 50%;

[0016] The organic solvent used to prepare the organic solution containing phospholipids is selected from one or more of n-hexane, dichloromethane and chloroform;

[0017] The hydration is performed using a buffer solution, wherein the buffer solution is selected from PBS or Tris-HCl; the PBS is a sodium dihydrogen phosphate-disodium hydrogen phosphate aqueous solution with a pH of 7.4; the Tris-HCl is a trimethylammonium hydrochloride-hydrochloric acid aqueous solution with a pH of 7.5.

[0018] The hydration temperature is 50-80° C. and the hydration time is 2-6 hours.

[0019] Preferably, the silicon negative electrode material is selected from silicon monoxide SiO x , where 0 <x<2;

[0020] Preferably, the silicon oxide comprises: nano silicon oxide particles with a particle size of less than 1.2 nm and nano silicon oxide particles with a particle size of more than 22 nm;

[0021] Preferably, nano-silicon oxide particles with a particle size of less than 1.2 nm account for 5-10% of the total mass of silicon oxide, and nano-silicon oxide particles with a particle size of more than 22 nm account for 90-95% of the total mass of silicon oxide.

[0022] Preferably, the method for preparing the silicon negative electrode material coated with phospholipid vesicles comprises the following steps:

[0023] 1) dissolving phospholipid vesicles, stabilizer and silicon negative electrode material in a solvent to form solution A;

[0024] 2) dissolving the emulsifier in the buffer solution to prepare solution B;

[0025] 3) Mixing solution A and solution B and stirring to obtain a reaction solution;

[0026] 4) washing, centrifuging and drying the reaction solution to obtain a silicon negative electrode material coated with phospholipid vesicles.

[0027] Preferably, the stabilizer is selected from one or more of cholesterol, stearic acid and sphingomyelin, and the added amount is 20% to 50% of the amount of phospholipids;

[0028] The selected emulsifier is one or more of Tween-80, Tween-20, Tween-40 and Tween-60;

[0029] In step 3), the mixing and stirring temperature is 40 to 80° C. and the time is 1 to 5 hours.

[0030] Preferably, the first coating layer further includes a conductive agent and a binder.

[0031] Preferably, the conductive agent is selected from one or more of graphite, carbon black, and activated carbon;

[0032] The binder is selected from one or more of polyvinylidene fluoride, polyacrylic acid, styrene-butadiene rubber, and hydroxypropyl methylcellulose;

[0033] The mass ratio of the silicon negative electrode material coated by the phospholipid vesicles, the conductive agent and the binder is 85-95:2-5:2-5.

[0034] Preferably, the preparation method of the anionic polymer complex comprises the following steps:

[0035] mixing anionic polymer, lithium salt and water to react and obtain a reaction product;

[0036] The reaction product is centrifuged and then dried to obtain the anionic polymer complex.

[0037] Preferably, the anionic polymer is one or more of sodium polystyrene sulfonate, sodium carboxymethyl cellulose and sodium polyacrylate;

[0038] The lithium salt is one or more of LiCl, LiBr, LiI, LiNO3, Li3PO4, and LiC2H3O2.

[0039] Preferably, the second coating layer further includes a conductive agent and a binder.

[0040] Preferably, the conductive agent is one or more of graphite, carbon black, and activated carbon;

[0041] The binder is selected from one or more of polyvinylidene fluoride, polyacrylic acid, styrene-butadiene rubber, and hydroxypropyl methylcellulose;

[0042] The mass ratio of the anionic polymer complex, the conductive agent and the binder is 90-95:2-5:2-5.

[0043] Preferably, the thickness of the first coating is 0.02 to 150 μm;

[0044] The thickness of the second coating is 0.02 to 12 μm;

[0045] The thickness of the organic solid electrolyte coating layer is 0.1-5 μm.

[0046] The present invention also provides a method for preparing the above-mentioned negative electrode sheet, comprising the following steps:

[0047] A) mixing a silicon negative electrode material coated with phospholipid vesicles, a conductive agent, a binder and a solvent to obtain a first coating slurry;

[0048] Applying the first coating slurry on the surface of the current collector and drying it to obtain a pole piece composited with the first coating;

[0049] B) mixing the anionic polymer complex, the conductive agent, the binder and the solvent to obtain a second coating slurry;

[0050] Applying the second coating slurry to the surface of the electrode composited with the first coating, and drying the electrode composited with the first coating and the second coating to obtain the electrode composited with the first coating;

[0051] C) placing the electrode sheet having the first coating layer and the second coating layer on the surface of the substrate, placing the electrode sheet in a sealed container containing ammonium carbonate, and heating the electrode sheet at a certain temperature for a period of time to obtain an organic solid electrolyte coated silicon-based negative electrode sheet.

[0052] Preferably, in step A) and step B), the solvent is selected from NMP and water;

[0053] In step C), the heating temperature is 40 to 100° C. and the heating time is 1 to 4 hours.

[0054] The present invention also provides a secondary battery, comprising the above-mentioned negative electrode plate.

[0055] Compared with the prior art, the present invention provides a negative electrode sheet with an artificially constructed SEI film, comprising: a negative electrode current collector; a first coating compounded on the surface of the negative electrode current collector, the first coating comprising a silicon negative electrode material coated with phospholipid vesicles; a second coating compounded on the first coating, the second coating comprising an anionic polymer complex; and an organic solid electrolyte coating layer compounded on the second coating. The silicon substrate with an artificially constructed SEI film provided by the present invention is applied as a negative electrode sheet, which can form a protective layer outside the silicon negative electrode material particles, buffering volume expansion and preventing the contact between the active material and the electrolyte, thereby ensuring the stability of silicon oxide, while ensuring the release of more active lithium and obtaining more reversible capacity. DETAILED DESCRIPTION

[0056] The present invention provides a negative electrode sheet with an artificially constructed SEI film, comprising:

[0057] Anode current collector;

[0058] A first coating layer composited on the surface of the negative electrode current collector, wherein the first coating layer comprises a silicon negative electrode material coated with phospholipid vesicles;

[0059] A second coating layer composited with the first coating layer, wherein the second coating layer comprises an anionic polymer complex;

[0060] An organic solid electrolyte coating layer is compounded on the second coating layer.

[0061] The negative electrode sheet with artificially constructed SEI film provided by the present invention comprises a negative electrode current collector. In the present invention, the negative electrode current collector is selected from copper foil.

[0062] The negative electrode plate with artificially constructed SEI film provided by the present invention also includes a first coating compounded on the surface of the negative electrode current collector, and the first coating includes a silicon negative electrode material coated with phospholipid vesicles.

[0063] In the present invention, the phospholipid vesicle is composed of a single-layer phospholipid structure. The preparation method of the phospholipid vesicle comprises the following steps:

[0064] 1) preparing an organic solution containing phospholipids;

[0065] 2) After removing the organic solvent in the organic solution, a layer of phospholipid dry film is obtained;

[0066] 3) The phospholipid dry film is hydrated to obtain phospholipid vesicles.

[0067] Specifically, the phospholipid is mixed with an organic solvent to obtain an organic solution containing phospholipids. The phospholipid is selected from one or more of phosphatidylcholine (PC), phosphatidylglycerol (PG), dioleylphosphatidylcholine (DOPC), and dioleylphosphatidylglycerol (DOPG). The organic solvent used to prepare the organic solution containing phospholipids is selected from one or more of n-hexane, dichloromethane and chloroform. The ratio of the phospholipid to the organic solvent is 1-4g: (50-200)ml, which can be 1g: 50ml, 1g: 100ml, 1g: 150ml, 1g: 200ml, 2g: 50ml, 3g: 50ml, 4g: 50ml, or any value between 1-4g: (50-200)ml.

[0068] The mass percentage of the phospholipid to the silicon negative electrode material is 20% to 50%, and can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, or any value between 20% and 50%.

[0069] Next, after removing the organic solvent from the organic solution, a layer of phospholipid dry film is obtained. In the present invention, preferably, a rotary evaporation method is used to form a layer of phospholipid film on the wall of the rotary evaporator, and then it is dried with a protective atmosphere and then vacuum dried to obtain a layer of phospholipid dry film. The protective atmosphere is preferably nitrogen or argon.

[0070] Then, the phospholipid dry film is hydrated to obtain phospholipid vesicles. In the present invention, a buffer solution is selected for hydration to ensure uniform dispersion in the buffer solution, thereby forming a liposome structure, followed by vortexing and standing to precipitate the solution completely. The upper phase is transferred into a centrifuge tube containing a certain amount of cell buffer solution for centrifugation, and phospholipid vesicles can be obtained in the lower solution. In the buffer solution, phosphate buffer (PBS) and tris-hydroxymethylaminomethane hydrochloride (Tris-HCl buffer) are selected. The ratio of the phospholipid dry film to the buffer solution is 0.2-0.8g: (50-200)ml. The hydration temperature is 50-80°C, which can be 50, 55, 60, 65, 70, 75, 80, or any value between 50-80°C, and the time is 2-6h, which can be 2, 3, 4, 5, 6, or any value between 2-6h.

[0071] In the present invention, the method for preparing the silicon negative electrode material coated with phospholipid vesicles comprises the following steps:

[0072] 1) dissolving phospholipid vesicles, stabilizer and silicon negative electrode material in a solvent to form solution A;

[0073] 2) dissolving the emulsifier in the buffer solution to prepare solution B;

[0074] 3) Mix solution A and solution B with stirring to obtain a reaction solution;

[0075] 4) Wash, centrifuge and dry the reaction solution to obtain a silicon negative electrode material coated with phospholipid vesicles.

[0076] Specifically, in the present invention, phospholipid vesicles, a stabilizer and a silicon negative electrode material are dissolved in a solvent to form solution A. Among them, the stabilizer is selected from one or more of cholesterol, stearic acid and sphingomyelin, and the addition amount is 20% - 50% of the mass of phospholipids, which can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, or any value between 20% and 50%.

[0077] The silicon negative electrode material is selected from silicon suboxide SiOx, where 0 < x < 2, and x can be 0.2, 0.5, 0.8, 1, 1.5.

[0078] Dissolve an emulsifier in a buffer solution to prepare solution B. The selected emulsifier is polysorbate 80 (Tween - 80), polysorbate 20 (Tween - 20), polysorbate 40 (Tween - 40) or polysorbate 60 (Tween - 60). The buffer solution is selected from PBS (pH 7.4) or Tris - HCl (pH 7.5). The ratio of the emulsifier to the buffer solution is 40 - 100 ml: 20 - 80 ml.

[0079] Mix solution A and solution B with stirring to obtain a reaction solution. Preferably, inject solution A into solution B and stir at a certain temperature. Among them, the temperature of mixing and stirring is 40 - 80 °C, which can be 40, 45, 50, 55, 60, 65, 70, 75, 80, or any value between 40 - 80 °C, and the time is 1 - 5 h, which can be 1, 2, 3, 4, 5, or any value between 1 - 5 h.

[0080] Finally, wash the reaction solution several times with a buffer solution to remove free phospholipid vesicles, centrifuge and then dry in a vacuum freeze dryer to obtain a silicon negative electrode material coated with phospholipid vesicles.

[0081] In the present invention, amphoteric phospholipids are selected to coat silicon suboxide. The monolayer phospholipid vesicles have high stability and can be evenly distributed on the surface of silicon suboxide, increasing the specific surface area and stability of the material surface, reducing its dissolution and decomposition in the electrolyte, thereby contributing to the formation of a more stable SEI film. At the same time, the interactions between silicon suboxides of different sizes and the lipid membrane are also different. Nano - silicon suboxide particles with a particle size < 1.2 nm can better penetrate into the lipid membrane and do not damage the membrane structure; particles with a particle size between 1.2 - 22 nm will form pores when penetrating the lipid membrane; nano - silicon suboxide particles with a particle size > 22 nm will be firmly wrapped by the lipid membrane.

[0082] Therefore, the present invention selects nano silicon oxide particles with a particle size of less than 1.2nm and nano silicon oxide particles with a particle size of more than 22nm, so that the role of silicon oxide can be better played. Among them, silicon oxide with a particle size of less than 1.2nm accounts for 5-10% of the total mass of silicon oxide, and silicon oxide with a particle size of more than 22nm accounts for 90-95% of the total mass of silicon oxide, wherein the particle size range of the nano silicon oxide particles with a particle size of more than 22nm is preferably greater than 22nm and ≤200nm.

[0083] The microstructure of the membrane is changed through the interaction between phospholipids and silicon oxide, thereby ensuring better adsorption and stabilizing the structure of the active material.

[0084] In the present invention, the first coating layer includes a silicon negative electrode material coated with phospholipid vesicles, and also includes a conductive agent and a binder.

[0085] Wherein, the conductive agent is selected from one or more of graphite, carbon black, and activated carbon;

[0086] The binder is selected from one or more of polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), styrene-butadiene rubber (SBR), and hydroxypropyl methylcellulose (HPMC);

[0087] The mass ratio of the silicon negative electrode material coated with phospholipid vesicles, the conductive agent and the binder is 85-95:2-5:2-5, and can be 90:5:5, 91:4:5, 92:3:5, 92:4:4, 93:2:5, 93:3:4, 93:4:3, 94:2:4, 94:3:3, 95:2:3, 95:3:2, or any value between 90-95:2-5:2-5.

[0088] The negative electrode plate with artificially constructed SEI film provided by the present invention further comprises a second coating layer compounded with the first coating layer, and the second coating layer comprises an anionic polymer complex.

[0089] Wherein, the preparation method of the anionic polymer complex comprises the following steps:

[0090] mixing anionic polymer, lithium salt and water to react and obtain a reaction product;

[0091] The reaction product is centrifuged and then dried to obtain the anionic polymer complex.

[0092] Specifically, a certain mass fraction of anionic polymer solution is prepared with deionized water, the mass fraction is 2% to 10%, which can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any value between 2% and 10%, and then a certain amount of metal lithium salt (Li +represents) solution, making the metal Li + Exchange with the cations in the anionic polymer to obtain Li + The anionic polymer solution is centrifuged and dried in a vacuum dryer to obtain an anionic polymer complex. The mass ratio of lithium salt to anionic polymer is 1:50.

[0093] Wherein, the anionic polymer is one or more of sodium polystyrene sulfonate (PSS), sodium carboxymethyl cellulose (CMC) and sodium polyacrylate (PAAS);

[0094] The lithium salt is one or more of lithium chloride (LiCl), lithium bromide (LiBr), lithium iodide (LiI), lithium nitrate (LiNO3), lithium phosphate (Li3PO4), and lithium acetate (LiC2H3O2).

[0095] In the present invention, the second coating layer further includes a conductive agent and a binder. The conductive agent is any one or at least two of graphite, carbon black, and activated carbon; the binder is any one or at least one of PVDF, PAA, SBR, and HPMC; the mass ratio of the anionic polymer complex, the conductive agent, and the binder is 90-95:2-5:2-5, and can be 90:5:5, 91:4:5, 92:3:5, 92:4:4, 93:2:5, 93:3:4, 93:4:3, 94:2:4, 94:3:3, 95:2:3, 95:3:2, or any value between 90-95:2-5:2-5.

[0096] In the present invention, the thickness of the first coating layer is 0.02 to 150 μm, and can be 0.02, 0.05, 0.08, 0.1, 0.15, 0.2, 0.5, 0.8, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, or any value between 0.02 and 150 μm;

[0097] The thickness of the second coating is 0.02 to 12 μm, 0.02, 0.05, 0.08, 0.1, 0.3, 0.5, 0.8, 1.0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, or any value between 0.02 and 12 μm.

[0098] The negative electrode plate with artificially constructed SEI film provided by the present invention also includes an organic solid electrolyte coating layer compounded with the second coating layer.

[0099] The organic solid electrolyte coating layer is a long-chain polymer, preferably an ether polymer and a vinyl polymer, more preferably one or more of polyethylene oxide, polypropylene oxide, polyvinylidene fluoride, polyethylene glycol, and polyethylene glycol diacrylate, with a molecular weight of 5000-200000.

[0100] The thickness of the organic solid electrolyte coating layer is 0.1-5 μm, and can be 0.1, 0.3, 0.5, 0.7, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, or any value between 0.1-5 μm.

[0101] In addition to the formation of SEI film in the first cycle of silicon oxide negative electrode materials, a large amount of irreversible phase (Li2O and Li2CO3) is formed, which further aggravates the loss of active lithium. The present invention uses lithium carbonate to form an inorganic film on the negative electrode silicon base surface to increase the active lithium content of the entire battery. This structure not only protects the internal silicon oxide structure, but also enhances the bonding performance of the pole piece, so that no active material falls off the pole piece after the cycle. Secondly, Li2CO3 also plays a buffering role in the cycle process and maintains the stability of the SEI film, effectively accommodating Li + The problem of volume change during the deintercalation process.

[0102] The present invention uses a single layer of phospholipids to make vesicles to coat the negative electrode silicon dioxide. This biofilm is coated on the surface of silicon dioxide by chemical deposition, which can effectively inhibit the occurrence of side reactions on the electrode surface and stabilize the structure of the active material. Then a second layer containing Li + The polymer slurry will finally be passed through the CO3 2- The ammonium salt reaction is used to obtain a silicon-based electrode coated with an organic solid electrolyte. The organic / inorganic coating layer is used to improve the thermal stability and mechanical strength of the surface of the silicon negative electrode material, improve the ionic conductivity of the artificial SEI membrane interface, and ensure the cycle stability and energy density of the lithium battery.

[0103] The present invention also provides a method for preparing a negative electrode sheet, comprising the following steps:

[0104] A) mixing a silicon negative electrode material coated with phospholipid vesicles, a conductive agent, a binder and a solvent to obtain a first coating slurry; wherein the solvent is selected from N-methylpyrrolidone (NMP) and water;

[0105] Applying the first coating slurry on the surface of the current collector and drying it to obtain a pole piece composited with the first coating;

[0106] B) mixing an anionic polymer complex, a conductive agent, a binder and a solvent to obtain a second coating slurry; wherein the solvent is selected from N-methylpyrrolidone (NMP) and water;

[0107] Applying the second coating slurry to the surface of the electrode composited with the first coating, and drying the electrode composited with the first coating and the second coating to obtain the electrode composited with the first coating;

[0108] C) placing the electrode sheet with the first coating and the second coating on the surface of the substrate, placing it in a sealed container containing ammonium carbonate, and heating it at a certain temperature for a period of time to obtain an organic solid electrolyte coated silicon-based negative electrode sheet. The heating temperature is 40 to 100°C, and can be 40, 50, 60, 70, 80, 90, 100, or any value between 40 and 100°C, and the heating time is 1 to 4 hours, and can be 1, 2, 3, 4, or any value between 1 to 4 hours.

[0109] The present invention uses Li + PSS anionic polymer and CO3 2- The ammonium salt reaction obtains the PSS-Li2CO3 coated silicon pole piece, so that the artificial SEI film has good mechanical properties, good flexibility and wettability, and finally ensures the stability of the film. The present invention uses the gas phase diffusion method to reduce the reaction rate of generating Li2CO3, so that the generated Li2CO3 is evenly distributed, so that it has better thermal stability and mechanical strength.

[0110] The present invention also provides a secondary battery, comprising the above-mentioned negative electrode plate. The secondary battery also comprises a positive electrode plate, a separator and an electrolyte.

[0111] The present invention has no particular limitation on the specific types of the positive electrode plate, separator and electrolyte, and any type known to those skilled in the art may be used.

[0112] In some specific embodiments of the present invention, the positive electrode material in the positive electrode plate is preferably one of lithium iron phosphate, lithium iron manganese phosphate, lithium manganese phosphate, lithium cobalt phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel manganese oxide and lithium-rich layered oxide.

[0113] The separator is preferably one of polypropylene (PP) and polyethylene (PE).

[0114] The electrolyte is preferably a mixed solution of LiPF6 with a concentration of 1 mol / L and an organic solvent, wherein the organic solvent is selected from a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC), and the volume ratio of EC to MC is 1:2.

[0115] The present invention constructs a multi-layer protective film based on the negative electrode silicon based on the biofilm, so that it has a high specific surface area and effectively inhibits its volume expansion. An artificial SEI film with high ionic conductivity, certain flexibility, high wettability and stability is formed on its surface, thereby improving the performance of the battery when charged to a higher voltage.

[0116] The present invention has the following beneficial effects:

[0117] 1. The present invention prepares an artificial SEI membrane, in which a phospholipid coating is obtained on the surface of silicon dioxide nanoparticles, and the two together constitute a strong electrode. The phospholipids with phospholipid roots and glycerol have multiple forces with mesoporous silicon dioxide, which makes the electrode have strong mechanical properties. In addition to the binder, the silicon dioxide phospholipid layer also plays the role of a protective layer, which can buffer the volume change of silicon dioxide and prevent oxidation and corrosion on the surface of the current collector, and can inhibit the side reaction between the negative electrode material and the electrolyte, thereby improving the battery cycle stability and cycle efficiency.

[0118] 2. The present invention prepares an artificial SEI film, in which the silicon oxide coating can be used as a buffer layer, thereby improving the structural stability of the electrode and protecting the internal silicon oxide from being crushed.

[0119] 3. The present invention prepares an artificial SEI film, in which the PSS in the second coating contains abundant polar groups, which will react with the Li + Combined with each other to build a uniform Li + The diffusion layer can initiate the formation of in-situ SEI during the electroplating / stripping process, and interact with the solvent molecules in the electrolyte to form hydrogen bonds or van der Waals forces, thereby improving the wettability and compatibility of the interface.

[0120] 4. The present invention prepares an artificial SEI film, in which the three-layer multi-film on the surface of silicon oxide has excellent chemical stability, heat resistance and mechanical strength, improves the cycle performance of the negative electrode material at high temperature, reduces the problems of capacity attenuation and life shortening, short circuit and thermal runaway

[0121] 5. The present invention prepares an artificial SEI film, in which the lithium carbonate formed on the surface of silicon oxide increases the active lithium content of the entire battery. This structure not only protects the internal silicon oxide structure, but also enhances the bonding performance of the pole piece, so that no active material falls off the pole piece after the cycle. Secondly, Li2CO3 also plays a buffering role in the cycle process and maintains the stability of the SEI film, effectively accommodating Li + The problem of volume change during the embedding and de-embedding process.

[0122] In summary, the present invention provides a slurry with coating functionality and establishes an artificial SEI film, which has high ionic conductivity, certain flexibility, wettability and thermal stability. When the silicon-based pole piece prepared by the present invention is used in lithium batteries, it can slow down the volume expansion of negative silicon oxide, improve the initial storage efficiency, make the lithium electrode have obvious stability, and thus prolong the Li +The cycle life of the battery; the biggest difference between the present invention and other silicon oxide negative electrode materials is that the silicon oxide coated with a single layer of phospholipids is established, and the silicon oxide forms a solid electrode, providing sufficient buffer space to avoid "complete cracking" and "powder loss", thereby improving the cycle stability and cycle efficiency of the lithium battery. In addition, the negative electrode material prepared by the present invention with an artificial SEI film is more stable than other negative electrode silicon oxides, and the multiple protective films constructed by the organic solid electrolyte coating help to improve the effective interface contact with the negative electrode electrolyte, thereby constructing a uniform Li + Diffusion layer, to achieve good interface ion conduction. This is rarely available in other artificially constructed SEI membranes, so the artificial SEI membrane prepared by the present invention can achieve multiple technical effects in lithium battery applications.

[0123] In order to further understand the present invention, the negative electrode sheet with an artificially constructed SEI film provided by the present invention, its preparation method and application are described below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0124] Example 1

[0125] 1. Material preparation

[0126] 1. Weigh 2.53g PC and dissolve it in 50ml chloroform to obtain PC solution. Then form a phospholipid film on the wall of the rotary evaporator with the PC solution, blow it dry with argon gas, and dry it in a vacuum drying oven for 12h to prepare a phospholipid dry film. Then add 50ml PBS (pH7.4) at 60℃ for hydration for about 2h, vortex, and let it stand until the solution is completely precipitated. Transfer the upper phase into a centrifuge tube containing 10ml PBS (pH7.4) for centrifugation, and phospholipid vesicles can be obtained in the lower solution.

[0127] 2. Dissolve the phospholipid vesicles obtained in step 1, 0.64 g of cholesterol and 10 g of silica (nano silica particles with a particle size of less than 1.2 nm account for 5%, and nano silica particles with a particle size greater than 22 nm and ≤ 200 nm account for 95%) in 200 ml of ethanol to form solution A. Dissolve 27.6 ml of Tween-80 in 18.6 ml of PBS (pH 7.4) to prepare solution B. Inject solution A into solution B and stir at 55°C for 2 hours. Finally, wash the sample three times with PBS (pH 7.4) to remove free vesicles. After centrifugation, dry it in a vacuum freeze dryer to obtain vesicle-coated silica.

[0128] 3. The first coating layer contains vesicle-coated silicon oxide, a conductive agent, and a binder, wherein the conductive agent is carbon black and the binder is PVDF. In the first coating layer, the mass fraction of vesicle-coated silicon oxide is 95%, the mass fraction of carbon black is 3%, and the mass fraction of PVDF is 2%.

[0129] 4. Prepare 2.5% CMC solution with deionized water, then add 1.8g of lithium iodide to the CMC solution to obtain a solution containing Li + The CMC solution was centrifuged and dried in a vacuum dryer to obtain a CMC complex, referred to as CL.

[0130] 5. The second coating contains CL: conductive agent: binder, where the conductive agent is carbon black and the binder is PVDF. In the second coating, the mass fraction of PL is 93%, the mass fraction of carbon black is 5%, and the mass fraction of PVDF is 2%.

[0131] 2. Negative electrode current collector coating

[0132] 1. According to the formula in step 3, the prepared vesicle-coated silicon dioxide, carbon black, PVDF and NMP are mixed to obtain a first coating slurry. The first coating slurry is coated on a copper foil current collector using a coating machine and dried.

[0133] 2. Mix CL, carbon black, PVDF agent and NMP according to the formula in step 5 to obtain a second coating slurry. Use a coating machine to apply the second coating slurry to the surface of the electrode sheet containing the first coating and dry it. After drying, roll pressing, slitting and spot welding are performed to prepare a silicon-containing negative electrode sheet, wherein the single-sided thickness of the first coating is 40 μm, and the single-sided thickness of the second coating is 3 μm.

[0134] 3. Organic solid electrolyte coated silicon substrate

[0135] The silicon electrode sheet containing the first coating and the second coating was spread flat on glass, placed in a sealed container containing ammonium carbonate, and then heated at 70°C for 1.5 hours to react, thereby obtaining a CMC-Li2CO3-coated silicon-based negative electrode sheet.

[0136] Example 2

[0137] 1. Material preparation

[0138] 1. Weigh 3.27g PG and dissolve it in 80ml n-hexane to obtain PG solution. Then form a layer of phospholipid film on the wall of the rotary evaporator with the PG solution, blow it dry with argon gas, and dry it in a vacuum drying oven for 12 hours to prepare a phospholipid dry film. Then add 60ml of PBS (pH7.4) at 60°C for hydration. The hydration time is about 3.5h, vortex, and let it stand until the solution is completely precipitated. Transfer the upper phase into a centrifuge tube containing 20ml PBS (pH7.4) for centrifugation. Phospholipid vesicles can be obtained in the lower solution.

[0139] 2. Dissolve the phospholipid vesicles obtained in step 1, 0.98 g of sphingomyelin and 10 g of silica (nano-silica particles with a particle size of less than 1.2 nm account for 10%, and nano-silica particles with a particle size greater than 22 nm and ≤ 200 nm account for 90%) in 500 ml of ethanol to form solution A. Dissolve 35 ml of Tween-20 in 23 ml of PBS (pH 7.4) to prepare solution B. Inject solution A into solution B and stir at 60°C for 3 hours. Finally, wash the sample three times with PBS (pH 7.4) to remove free vesicles. After centrifugation, dry it in a vacuum freeze dryer to obtain vesicle-coated silica.

[0140] 3. The first coating contains vesicle-coated silicon oxide, a conductive agent, and a binder, wherein the conductive agent is graphite and the binder is PVDF. In the first coating, the mass fraction of vesicle-coated silicon oxide is 96%, the mass fraction of graphite is 2%, and the mass fraction of SBR is 2%.

[0141] 4. Prepare a 4.5% PAAS solution with deionized water, then add 3.3 g of lithium nitrate to the PAAS solution to obtain a PAAS solution containing Li+, centrifuge and dry in a vacuum dryer to obtain a PAAS complex, referred to as PAL.

[0142] 5. The second coating contains PAL: conductive agent: binder, where the conductive agent is graphite and the binder is SBR. In the second coating, the mass fraction of PAL is 93.5%, the mass fraction of graphite is 4.5%, and the mass fraction of SBR is 2%.

[0143] 2. Negative electrode current collector coating

[0144] 1. Mix the prepared vesicle-coated silicon dioxide, graphite, SBR and water according to the formula in step 3 to obtain a first coating slurry. Apply the first coating slurry on the current collector using a coating machine and dry it.

[0145] 2. PAL, graphite, SBR and water are mixed according to the formula in step 5 to obtain a second coating slurry. The second coating slurry is applied to the surface of the electrode sheet containing the first coating by a coating machine and dried. After drying, the silicon-containing negative electrode sheet is prepared by rolling, slitting and spot welding, wherein the single-sided thickness of the first coating is 60 μm and the single-sided thickness of the second coating is 5.5 μm.

[0146] 3. Organic solid electrolyte coated silicon substrate

[0147] The silicon electrode sheet with the first coating and the second coating was laid flat on glass, placed in a sealed container containing ammonium carbonate, and then heated at 80°C for 2 hours to react, thereby obtaining a CMC-Li2CO3 coated silicon-based negative electrode sheet.

[0148] Example 3

[0149] 1. Material preparation

[0150] 1. Weigh 5.19g DOPC and dissolve it in 100ml dichloromethane to obtain a DOPC solution. Then form a layer of phospholipid film on the wall of the rotary evaporator with the DOPC solution, blow it dry with nitrogen, and dry it in a vacuum drying oven for 12 hours to prepare a phospholipid dry film. Then add 100ml of Tris-HCl (pH7.5) at 60°C for hydration. The hydration time is about 5.5h, vortex, and let it stand until the solution is completely precipitated. Transfer the upper phase into a centrifuge tube containing 50ml of Tris-HCl (pH7.5) for centrifugation. Phospholipid vesicles can be obtained in the solution below.

[0151] 2. Dissolve the phospholipid vesicles obtained in step 1, 1.84 g of stearic acid and 10 g of silicon dioxide (nano-silicon dioxide particles with a particle size of less than 1.2 nm account for 7%, and nano-silicon dioxide particles with a particle size greater than 22 nm and ≤ 200 nm account for 93%) in 800 ml of ethanol to form solution A. Dissolve 50.6 ml of Tween-40 in 34 ml of Tris-HCl (pH 7.5) to prepare solution B. Inject solution A into solution B and stir at 70°C for 5 hours. Finally, wash the sample three times with Tris-HCl (pH 7.5) to remove free vesicles. After centrifugation, dry it in a vacuum freeze dryer to obtain vesicle-coated silicon dioxide.

[0152] 3. The first coating layer contains vesicle-encapsulated silicon oxide, a conductive agent, and a binder, wherein the conductive agent is activated carbon and the binder is PVDF. In the first coating layer, the mass fraction of vesicle-encapsulated silicon oxide is 95.5%, the mass fraction of activated carbon is 2.5%, and the mass fraction of PAA is 2%.

[0153] 4. Prepare 8% PSS solution with deionized water, then add 6.2 g of lithium nitrate to the PSS solution to obtain a PSS solution containing Li+, centrifuge and dry in a vacuum dryer to obtain a PSS complex, referred to as PL.

[0154] 5. The second coating contains PL: conductive agent: binder, wherein the conductive agent is activated carbon and the binder is PAA. In the second coating, the mass fraction of PL is 95.5%, the mass fraction of graphite is 2.5%, and the mass fraction of SBR is 2%.

[0155] 2. Negative electrode current collector coating

[0156] 1. According to the formula in step 3, the prepared vesicle-encapsulated silicon dioxide, activated carbon, PAA and water are mixed to obtain a first coating slurry. The first coating slurry is coated on the current collector by a coating machine and dried.

[0157] 2. Mix PL, activated carbon, PAA and water according to the formula in step 5 to obtain a second coating slurry. Use a coating machine to apply the second coating slurry to the surface of the electrode sheet containing the first coating and dry it. After drying, roll pressing, slitting and spot welding are performed to prepare a silicon-containing negative electrode sheet, wherein the single-sided thickness of the first coating is 45 μm, and the single-sided thickness of the second coating is 8 μm.

[0158] 3. Organic solid electrolyte coated silicon substrate

[0159] The silicon electrode sheet containing the first coating and the second coating was spread flat on glass, placed in a sealed container containing ammonium carbonate, and then heated at 80°C for 3 hours to react, thereby obtaining a PSS-Li2CO3-coated silicon-based negative electrode sheet.

[0160] Example 4

[0161] 1. Material preparation

[0162] 1. Weigh 4.56g DOPG and dissolve it in 70ml chloroform to obtain DOPG solution. Then form a phospholipid film on the wall of the rotary evaporator with the DOPG solution, blow it dry with nitrogen, and dry it in a vacuum drying oven for 12h to prepare a phospholipid dry film. Then add 70ml of Tris-HCl (pH7.5) at 60℃ for hydration for about 5h, vortex, and let it stand until the solution is completely precipitated. Transfer the upper phase into a centrifuge tube containing 30ml of Tris-HCl (pH7.5) for centrifugation, and phospholipid vesicles can be obtained in the lower solution.

[0163] 2. Dissolve the phospholipid vesicles obtained in step 1, 2.05 g of cholesterol and 10 g of silica (nano silica particles with a particle size of less than 1.2 nm account for 5%, and nano silica particles with a particle size greater than 22 nm and ≤ 200 nm account for 95%) in 1000 ml of ethanol to form solution A. Dissolve 42.3 ml of Tween-40 in 37.1 ml of Tris-HCl (PH7.5) to prepare solution B. Inject solution A into solution B and stir at 80°C for 3 hours. Finally, wash the sample three times with Tris-HCl (pH7.5) to remove free vesicles. After centrifugation, dry it in a vacuum freeze dryer to obtain vesicle-coated silica.

[0164] 3. The first coating layer contains vesicle-coated silicon oxide, a conductive agent, and a binder, wherein the conductive agent is carbon black and the binder is HPMC. In the first coating layer, the mass fraction of vesicle-coated silicon oxide is 89%, the mass fraction of carbon black is 5%, and the mass fraction of HPMC is 6%.

[0165] 4. Prepare a 6.5% CMC solution with deionized water, then add 5.7 g of lithium nitrate to the CMC solution to obtain a CMC solution containing Li+, centrifuge and dry in a vacuum dryer to obtain a CMC complex, referred to as CL.

[0166] 5. The second coating contains CL: conductive agent: binder, wherein the conductive agent is carbon black and the binder is HPMC. In the second coating, the mass fraction of CL is 96%, the mass fraction of carbon black is 2%, and the mass fraction of HPMC is 2%.

[0167] 2. Negative electrode current collector coating

[0168] 1. According to the formula in step 3, the prepared vesicle-coated silicon dioxide, carbon black, HPMC and NMP are mixed to obtain a first coating slurry. The first coating slurry is coated on the current collector by a coating machine and dried.

[0169] 2. Mix CL, carbon black, HPMC and NMP in the amount of step 5 to obtain a second coating slurry. Use a coating machine to apply the second coating slurry to the surface of the electrode sheet containing the first coating and dry it. After drying, roll pressing, slitting and spot welding are performed to prepare a silicon-containing negative electrode sheet, wherein the single-sided thickness of the first coating is 70 μm, and the single-sided thickness of the second coating is 10 μm.

[0170] 3. Organic solid electrolyte coated silicon substrate

[0171] The silicon electrode sheet containing the first coating and the second coating was spread flat on glass, placed in a sealed container containing ammonium carbonate, and then heated at 80°C for 4 hours to react, thereby obtaining a PSS-Li2CO3-coated silicon-based negative electrode sheet.

[0172] Example 5

[0173] 1. Material preparation

[0174] 1. Weigh 4.93g DOPG and dissolve it in 70ml chloroform to obtain DOPG solution. Then form a phospholipid film on the wall of the rotary evaporator with the DOPG solution, blow it dry with nitrogen, and dry it in a vacuum drying oven for 12h to prepare a phospholipid dry film. Then add 70ml of Tris-HCl (pH7.5) at 60℃ for hydration. The hydration time is about 5h, vortex, and let it stand until the solution is completely precipitated. Transfer the upper phase into a centrifuge tube containing 30ml of Tris-HCl (pH7.5) for centrifugation, and phospholipid vesicles can be obtained in the lower solution.

[0175] 2. Dissolve the phospholipid vesicles obtained in step 1, 2.05 g of cholesterol and 10 g of silica (nano silica particles with a particle size of less than 1.2 nm account for 8%, and nano silica particles with a particle size greater than 22 nm and ≤ 200 nm account for 92%) in 1000 ml of ethanol to form solution A. Dissolve 42.3 ml of Tween-40 in 37.1 ml of Tris-HCl (pH 7.5) to prepare solution B. Inject solution A into solution B and stir at 80°C for 3 hours. Finally, wash the sample three times with Tris-HCl (pH 7.5) to remove free vesicles. After centrifugation, dry it in a vacuum freeze dryer to obtain vesicle-coated silica.

[0176] 3. The first coating layer contains vesicle-coated silicon oxide, a conductive agent, and a binder, wherein the conductive agent is carbon black and the binder is HPMC. In the first coating layer, the mass fraction of vesicle-coated silicon oxide is 89%, the mass fraction of carbon black is 5%, and the mass fraction of HPMC is 6%.

[0177] 4. Prepare a 6.5% CMC solution with deionized water, then add 5.7 g of lithium nitrate to the CMC solution to obtain a CMC solution containing Li+, centrifuge and dry in a vacuum dryer to obtain a CMC complex, referred to as CL.

[0178] 5. The second coating contains CL: conductive agent: binder, wherein the conductive agent is carbon black and the binder is HPMC. In the second coating, the mass fraction of CL is 96%, the mass fraction of carbon black is 2%, and the mass fraction of HPMC is 2%.

[0179] 2. Negative electrode current collector coating

[0180] 1. According to the formula in step 3, the prepared vesicle-coated silicon dioxide, carbon black, HPMC and NMP are mixed to obtain a first coating slurry. The first coating slurry is coated on the current collector by a coating machine and dried.

[0181] 2. Mix CL, carbon black, HPMC and NMP in the amount of step 5 to obtain a second coating slurry. Use a coating machine to apply the second coating slurry to the surface of the electrode sheet containing the first coating and dry it. After drying, roll pressing, slitting and spot welding are performed to prepare a silicon-containing negative electrode sheet, wherein the single-sided thickness of the first coating is 70 μm, and the single-sided thickness of the second coating is 10 μm.

[0182] 3. Organic solid electrolyte coated silicon substrate

[0183] The silicon electrode sheet containing the first coating and the second coating was spread flat on glass, placed in a sealed container containing ammonium carbonate, and then heated at 80°C for 4 hours to react, thereby obtaining a PSS-Li2CO3-coated silicon-based negative electrode sheet.

[0184] Example 6

[0185] 1. Material preparation

[0186] 1. Weigh 3.27g DOPC and dissolve it in 70ml chloroform to obtain DOPC solution. Then form a phospholipid film on the wall of the rotary evaporator with the DOPC solution, blow it dry with nitrogen, and dry it in a vacuum drying oven for 12h to prepare a phospholipid dry film. Then add 80ml PBS (pH7.4) at 60℃ for hydration for about 6h, vortex, and let it stand until the solution is completely precipitated. Transfer the upper phase into a centrifuge tube containing 20ml PBS (pH7.4) for centrifugation, and obtain phospholipid vesicles in the lower solution.

[0187] 2. Dissolve the phospholipid vesicles obtained in step 1, 1.08 g of cholesterol and 10 g of silica (nano silica particles with a particle size of less than 1.2 nm account for 10%, and nano silica particles with a particle size greater than 22 nm and ≤ 200 nm account for 90%) in 1000 ml of ethanol to form solution A. Dissolve 35 ml of Tween-20 in 23 ml of PBS (pH 7.4) to prepare solution B. Inject solution A into solution B and stir at 60°C for 5 hours. Finally, wash the sample three times with PBS (pH 7.4) to remove free vesicles. After centrifugation, dry it in a vacuum freeze dryer to obtain vesicle-coated silica.

[0188] 3. The first coating layer contains vesicle-coated silicon oxide, a conductive agent, and a binder, wherein the conductive agent is graphite and the binder is SBR. In the first coating layer, the mass fraction of vesicle-coated silicon oxide is 96%, the mass fraction of graphite is 2%, and the mass fraction of SBR is 2%.

[0189] 4. Prepare 8% PSS solution with deionized water, then add 6.2 g of lithium nitrate to the PSS solution to obtain a PSS solution containing Li+, centrifuge and dry in a vacuum dryer to obtain a PSS complex, referred to as PL.

[0190] 5. The second coating contains PL: conductive agent: binder, wherein the conductive agent is graphite and the binder is SBR. In the second coating, the mass fraction of PL is 93.5%, the mass fraction of graphite is 4.5%, and the mass fraction of SBR is 2%.

[0191] 2. Negative electrode current collector coating

[0192] 1. According to the formula in step 3, the prepared vesicle-coated silicon dioxide, graphite, SBR and NMP are mixed to obtain a first coating slurry. The first coating slurry is coated on the current collector by a coating machine and dried.

[0193] 2. Mix PL, graphite, SBR and NMP according to the formula in step 5 to obtain a second coating slurry. Use a coating machine to apply the second coating slurry to the surface of the electrode sheet containing the first coating and dry it. After drying, roll pressing, slitting and spot welding are performed to prepare a silicon-containing negative electrode sheet, wherein the single-sided thickness of the first coating is 60 μm, and the single-sided thickness of the second coating is 10 μm.

[0194] 3. Organic solid electrolyte coated silicon substrate

[0195] The silicon electrode sheet containing the first coating and the second coating was spread flat on glass, placed in a sealed container containing ammonium carbonate, and then heated at 90°C for 3 hours to react, thereby obtaining a PSS-Li2CO3-coated silicon-based negative electrode sheet.

[0196] Example 7

[0197] 1. Material preparation

[0198] 1. Weigh 2g DOPC and dissolve it in 70ml chloroform to obtain DOPC solution. Then form a phospholipid film on the wall of the rotary evaporator with the DOPC solution, blow it dry with nitrogen, and dry it in a vacuum drying oven for 12h to prepare a phospholipid dry film. Then add 80ml PBS (pH7.4) at 60℃ for hydration for about 5h, vortex, and let it stand until the solution is completely precipitated. Transfer the upper phase into a centrifuge tube containing 20ml PBS (pH7.4) for centrifugation, and phospholipid vesicles can be obtained in the lower solution.

[0199] 2. Dissolve the phospholipid vesicles obtained in step 1, 0.4 g of cholesterol and 10 g of silica (nano-silica particles with a particle size of less than 1.2 nm account for 10%, and nano-silica particles with a particle size greater than 22 nm and ≤ 200 nm account for 90%) in 1000 ml of ethanol to form solution A. Dissolve 35 ml of Tween-20 in 23 ml of PBS (pH 7.4) to prepare solution B. Inject solution A into solution B and stir at 40°C for 1 hour. Finally, wash the sample three times with PBS (pH 7.4) to remove free vesicles. After centrifugation, dry it in a vacuum freeze dryer to obtain vesicle-coated silica.

[0200] 3. The first coating layer contains vesicle-coated silicon oxide, a conductive agent, and a binder, wherein the conductive agent is graphite and the binder is SBR. In the first coating layer, the mass fraction of vesicle-coated silicon oxide is 90%, the mass fraction of graphite is 5%, and the mass fraction of SBR is 5%.

[0201] 4. Prepare a 2% PSS solution with deionized water, then add 4.3 g of LiC2H3O2 to the PSS solution to obtain a PSS solution containing Li+, centrifuge and dry in a vacuum dryer to obtain a PSS complex, referred to as PL.

[0202] 5. The second coating contains PL: conductive agent: binder, wherein the conductive agent is graphite and the binder is SBR. In the second coating, the mass fraction of PL is 93.5%, the mass fraction of graphite is 4.5%, and the mass fraction of SBR is 2%.

[0203] 2. Negative electrode current collector coating

[0204] 1. According to the formula in step 3, the prepared vesicle-coated silicon dioxide, graphite, SBR and NMP are mixed to obtain a first coating slurry. The first coating slurry is coated on the current collector by a coating machine and dried.

[0205] 2. Mix PL, graphite, SBR and NMP according to the formula in step 5 to obtain a second coating slurry. Use a coating machine to apply the second coating slurry to the surface of the electrode sheet containing the first coating and dry it. After drying, roll pressing, slitting and spot welding are performed to prepare a silicon-containing negative electrode sheet, wherein the single-sided thickness of the first coating is 0.02 μm, and the single-sided thickness of the second coating is 0.02 μm.

[0206] 3. Organic solid electrolyte coated silicon substrate

[0207] The silicon electrode sheet containing the first coating and the second coating was spread flat on glass, placed in a sealed container containing ammonium carbonate, and then heated at 40°C for 1 hour to react, thereby obtaining a PSS-Li2CO3-coated silicon-based negative electrode sheet.

[0208] Example 8

[0209] 1. Material preparation

[0210] 1. Weigh 5g PC and dissolve it in 70ml dichloromethane to obtain PC solution. Then form a phospholipid film on the wall of the rotary evaporator, blow it dry with nitrogen, and dry it in a vacuum drying oven for 12h to prepare a phospholipid dry film. Then add 80ml PBS (pH7.4) at 80℃ for hydration for about 6h, vortex, and let it stand until the solution is completely precipitated. Transfer the upper phase into a centrifuge tube containing 20ml PBS (pH7.4) for centrifugation, and phospholipid vesicles can be obtained in the lower solution.

[0211] 2. Dissolve the phospholipid vesicles obtained in step 1, 2.5 g of cholesterol and 10 g of silica (nano-silica particles with a particle size of less than 1.2 nm account for 10%, and nano-silica particles with a particle size greater than 22 nm and ≤ 200 nm account for 90%) in 1000 ml of ethanol to form solution A. Dissolve 35 ml of Tween-20 in 23 ml of PBS (pH 7.4) to prepare solution B. Inject solution A into solution B and stir at 80°C for 5 hours. Finally, wash the sample three times with PBS (pH 7.4) to remove free vesicles. After centrifugation, dry it in a vacuum freeze dryer to obtain vesicle-coated silica.

[0212] 3. The first coating layer contains vesicle-coated silicon oxide, a conductive agent, and a binder, wherein the conductive agent is activated carbon and the binder is SBR. In the first coating layer, the mass fraction of vesicle-coated silicon oxide is 93%, the mass fraction of activated carbon is 4%, and the mass fraction of SBR is 3%.

[0213] 4. Prepare a 10% CMC solution with deionized water, then add 5.7 g of Li3PO4 to the CMC solution to obtain a CMC solution containing Li+, centrifuge and dry in a vacuum dryer to obtain a CMC complex, referred to as CL.

[0214] 5. The second coating contains CMC: conductive agent: binder, wherein the conductive agent is activated carbon and the binder is SBR. In the second coating, the mass fraction of CMC is 91%, the mass fraction of activated carbon is 3%, and the mass fraction of SBR is 5%.

[0215] 2. Negative electrode current collector coating

[0216] 1. According to the formula in step 3, the prepared vesicle-coated silicon dioxide, activated carbon, SBR and NMP are mixed to obtain a first coating slurry. The first coating slurry is coated on the current collector by a coating machine and dried.

[0217] 2. Mix CL, activated carbon, SBR and NMP according to the formula in step 5 to obtain a second coating slurry. Use a coating machine to apply the second coating slurry to the surface of the electrode sheet containing the first coating and dry it. After drying, roll pressing, slitting and spot welding are performed to prepare a silicon-containing negative electrode sheet, wherein the single-sided thickness of the first coating is 150 μm, and the single-sided thickness of the second coating is 12 μm.

[0218] 3. Organic solid electrolyte coated silicon substrate

[0219] The silicon electrode sheet containing the first coating and the second coating was spread flat on glass, placed in a sealed container containing ammonium carbonate, and then heated at 100°C for 4 hours to react, thereby obtaining a CMC-Li2CO3-coated silicon-based negative electrode sheet.

[0220] Example 9

[0221] 1. Material preparation

[0222] 1. Weigh 4g DOPG and dissolve it in 70ml n-hexane to obtain DOPG solution. Then form a phospholipid film on the wall of the rotary evaporator with the DOPG solution, blow it dry with nitrogen, and dry it in a vacuum drying oven for 12h to prepare a phospholipid dry film. Then add 80ml PBS (pH7.4) at 70℃ for hydration for about 5h, vortex, and let it stand until the solution is completely precipitated. Transfer the upper phase into a centrifuge tube containing 20ml PBS (pH7.4) for centrifugation, and phospholipid vesicles can be obtained in the lower solution.

[0223] 2. Dissolve the phospholipid vesicles obtained in step 1, 2 g of cholesterol and 10 g of silica (nano silica particles with a particle size of less than 1.2 nm account for 10%, and nano silica particles with a particle size greater than 22 nm and ≤ 200 nm account for 90%) in 1000 ml of ethanol to form solution A. Dissolve 35 ml of Tween-40 in 23 ml of Tris-HCl (pH 7.5) to prepare solution B. Inject solution A into solution B and stir at 60°C for 3 hours. Finally, wash the sample three times with Tris-HCl (pH 7.5) to remove free vesicles. After centrifugation, dry it in a vacuum freeze dryer to obtain vesicle-coated silica.

[0224] 3. The first coating layer contains vesicle-coated silicon oxide, a conductive agent, and a binder, wherein the conductive agent is graphite and the binder is SBR. In the first coating layer, the mass fraction of vesicle-coated silicon oxide is 96%, the mass fraction of graphite is 2%, and the mass fraction of SBR is 2%.

[0225] 4. Prepare a 9% CMC solution with deionized water, then add 8.1 g of LiBr to the CMC solution to obtain a CMC solution containing Li+, centrifuge and dry in a vacuum dryer to obtain a CMC complex, referred to as CL.

[0226] 5. The second coating contains CL: conductive agent: binder, wherein the conductive agent is graphite and the binder is SBR. In the second coating, the mass fraction of CL is 93.5%, the mass fraction of graphite is 4.5%, and the mass fraction of SBR is 2%.

[0227] 2. Negative electrode current collector coating

[0228] 1. According to the formula in step 3, the prepared vesicle-coated silicon dioxide, graphite, SBR and NMP are mixed to obtain a first coating slurry. The first coating slurry is coated on the current collector by a coating machine and dried.

[0229] 2. Mix CL, graphite, SBR and NMP according to the formula in step 5 to obtain a second coating slurry. Use a coating machine to apply the second coating slurry to the surface of the electrode sheet containing the first coating and dry it. After drying, roll pressing, slitting and spot welding are performed to prepare a silicon-containing negative electrode sheet, wherein the single-sided thickness of the first coating is 100 μm, and the single-sided thickness of the second coating is 12 μm.

[0230] 3. Organic solid electrolyte coated silicon substrate

[0231] The silicon electrode sheet containing the first coating and the second coating was spread flat on glass, placed in a sealed container containing ammonium carbonate, and then heated at 90°C for 3 hours to react, thereby obtaining a CMC-Li2CO3-coated silicon-based negative electrode sheet.

[0232] Comparative Example 1

[0233] SiO2 is added to a multi-walled carbon nanotube dispersion, and evenly dispersed by ultrasonication at 100 Hz, and then filtered, and the solid matter obtained by filtration is washed and dried to obtain a precursor A; the precursor A is added to a tube furnace, and sintered at 300°C under a nitrogen atmosphere to form a carbon layer on the surface of SiO2 to obtain a carbon nanotube-coated silicon-based negative electrode material, that is, a conventional carbon nanotube-coated negative electrode material. The mass of the multi-walled carbon nanotube accounts for 0.03% of the total mass of the silicon-based negative electrode material.

[0234] Comparative Example 2

[0235] The uncoated negative electrode material silicon dioxide is selected. According to the test method of the present invention, a button cell is directly prepared for testing.

[0236] Comparative Example 3

[0237] The first layer of uncoated silicon monoxide was selected and the second layer of coating and solid electrolyte coating were performed according to Example 1. According to the test method of the present invention, button cells were directly prepared for testing.

[0238] Comparative Example 4

[0239] The first coating and anionic polymer coating were performed according to Example 1, and no lithium salt and solid electrolyte coating were added. A button cell was directly prepared and tested according to the test method of the present invention.

[0240] Comparative Example 5

[0241] The first coating and the second coating were performed according to Embodiment 1 without solid electrolyte coating. A button cell was directly prepared and tested according to the test method of the present invention.

[0242] Comparative Example 6

[0243] The coating was performed according to Embodiment 6, wherein silicon dioxide particles with a particle size of 1.2-22 nm were selected in step 2, and the other steps were the same. A button cell was directly prepared and tested according to the test method of the present invention.

[0244] The negative electrode sheet obtained by the preparation method of Examples 1-9 and Comparative Examples 1 and 2 was placed in a vacuum drying oven at 90°C and dried for 12 hours. The dried negative electrode sheet was transferred to a glove box, and a metal lithium sheet was used as a counter electrode. A 2032-type button cell was assembled in a glove box filled with dry argon. The diaphragm was polypropylene (PP), and the electrolyte was a solution of 1 mol / L (LiPF6) and ethylene carbonate (EC) / dimethyl carbonate (DMC) (the volume ratio of EC and MC was 1:2). The electrochemical performance of the 2032-type button cell was tested at 25°C, and the first coulomb efficiency and first discharge specific capacity were tested at a discharge rate of 0.1C, with a voltage range of 0.005-1.5V. The capacity retention rate was tested after 100 and 500 cycles at a 1C rate. At the same time, at a high temperature of 120°C, a charging voltage of 2.8V-4.2V (voltage range), and a charge and discharge rate of 0.5C, the battery capacity retention rate was tested after 100 cycles.

[0245] From the electrical performance results of the button-type batteries of Examples 1-9 and Comparative Example 1, it can be seen that the uniformity of dispersion of multi-walled carbon nanotubes added by conventional coating methods is difficult to ensure, and there is a large interface resistance, resulting in a significant decrease in the product rate performance.

[0246] From the battery performance structure of Implementation 1-9 and Comparative Example 6, it can be seen that the scheme of selecting silicon dioxide particles with a specific particle size and ratio has better effects in improving the specific capacity, coulombic efficiency and cycle stability of the material. Among them, nano silicon dioxide particles with a particle size of less than 1.2nm can better penetrate into the lipid membrane without destroying the membrane structure, and nano silicon dioxide particles with a particle size greater than 22nm and ≤200nm will be firmly wrapped by the lipid membrane. The combined effect of the two helps to form a more stable SEI membrane, reduce the dissolution and decomposition of silicon dioxide in the electrolyte, and thus play a better role of silicon dioxide.

[0247] From the data in the table of Examples 1-9 and Comparative Examples 2-6, it can be seen that the biofilm-like coating method is used to synthesize the material, which effectively improves the discharge capacity and rate performance of the material, and the first capacity discharge specific capacity is as high as 1412 mAh / g. The capacity retention rate of 500 cycles is as high as 76.3%, and the capacity retention rate of 100 cycles under high temperature conditions (120°C) is as high as 84.7%. The cycle performance is improved significantly, and the biofilm-like coating of the negative electrode material has a significant effect. This is because the biofilm-like membrane provides a layer of stable interface film for the negative electrode material, reduces the occurrence of side reactions, and also limits the structural damage and capacity attenuation caused by expansion, so that the battery still maintains a high performance in a long cycle. At the same time, combined with the joint effect of pre-lithiation, the amount of lithium ions embedded in the battery during the first charge is further reduced, and the capacity and cycle life of the battery are further improved.

[0248] Table 1

[0249]

[0250] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A negative electrode plate having an artificially constructed SEI film, characterized in that: include: Anode current collector; A first coating layer composited on the surface of the negative electrode current collector, wherein the first coating layer comprises a silicon negative electrode material coated with phospholipid vesicles; A second coating layer composited with the first coating layer, wherein the second coating layer comprises an anionic polymer complex; An organic solid electrolyte coating layer is compounded on the second coating layer.

2. The negative electrode sheet according to claim 1, characterized in that: The preparation method of the phospholipid vesicles comprises the following steps: 1) preparing an organic solution containing phospholipids; 2) After removing the organic solvent in the organic solution, a layer of phospholipid dry film is obtained; 3) The phospholipid dry film is hydrated to obtain phospholipid vesicles.

3. The negative electrode sheet according to claim 2, characterized in that: The phospholipid is selected from one or more of phosphatidylcholine, phosphatidylglyceride, dioleylphosphatidylcholine, and dioleylphosphatidylglycerol; The mass percentage of the phospholipid in the silicon negative electrode material is 20% to 50%; The organic solvent used to prepare the organic solution containing phospholipids is selected from one or more of n-hexane, dichloromethane and chloroform; Hydration is performed using a buffer selected from PBS or Tris-HCl; The hydration temperature is 50-80° C. and the hydration time is 2-6 hours.

4. The negative electrode sheet according to claim 1, characterized in that: The silicon negative electrode material is selected from silicon oxide SiO x , where 0 <x<2; Preferably, the silicon oxide comprises: nano silicon oxide particles with a particle size of less than 1.2 nm and nano silicon oxide particles with a particle size of more than 22 nm; Preferably, nano-silicon oxide particles with a particle size of less than 1.2 nm account for 5-10% of the total mass of silicon oxide, and nano-silicon oxide particles with a particle size of more than 22 nm account for 90-95% of the total mass of silicon oxide.

5. The negative electrode sheet according to claim 1, characterized in that: The method for preparing a silicon negative electrode material coated with phospholipid vesicles comprises the following steps: 1) dissolving phospholipid vesicles, stabilizer and silicon negative electrode material in a solvent to form solution A; 2) dissolving the emulsifier in the buffer solution to prepare solution B; 3) Mixing solution A and solution B and stirring to obtain a reaction solution; 4) washing, centrifuging and drying the reaction solution to obtain a silicon negative electrode material coated with phospholipid vesicles.

6. The negative electrode material according to claim 5, characterized in that The stabilizer is selected from one or more of cholesterol, stearic acid and sphingomyelin, and the added amount is 20% to 50% of the phospholipids; The selected emulsifier is one or more of Tween-80, Tween-20, Tween-40 and Tween-60; In step 3), the mixing and stirring temperature is 40 to 80° C. and the time is 1 to 5 hours.

7. The negative electrode material according to claim 5, characterized in that The first coating layer further includes a conductive agent and a binder.

8. The negative electrode material according to claim 7, characterized in that The conductive agent is selected from one or more of graphite, carbon black, and activated carbon; The binder is selected from one or more of polyvinylidene fluoride, polyacrylic acid, styrene-butadiene rubber, and hydroxypropyl methylcellulose; The mass ratio of the silicon negative electrode material coated by the phospholipid vesicles, the conductive agent and the binder is 85-95:2-5:2-5.

9. The negative electrode sheet according to claim 1, characterized in that: The preparation method of the anionic polymer complex comprises the following steps: mixing anionic polymer, lithium salt and water to react and obtain a reaction product; The reaction product is centrifuged and then dried to obtain the anionic polymer complex.

10. The negative electrode sheet according to claim 9, characterized in that: The anionic polymer is one or more of sodium polystyrene sulfonate, sodium carboxymethyl cellulose and sodium polyacrylate; The lithium salt is one or more of LiCl, LiBr, LiI, LiNO3, Li3PO4, and LiC2H3O2.

11. The negative electrode sheet according to claim 1, characterized in that: The second coating layer further includes a conductive agent and a binder.

12. The negative electrode sheet according to claim 11, characterized in that: The conductive agent is one or more of graphite, carbon black, and activated carbon; The binder is selected from one or more of polyvinylidene fluoride, polyacrylic acid, styrene-butadiene rubber, and hydroxypropyl methylcellulose; The mass ratio of the anionic polymer complex, the conductive agent and the binder is 90-95:2-5:2-5.

13. The negative electrode sheet according to claim 1, characterized in that: The thickness of the first coating is 0.02 to 150 μm; The thickness of the second coating is 0.02 to 12 μm; The thickness of the organic solid electrolyte coating layer is 0.1-5 μm.

14. A method for preparing a negative electrode sheet according to any one of claims 1 to 13, characterized in that: The following steps are involved: A) mixing a silicon negative electrode material coated with phospholipid vesicles, a conductive agent, a binder and a solvent to obtain a first coating slurry; Applying the first coating slurry on the surface of the current collector and drying it to obtain a pole piece composited with the first coating; B) mixing the anionic polymer complex, the conductive agent, the binder and the solvent to obtain a second coating slurry; Applying the second coating slurry to the surface of the electrode composited with the first coating, and drying the electrode composited with the first coating and the second coating to obtain the electrode composited with the first coating; C) placing the electrode sheet having the first coating layer and the second coating layer on the surface of the substrate, placing the electrode sheet in a sealed container containing ammonium carbonate, and heating the electrode sheet at a certain temperature for a period of time to obtain an organic solid electrolyte coated silicon-based negative electrode sheet.

15. The preparation method according to claim 14, characterized in that: In step A) and step B), the solvent is selected from NMP and water; In step C), the heating temperature is 40 to 100° C. and the heating time is 1 to 4 hours.

16. A secondary battery, characterized in that: The negative electrode sheet comprises the negative electrode sheet as described in any one of claims 1 to 13.

Citation Information

Cited By

  • Method for preparing lithium battery negative electrode material by using phosphate fertilizer solid waste and application of lithium battery negative electrode material

    CN121536938A