A preparation method of polyphenol and probiotic co-encapsulated nanofiber

By co-encapsulating polyphenols and probiotics in nanofibers, the problem of decreased vitality of probiotics during processing and storage is solved, and its thermal stability and antioxidant ability are significantly improved, and the functional effect of probiotic products is improved.

CN117904741BActive Publication Date: 2024-12-03NORTHEAST AGRICULTURAL UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410002887.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-02
Publication Date
2024-12-03
Estimated Expiration
2044-01-02

AI Technical Summary

Technical Problem

Probiotics are susceptible to environmental and in vivo factors during processing, storage and in vivo delivery, resulting in a decrease in vitality, and only a small part of them arrives at designated locations to exert health benefits. How to improve the functional effect of probiotic products is an urgent problem to be solved.

Method used

The preparation method of co-encapsulating nanofibers with polyphenols and probiotics is used to add polyphenols (such as gallic acid, chlorogenic acid, dihydromycetein and hesperidin) to a blended solution of polyvinyl alcohol and fucoidan. Electrospinning encapsulates probiotics in nanofibers, improving their thermal stability and antioxidant ability.

Benefits of technology

It significantly improves the thermal stability and antioxidant ability of probiotics, extends the shelf life stability, and thus improves the functional effect of probiotic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117904741B_ABST
    Figure CN117904741B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of construction of probiotic delivery systems, and in particular to a method for preparing polyphenol-probiotic co-encapsulated nanofibers. The method comprises the following steps: adding polyphenols to a blended solution of polyvinyl alcohol and fucoidan to obtain a blended solution of the three; adding probiotics to the blended solution of the three and mixing them evenly to obtain an electrospinning solution; electrospinning the electrospinning solution to obtain polyphenol-probiotic co-encapsulated nanofibers; the polyphenols are at least one of gallic acid, chlorogenic acid, dihydromyricetin and hesperidin. The present invention significantly improves the thermal stability, antioxidant capacity and shelf life stability of probiotics by adding polyphenols (at least one of gallic acid, chlorogenic acid, dihydromyricetin and hesperidin) to an electrospinning solution containing probiotics, and encapsulating the probiotics in nanofibers by electrospinning.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of constructing a probiotic delivery system, and in particular to a method for preparing a polyphenol and probiotic co-encapsulated nanofiber. Background Art

[0002] In recent years, probiotics have been a hot research topic in the fields of food, medicine and nutrition. According to the Food and Agriculture Organization (FAO) and the World Health Organization (WHO), probiotics are defined as active microorganisms that can provide health benefits to the host when ingested in sufficient quantities, and probiotics are safe. The main types of probiotics include Lactobacillus, Bifidobacterium, Lactococcus and Streptococcus thermophilus. Some studies have shown that active probiotics have beneficial health and disease prevention effects, such as maintaining intestinal homeostasis, enhancing intestinal barrier function, and alleviating disease. However, it is necessary to ensure that probiotics are metabolically active and in sufficient quantities to work. Studies have shown that the number of probiotics needs to exceed 10 during the delivery process. 6 CFU / g is needed to exert the health benefits of probiotics. However, probiotics are easily affected by environmental stress during processing and storage, such as oxygen, temperature, pH, light, osmotic pressure and other factors in the environment, which lead to a decrease in the activity of probiotics or the number of live bacteria. In addition, probiotics are also affected by internal factors after being ingested into the body, such as: water, lysozyme, inorganic salt ions in oral saliva, water, hydrochloric acid, pepsinogen in gastric juice, bile salts, digestive enzymes in the small intestine, etc. Therefore, only a small part reaches the designated part to exert health benefits. How to improve the functional effects of probiotic products is a technical problem that needs to be solved urgently by technicians in this field. Summary of the invention

[0003] Based on the above content, the present invention provides a method for preparing polyphenol and probiotic co-encapsulated nanofibers.

[0004] To achieve the above object, the present invention provides the following solutions:

[0005] One of the technical solutions of the present invention is a method for preparing polyphenol and probiotic co-encapsulated nanofibers, comprising the following steps:

[0006] Adding polyphenols to a mixed solution of polyvinyl alcohol and fucoidan to obtain a mixed solution of the three;

[0007] Adding probiotics to the blended solution of the three and mixing evenly to obtain an electrospinning solution;

[0008] Electrospinning the electrospinning solution to obtain polyphenol and probiotic co-encapsulated nanofibers;

[0009] The polyphenol is at least one of gallic acid, chlorogenic acid, dihydromyricetin and hesperidin.

[0010] The second technical solution of the present invention is to prepare the polyphenol and probiotic co-encapsulated nanofibers using the above-mentioned method for preparing the polyphenol and probiotic co-encapsulated nanofibers.

[0011] The third technical solution of the present invention is the use of the above-mentioned polyphenols and probiotics co-encapsulated nanofibers in the preparation of medicines and foods.

[0012] The present invention discloses the following technical effects:

[0013] The present invention studies the probiotic effects of four polyphenols, gallic acid, chlorogenic acid, dihydromyricetin and hesperidin, on probiotics (Lactobacillus plantarum), and further studies the effects of the four polyphenols on the viable count of probiotics. The present invention adds polyphenols (at least one of gallic acid, chlorogenic acid, dihydromyricetin and hesperidin) to an electrospinning solution containing probiotics, and encapsulates the probiotics in nanofibers by electrospinning, thereby significantly improving the thermal stability, antioxidant capacity and storage stability of the probiotics, thereby improving the functional effects of the probiotic products. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0015] Figure 1 To investigate the effects of adding different types of polyphenols on the viable count of L. plantarum 69-2.

[0016] Figure 2 The left picture is the SEM image and the right picture is the fiber diameter distribution histogram of pure PVA fiber.

[0017] Figure 3 The left figure is the SEM image and the right figure is the fiber diameter distribution histogram of PVA / FUC fiber.

[0018] Figure 4 The left figure is the SEM image and the right figure is the fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 fiber.

[0019] Figure 5The left figure is the SEM image and the right figure is the fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 / GA fiber.

[0020] Figure 6 The SEM image and fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 / CA fiber; the left image is the SEM image, and the right image is the fiber diameter distribution histogram.

[0021] Figure 7 The left figure is the SEM image and the right figure is the fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 / DMY fiber.

[0022] Figure 8 The left figure is the SEM image and the right figure is the fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 / HES fiber.

[0023] Fig. 9 Fourier transform infrared spectra of different electrospun nanofibers and powder samples (polyvinyl alcohol (PVA), fucoidan (FUC), gallic acid (GA), chlorogenic acid (CA), dihydromyricetin (DMY) and hesperidin (HES)) (a), and structural diagrams of different polyphenols (b).

[0024] Fig.10 XRD spectra of different electrospun nanofibers and powder samples; the left picture shows different electrospun nanofibers, and the right picture shows different powder samples.

[0025] Fig.11 The left figure is the TGA curve, and the right figure is the DTG curve.

[0026] Fig.12 The left figure is the TGA curve, and the right figure is the DTG curve.

[0027] Fig.13Fluorescence inversion images of L. plantarum 69-2 encapsulated in different electrospun nanofibers; among them, a represents PVA / FUC / L. plantarum 69-2, b represents PVA / FUC / L. plantarum 69-2 / GA, c represents PVA / FUC / L. plantarum 69-2 / CA, d represents PVA / FUC / L. plantarum 69-2 / HES, and e represents PVA / FUC / L. plantarum69-2 / DMY fiber.

[0028] Fig.14 Antioxidant activity of different electrospun nanofibers.

[0029] Fig.15 Schematic diagram of the electrospinning equipment used in the present invention. DETAILED DESCRIPTION

[0030] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0031] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0032] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0033] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0034] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0035] The "%" described in the present invention, unless otherwise specified, refers to mass percentage.

[0036] The first aspect of the present invention provides a method for preparing polyphenol and probiotic co-encapsulated nanofibers, comprising the following steps:

[0037] Adding polyphenols to a mixed solution of polyvinyl alcohol and fucoidan to obtain a mixed solution of the three;

[0038] Adding probiotics to the blended solution of the three and mixing evenly to obtain an electrospinning solution;

[0039] Electrospinning the electrospinning solution to obtain polyphenol and probiotic co-encapsulated nanofibers;

[0040] The polyphenol is at least one of gallic acid (GA), chlorogenic acid (CA), dihydromyricetin (DMY) and hesperidin (HES); the structural formula of the polyphenol is as follows:

[0041] GA

[0042] CA

[0043] DMY

[0044] HES

[0045] In a preferred embodiment of the present invention, in the blended solution of polyvinyl alcohol and fucoidan, the mass concentration of polyvinyl alcohol is 10%, and the mass concentration of fucoidan is 3%.

[0046] The present invention found in the preliminary experiment that fucoidan with a mass concentration of 3% has a promoting effect on the growth of probiotics (L. plantarum 69-2). When the mass concentration of fucoidan is 1% and 2%, the promoting effect on the growth of L. plantarum 69-2 is not as good as when it is 3%. When the mass concentration is 4%, the promoting effect on the growth of L. plantarum 69-2 is not significantly increased compared with 3%. When the mass concentration is 5%, the promoting effect on the growth of L. plantarum 69-2 decreases. Therefore, the present invention preferably limits the mass concentration of fucoidan to 3%.

[0047] The present invention found in the preliminary experiment that when the mass concentration of polyvinyl alcohol is 10%, the spinning effect is good, the spinning is uniform, and the spinning amount is large. When the mass concentration of polyvinyl alcohol is higher than 10%, the increase in the amount of spinning in the same time is not obvious, and when the mass concentration of polyvinyl alcohol is lower than 10%, the amount of spinning in the same time is small. Therefore, the present invention selects the mass concentration of polyvinyl alcohol to be 10%.

[0048] In a preferred embodiment of the present invention, the concentration of polyphenols in the three-mixed solution is 0.04%.

[0049] The present invention found in the preliminary experiment process that gallic acid, chlorogenic acid, and aurantium have a promoting effect on the growth of Lactobacillus plantarum 69-2 when the mass concentration is 0.04%. When the mass concentration of polyphenols is higher than 0.04%, the effect of promoting the growth of L. plantarum 69-2 decreases. When the mass concentration of polyphenols is lower than 0.04%, the effect of promoting the growth of L. plantarum 69-2 is not as good as when the mass concentration is 0.04%. Therefore, the present invention selects the mass concentration of polyphenols to be 0.04%.

[0050] In a preferred embodiment of the present invention, the probiotic is Lactobacillus plantarum.

[0051] In a preferred embodiment of the present invention, the probiotics further include the steps of culturing to the second generation and resuspending before being added to the three-component blend solution.

[0052] In a preferred embodiment of the present invention, the content of probiotics in the electrospinning solution is 9-10 log CFU / mL

[0053] A high content of probiotics in the electrospinning solution will increase the conductivity of the spinning solution, reduce the viscosity and pH, affect the fiber morphology, and deteriorate the spinning effect. A low content of probiotics in the electrospinning solution will result in a low amount of probiotics embedded in the electrospinning fiber, which cannot embed enough probiotics, affecting the efficacy of the probiotics.

[0054] In a preferred embodiment of the present invention, the electrospinning parameters are set as a spinning voltage of 12 kV, a spinning distance of 15 cm and an injection rate of 0.6 mL / h.

[0055] The second aspect of the present invention provides polyphenol and probiotic co-encapsulated nanofibers prepared by the above-mentioned method for preparing polyphenol and probiotic co-encapsulated nanofibers.

[0056] The third aspect of the present invention provides the use of the above-mentioned polyphenol and probiotic co-encapsulated nanofibers in the preparation of medicines and foods.

[0057] Unless otherwise specified, the experimental raw materials and chemical reagents used in the examples of the present invention are of analytical grade and can be obtained through commercial sources.

[0058] The polyvinyl alcohol used in the embodiments of the present invention has an alcoholysis degree of 88%, medium viscosity, and is of pharmaceutical grade.

[0059] The probiotics used in the embodiments of the present invention are Lactobacillus plantarum 69-2, which has been published in “Lactobacillus plantarum 69-2 Combined with Galacto-Oligosaccharides Alleviates D-Galactose-Induced Aging by Regulating the AMPK / SIRT1 Signaling Pathway and Gut Microbiota in Mice”, Wan Wang, Fei Liu, etc.

[0060] The composition of the MRS liquid culture medium used in the embodiment of the present invention is: peptone 10.0 g / L, beef powder 5.0 g / L, glucose 20.0 g / L, yeast powder 4.0 g / L, sodium acetate 5.0 g / L, dipotassium hydrogen phosphate 2.0 g / L, magnesium sulfate 0.2 g / L, ammonium citrate tribasic 2.0 g / L, manganese sulfate 0.05 g / L and Tween 80 1.0 mL / L.

[0061] The schematic diagram of the electrospinning equipment used in the present invention is as follows Fig.15 shown.

[0062] The present invention will be further described below by way of examples.

[0063] Example 1

[0064] 1. Preparation of different electrospun nanofibers

[0065] (1) Preparation of polyphenol and probiotic co-encapsulated nanofibers, the specific steps are as follows:

[0066] Step 1, dissolving polyvinyl alcohol (PVA) in deionized water to a concentration of 10% (w / v) of PVA in the deionized water, and magnetically stirring at 95° C. to obtain a PVA solution;

[0067] Adding fucoidan (FUC) to the PVA solution to make the concentration of fucoidan in the PVA solution 3% (w / v), stirring magnetically at 25° C., to obtain a PVA / FUC blended solution;

[0068] Different polyphenols (gallic acid (GA), chlorogenic acid (CA), dihydromyricetin (DMY) and hesperidin (HES)) with a mass fraction of 0.04% were added to the PVA / FUC blend solution and completely dissolved under magnetic stirring to obtain a blend solution of the three (labeled as PVA / FUC / GA, PVA / FUC / CA, PVA / FUC / DMY and PVA / FUC / HES mixed solutions for different polyphenols).

[0069] Step 2, preparation of bacterial suspension: take out frozen L.plantarum 69-2 and inoculate it into MRS liquid medium with 2% inoculation amount to culture for 18h-24h to activate the first generation, then inoculate the first generation bacterial solution into new MRS liquid medium with 2% inoculation amount to culture for 18h to activate the second generation, take 30mL of the second generation bacterial solution and centrifuge (4°C, 8000r / min, 5min), remove the supernatant with a sterile pipette and retain the precipitate, then wash it with PBS buffer solution 3 times, and then resuspend it to 1mL. Take 300μL of the resuspended bacterial solution and add it to 5mL of the three mixed solutions, stir magnetically until mixed evenly, and obtain a loaded L.plantarum 69-2 blended solution, which is the electrospinning solution (the content of L.plantarum 69-2 in the electrospinning solution is 9-10log CFU / mL).

[0070] Step 3, electrospinning the electrospinning solution prepared in step 2, and setting the electrospinning parameters as spinning voltage 12 kV, spinning distance 15 cm and injection rate 0.6 mL / h to obtain polyphenol and probiotic co-encapsulated nanofibers, corresponding to different polyphenols GA, CA, DMY and HES, respectively marked as PVA / FUC / L.plantarum 69-2 / GA, PVA / FUC / L.plantarum 69-2 / CA, PVA / FUC / L.plantarum 69-2 / DMY, PVA / FUC / L.plantarum 69-2 / HES.

[0071] (2) Preparation of pure PVA fibers

[0072] Step 1, dissolving polyvinyl alcohol (PVA) in deionized water to a concentration of 10% (w / v) of PVA in the deionized water, and magnetically stirring at 95° C. to obtain a PVA solution;

[0073] Step 2, electrospinning the PVA solution obtained in step 1, wherein the electrospinning parameters are set as spinning voltage 12 kV, spinning distance 15 cm and injection rate 0.6 mL / h to obtain pure PVA fibers.

[0074] (3) Preparation of PVA / FUC fibers

[0075] Step 1, dissolving polyvinyl alcohol (PVA) in deionized water to make the concentration of PVA in the deionized water be 10% (w / v), and magnetically stirring at 95° C. to obtain a PVA solution;

[0076] Adding fucoidan (FUC) to the PVA solution to make the concentration of fucoidan in the PVA solution 3% (w / v), and stirring magnetically at 25° C. to obtain a PVA / FUC blended solution;

[0077] Step 2, electrospinning the PVA / FUC blend solution obtained in step 1, wherein the electrospinning parameters are set as spinning voltage 12 kV, spinning distance 15 cm and injection rate 0.6 mL / h to obtain PVA / FUC fibers.

[0078] (4) Preparation of PVA / FUC / L. plantarum 69-2 fibers

[0079] Step 1, dissolving polyvinyl alcohol (PVA) in deionized water to make the concentration of PVA in the deionized water be 10% (w / v), and magnetically stirring at 95° C. to obtain a PVA solution;

[0080] Adding fucoidan (FUC) to the PVA solution to make the concentration of fucoidan in the PVA solution 3% (w / v), stirring magnetically at 25° C., to obtain a PVA / FUC blended solution;

[0081] Step 2, preparation of bacterial suspension: take out the frozen L.plantarum 69-2 and inoculate it into MRS liquid medium at a 2% inoculation amount to activate the first generation, then inoculate the first generation bacterial solution into a new MRS liquid medium at a 2% inoculation amount to activate the second generation for 18h, take 30mL of the second generation bacterial solution and centrifuge (4°C, 8000r / min, 5min), remove the supernatant with a sterile pipette and retain the precipitate, then wash it 3 times with PBS buffer solution, and then resuspend it to 1mL. Take 300μL of the resuspended bacterial solution and add it to the PVA / FUC blended solution, stir it magnetically until it is evenly mixed, and obtain the loaded L.plantarum 69-2 blended solution, which is the electrospinning solution.

[0082] Step 3, electrospinning the electrospinning solution obtained in step 2, wherein the electrospinning parameters are set as spinning voltage 12 kV, spinning distance 15 cm and injection rate 0.6 mL / h to obtain PVA / FUC / L. plantarum 69-2 fibers.

[0083] 2. Test methods

[0084] 2.1 Detection of solution properties

[0085] (1) Conductivity

[0086] The conductivity of different types of electrospinning solutions was measured by a conductivity meter. The probe of the conductivity meter was immersed in the solution to be tested to measure its conductivity. The measurement condition was 25°C and the measurement was repeated 3 times.

[0087] (2) Viscosity

[0088] The apparent viscosity was measured by a rotational rheometer. The cone plate used had a diameter of 35 mm, an angle of 1°, and a gap of 1 mm. The measurement was carried out at room temperature (25°C) with a shear range of 0.1 to 100 s. -1 , select 0.1s -1 The zero shear viscosity at 2 0° was taken as the apparent viscosity of the solution. The measurement was repeated 3 times.

[0089] (3) pH

[0090] The probe of the pH meter was immersed in different types of electrospinning solutions for measurement at 25° C. The measurement was repeated three times.

[0091] 2.2 Effects of different types of polyphenols on the probiotic effects of L. plantarum 69-2

[0092] L. plantarum 69-2 was cultured to the second generation according to the method of step 2 of Example 1, and 2% (v / v) of the second generation bacterial solution was added to 20 mL of MRS liquid culture medium, and 0.08% of gallic acid, chlorogenic acid, dihydromyricetin and hesperidin were added respectively. After culturing at 37° C. for 20 h, the number of viable bacteria was detected by the pouring method.

[0093] 2.3 Preparation and structural characterization of electrospun uniaxial nanofibers

[0094] 2.3.1 Preparation of electrospun uniaxial nanofibers

[0095] The electrospinning equipment is made by the laboratory and consists of a high-voltage power supply, a syringe propeller and a receiving plate. The specific structure is as follows Fig.15 As shown, a 2.5 mL syringe is used to absorb the spinning solution and placed on the propeller. The syringe is connected to a 16 G needle, and then connected to another 16 G needle through a PTFE hose, and then connected to the positive electrode of a high-voltage power supply. The spinning voltage is 12 kV, the spinning distance is 15 cm, and the injection rate is 0.6 mL / h. The aluminum foil is covered on the collection plate, and the nanofiber membrane is collected on the aluminum foil. The ambient temperature during the spinning process is controlled at 30±5°C, and the humidity is controlled at 55±5%.

[0096] 2.3.2 Structural characterization of uniaxial nanofibers

[0097] (1) Scanning electron microscope observation

[0098] Take the aluminum foil with fibers, cut the fibers and aluminum foil into 8mm×5mm rectangles with scissors, stick them on the stage of the scanning electron microscope with double-sided tape, spray gold on the surface, and observe the morphology and thickness of the nanofibers with a scanning electron microscope. The parameters of the scanning electron microscope are an acceleration voltage of 5kV and a magnification of 10,000 times. Randomly select 100 fibers from the scanning electron microscope image and use ImageJ software to measure the fiber diameter.

[0099] (2) ATR-FTIR analysis

[0100] Fourier transform infrared spectrometer was used to detect the infrared spectra of polyvinyl alcohol (PVA) powder, fucoidan (FUC) powder, four different polyphenol powders (gallic acid, chlorogenic acid, dihydromyricetin and hesperidin), and different electrospun nanofibers. The resolution was set to 4 cm -1 , scanning wavelength range is 4000-500cm -1 , scanned 32 times.

[0101] (3) XRD analysis

[0102] The XRD patterns of PVA powder, FUC powder, four different polyphenol powders, and different electrospun nanofibers were detected by X-ray diffractometer. XRD instrument parameters: Cu-Kα ray, voltage: 40 kV, current: 30 mA, scanning range: 5°-85° (2θ), scanning rate: 2° / min.

[0103] (4) Thermal performance analysis

[0104] PVA powder, FUC powder, four different polyphenol powders, and different electrospun nanofibers were weighed and added into a crucible. In a nitrogen environment, they were heated from 25°C to 700°C at a heating rate of 10°C / min.

[0105] (5) Observation of the distribution of L. plantarum 69-2 in fibers using fluorescence microscopy

[0106] The frozen Rhodamine 123 dye solution in the centrifuge tube was taken out and diluted to 5 μg / mL, added to the resuspended bacterial solution, incubated in the dark at 37°C for 30 min, centrifuged (4°C, 8000r / min, 5min), the residual dye solution in the supernatant was removed and the precipitate was retained, and the above steps were repeated three times with PBS buffer solution to obtain a dyed bacterial solution. According to step 2 of Example 1, the dyed bacterial solution was added to the mixed solution of PVA / FUC, PVA / FUC / GA, PVA / FUC / CA, PVA / FUC / DMY and PVA / FUC / HES, respectively, and mixed evenly in the dark. In order to prevent the quenching of Rhodamine 123, the electrospinning process was carried out in the dark, and the spinning parameters were the same as step 3 of Example 1. A thinner portion of the nanofiber was removed and placed on a glass slide, and the distribution of the dyed L. plantarum 69-2 in the nanofiber membrane was observed using a fluorescence microscope.

[0107] 2.4 Number of viable bacteria before and after packaging

[0108] Take 10 mg of the sample loaded with Lactobacillus plantarum, add it to the PBS buffer solution, stir until the nanofibers are completely dissolved in the PBS buffer solution. Take 100 μL of the PBS buffer solution in which the nanofibers are dissolved, dilute it 10 times, and detect the number of viable bacteria according to the pouring method in the national standard GB 4789.2-2016. Each dilution sample is tested three times in parallel.

[0109] 2.5 Antioxidant properties

[0110] The antioxidant activity of fibers with different formulations was evaluated as follows: 10 mg of fiber sample was dissolved in 1 mL of PBS buffer (pH = 7.4), and then vortexed for 10 min to obtain a solution containing the sample. + and DPPH determination.

[0111] (1) DPPH method:

[0112] Accurately weigh 0.0394 g of DPPH (M = 394.32 g / moL) and dilute to 100 ml with ethanol solution to prepare 1 mmol / L DPPH stock solution. When measuring, dilute 10 times with ethanol (absorb 1 ml and add 9 ml ethanol).

[0113] 1 mL of the solution containing the sample was mixed with 5 mL of DPPH (0.1 mM) solution, and the absorbance was measured at 517 nm in the dark (15 min).

[0114]

[0115] Wherein, A0: absorbance of solution containing only DPPH; Af: absorbance of solution containing sample.

[0116] (2) ABTS method:

[0117] 1) Reagents:

[0118] ①ABTS (7mmol / L): 384.076mg, distilled water to 100mL.

[0119] ② Potassium persulfate (140mmol / L): 3.78434g, distilled water to 100mL.

[0120] 2) ABTS + preparation:

[0121] Mix 5mL ABTS with 88μL potassium persulfate and react at room temperature in the dark for 12-16h to form ABTS + The free radical stock solution was then diluted 40 to 50 times with a PBS solution of pH = 7.4 to make its absorbance at a wavelength of 734 nm to be (0.7 ± 0.02) before use.

[0122] 3) Determination:

[0123] 1 mL of sample solution and 5 mL of diluted ABTS + The solutions were mixed and the absorbance of the solution was measured at 734 nm.

[0124]

[0125] Where A0: absorbance of solution containing only ABTS; Af: absorbance of solution containing sample.

[0126] 2.6 Storage stability

[0127] L. plantarum 69-2 samples packaged by different methods were stored at 4°C and room temperature (25°C), respectively. Samples were taken on the 0th, 1st, 7th, 14th and 21st days, and the number of viable bacteria was detected according to the method in the national standard. The unpackaged L. plantarum 69-2 was used as the control group and sampled at 4°C and room temperature to detect the number of viable bacteria.

[0128] 3. Results and analysis

[0129] 3.1 Study on the co-encapsulation of different types of polyphenols with L. plantarum 69-2 into nanofibers

[0130] 3.1.1 Effects of adding different types of polyphenols on the probiotic effects of L. plantarum 69-2

[0131] Figure 1 To investigate the effects of adding different types of polyphenols on the viable count of L. plantarum 69-2. Figure 1The study added four different types of polyphenols to MRS medium and evaluated the beneficial effects of different types of polyphenols on L. plantarum 69-2 by the changes in the number of viable bacteria. Figure 1 As shown, the viable count of L. plantarum 69-2 without polyphenols was 8.86 log CFU / mL. Compared with the group without polyphenols, the groups with gallic acid (GA), chlorogenic acid (CA), dihydromyricetin (DMY) and hesperidin (HES) added could significantly increase the viable count of L. plantarum 69-2 (P<0.05), by 1.99%, 2.14%, 5.63% and 1.28%, respectively. Among the four groups with polyphenols added to MRS medium, the group with DMY could significantly increase the viable count of L. plantarum 69-2 compared with the groups with other types of polyphenols (P<0.05). There was no significant difference among the groups with GA, chlorogenic acid CA, and HES added (P>0.05). It can be concluded that these four polyphenols can significantly increase the number of viable bacteria of L. plantarum 69-2 (P<0.05), among which DMY has better probiotic activity.

[0132] 3.1.2 Effects of adding different types of polyphenols on the physicochemical properties of electrospinning solution

[0133] The physical and chemical properties of the spinning solution, such as conductivity, viscosity and pH, have a direct impact on the electrospun nanofibers, which is mainly reflected in the spinnability, fiber diameter and morphology. Table 1 analyzes the effects of adding L. plantarum 69-2 and different types of polyphenols on the conductivity, viscosity and pH of the PVA and FUC blended spinning solution. The conductivity and viscosity of the pure PVA solution were 0.34±0.01mS / cm and 41.93±2.65mPa, respectively, which were significantly lower than those of the spinning solutions of other groups (P<0.05), and its pH value was 5.23±0.02, which was significantly higher than that of other solutions (P<0.05). Compared with pure PVA solution, the conductivity of the spinning solution after adding FUC was 1.48±0.02mS / cm, the viscosity was 753.47±5.52mPa, and the pH was 5.03±0.01. The conductivity and viscosity were significantly higher than those of the pure PVA group, and the pH value was significantly lower than that of the pure PVA solution (P<0.05). This is because there are more carboxyl groups on the FUC molecular chain, which makes the FUC molecule negatively charged. As an anionic polyelectrolyte, when FUC is added to the solution system, the charge and conductivity of the solution will increase. The sulfate group of FUC is weakly acidic. When FUC is added to the solution system, the pH value of the spinning solution also decreases. After adding L. plantarum 69-2 to the spinning solution, compared with the PVA / FUC group (i.e., the PVA / FUC blended solution in Example 1), the conductivity of the spinning solution of the PVA / FUC / 69-2 group (i.e., omitting the addition of polyphenols on the basis of Example 1, and the other step parameters are the same as Example 1) increased, and the viscosity and pH decreased, which may be attributed to the fact that L. plantarum 69-2 introduced additional extracellular proteins and ions into the blended solution. The addition of four polyphenols, GA, CA, DMY, and HES, to the spinning solution significantly increased the conductivity compared with the PVA / FUC / 69-2 group (P<0.05). Polyphenols are polar molecules with hydroxyl groups in their structures. The ionization of hydroxyl groups increases the ion concentration of the spinning solution, thereby increasing the conductivity of the spinning solution.

[0134] Table 1 Physicochemical properties of different electrospinning solutions

[0135]

[0136] Note: Different lowercase letters represent significant differences (P<0.05), and the same lowercase letters represent no significant differences (P>0.05).

[0137] 3.1.3 Effects of adding different types of polyphenols on the morphology and diameter distribution of electrospun fibers

[0138] Figure 2-8 is the SEM image and fiber diameter distribution histogram, where Figure 2is the SEM image of pure PVA fiber and the fiber diameter distribution histogram. Figure 3 is the SEM image of PVA / FUC fiber and the fiber diameter distribution histogram, Figure 4 The SEM image and fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 fiber are shown in Figure 2. Figure 5 The SEM image and fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 / GA fiber are shown in Figure 2. Figure 6 The SEM image and fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 / CA fiber are shown in Figure 2. Figure 7 The SEM image and fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 / DMY fiber are shown in Figure 2. Figure 8 Figure 2 is the SEM image and fiber diameter distribution histogram of PVA / FUC / L.plantarum 69-2 / HES fiber. When the polymer (PVA) concentration is set to 10% (w / v) and the applied voltage is 12 kV, Figure 2 As shown in the middle left figure, the average fiber diameter of pure PVA is between 225.50±31.31nm, and the fiber thickness is uniform. After adding FUC, the average fiber diameter is 338.04nm, and the fiber diameter becomes thicker. After adding L.plantarum 69-2, the average fiber diameter is 318.22±55.20nm, and the fiber diameter becomes thicker. This may be because the concentration of the solution increases. The concentration of the spinning solution directly affects its viscosity. The increase in solution concentration increases its viscosity, and the energy accumulated in the system also increases, resulting in an increase in the viscosity of the polymer solution. Under the condition of constant voltage, the tensile force on the jet and the electrospun nanofibers formed decreases, and the average fiber diameter gradually increases. When four polyphenols, GA, CA, DMY and HES, were added to the spinning solution, the average diameter of the fibers with added polyphenols was further reduced compared with the PVA / FUC / L.plantarum 69-2 group. This may be because the conductivity of the solution increased, and the increase in conductivity would increase the surface charge density of the solution jet, increase the tensile strength of the solution, and reduce the average fiber diameter. The average diameter of the fibers with added DMY and HES was smaller than that of the nanofibers with added GA and CA polyphenols. This may be due to the higher viscosity of the two polyphenols GA and CA, and the stronger aggregation of polyphenols.

[0139] like Figure 4-8As shown in the red circle, L. plantarum 69-2 is encapsulated inside the nanofibers. After encapsulating Lactobacillus plantarum, the fibers become locally thicker and oval, and the diameter becomes larger. L. plantarum 69-2 is randomly distributed in multiple fibers and arranged along the fibers. Similar phenomena have been obtained in some other studies. Although L. plantarum 69-2 is initially randomly distributed in the mixed solution, the spinning droplets form a Taylor cone at the needle tip. The sinking flow at the Taylor cone causes L. plantarum 69-2 to flow out along the stretched droplets in a directional manner. Under the action of the high-voltage electric field, the solvent evaporates rapidly, causing the directional outflow of L. plantarum 69-2 to be encapsulated in the PVA / FUC fiber.

[0140] 3.1.4ATR-FTIR analysis

[0141] The characteristic absorption peak of ATR-FTIR reflects the structural characteristics of different substances in the fiber membrane. Therefore, whether there is interaction between the substances, such as hydrogen bonding, can be studied by observing the changes in its peak intensity and peak position. Fig. 9 ATR-FTIR analysis of different electrospun nanofibers is shown. In the spectrum of PVA nanofiber membrane, 3305 cm -1 The broad peak near 2943 cm is caused by OH stretching of intramolecular and intermolecular hydrogen bonds. -1 The broad peak near is the -CH stretching vibration, 1429 cm -1 The broad peak near is the -CH2 bending vibration, 1097 cm -1 The absorption peak at 3045cm may be related to CO stretching or OH bending. The formation of hydrogen bonds in the single PVA nanofibers is possible because the PVA molecular chain contains a large number of hydroxyl groups, which can form hydrogen bonds between or within molecules. Compared with pure PVA nanofibers, after adding FUC, the OH vibration peak appears blue shifted from 3045cm -1 Increased to 3337cm -1 , proving that there is a certain interaction between PVA and FUC, which is due to the formation of hydrogen bonds between PVA and FUC molecules. The number of hydroxyl groups in different polyphenol structures is different, such as Figure 2 In the structural formula of polyphenols, the hydroxyl groups in HES are the most distributed, and accordingly, HES is at 3305cm -1 The signal strength is also the strongest.

[0142] Fig. 9 The results of the spectrum analysis show that no new substances are generated during the electrospinning process, and no obvious chemical reaction occurs between DMY and PVA. Only some complex and relatively weak physical interactions occur between them.

[0143] 3.1.5XRD analysis

[0144] XRD is an effective method to study the microstructure of crystalline materials and some amorphous materials. XRD can be used to analyze the structural changes of materials before and after electrospinning and the compatibility between different components. Figure 3-4 It can be seen that PVA is a monoclinic polymer, and its powder shows a sharp diffraction peak at 2θ=18.507°. However, PVA fibers show a weaker broad diffraction peak at 2θ=18.859°, indicating that PVA fibers exhibit a non-crystalline microstructure and the electrospinning process changes the crystallization state of PVA. It is reported that during the electrospinning process, the rapid evaporation of the solvent and the rapid stretching of the fiber lead to a limited time for fiber recrystallization, which reduces the order and tends to promote the formation of non-crystalline and semi-crystalline structures. It can be seen from the XRD spectrum of FUC powder that there is no diffraction peak. In PVA / FUC spun fibers, 2θ=18.819 shows a weaker broad diffraction peak, which is basically consistent with the diffraction peak of pure PVA fibers. The four polyphenol powders of GA, CA, DMY and HES show sharp characteristic peaks in the XRD spectrum, indicating that GA, CA, DMY and HES are crystalline. The peak width in the fibers added with GA, CA, DMY and HES became wider and the peak value became weaker, which indicates that there is a certain interaction between PVA and polyphenols. This phenomenon occurs because of the formation of hydrogen bonds between PVA and polyphenols.

[0145] 3.1.6 Thermal performance analysis

[0146] TGA is often used to study the thermal stability of polymer materials. Since it is difficult to distinguish the situation of small weight loss from a simple TGA curve, the first-order derivative of the temperature is taken to obtain the DTG curve (thermogravimetric differential). Fig.11 Figure 2 shows the TGA and DTG curves of different electrospun nanofiber samples. The first stage, which occurs below 100°C, is caused by the evaporation of volatile substances and adsorbed moisture, and the weight loss is about 10%. The second thermal degradation stage is between 190-240°C, and the fiber weight loss of PVA / FUC is about 28.23%, the fiber weight loss of PVA / FUC / L.plantarum 69-2 is about 27.37%, the fiber weight loss of PVA / FUC / L.plantarum 69-2 / GA is about 27.21%, the fiber weight loss of PVA / FUC / L.plantarum 69-2 / CA is about 26.79%, the fiber weight loss of PVA / FUC / L.plantarum 69-2 / DMY is about 27.17%, and the fiber weight loss of PVA / FUC / L.plantarum 69-2 / HES is about 27.64%, but due to Fig.12(TGA and DTG curves of different powder samples) It can be seen that there is no such degradation stage in PVA powder and pure PVA nanofibers. The decomposition temperature of PVA powder and pure PVA nanofibers is 260-370℃. The acetyl groups in PVA are converted into acetic acid molecules, and the thermal decomposition of the side chains produces small molecular carbon and hydrocarbons, followed by in-situ chain stripping, resulting in weight loss. Before this stage of FUC powder degradation, the decomposition temperature is between 170-196℃.

[0147] The third thermal degradation stage is between 380-500℃. The reason for this stage is that higher temperature will lead to thermal decomposition of PVA main chain. The thermal degradation curve of PVA / FUC is different from that of PVA powder, FUC powder and pure PVA nanofibers, and has its own unique thermal degradation curve, which may be due to the change of thermal degradation temperature caused by the effect of hydrogen bonding between PVA and FUC. Compared with pure PVA fiber, the total weight loss of PVA / FUC, PVA / FUC / L.plantarum 69-2, PVA / FUC / L.plantarum69-2 / GA, PVA / FUC / L.plantarum 69-2 / CA, PVA / FUC / L.plantarum 69-2 / DMY and PVA / FUC / L.plantarum 69-2 / HES decreased by 9.86%, 8.03%, 8.22%, 7.60%, 6.68% and 4.96%, respectively. This indicates that the addition of FUC, L. plantarum 69-2 and different polyphenols improved the thermal stability of the composite fibers.

[0148] 3.1.7 Observation of the distribution of L. plantarum 69-2 in fibers using fluorescence microscopy

[0149] After observing L. plantarum 69-2 encapsulated outside the electrospun fiber through SEM, the encapsulation of L. plantarum 69-2 in the fiber was further observed through fluorescence microscopy. Rhodamine 123 dye can enter the mitochondria of living cells and show green fluorescence under a fluorescence microscope. Therefore, the living L. plantarum 69-2 cells can show green fluorescence under a fluorescence microscope. Fig.13The distribution of L.plantarum 69-2 was observed using a fluorescence microscope. After spinning, L.plantarum 69-2 showed green fluorescence under a fluorescence microscope. After spinning, L.plantarum 69-2 was linearly arranged along the longitudinal direction of the fiber. Most of L.plantarum 69-2 could be successfully encapsulated into the PVA / FUC fiber, but a small part of L.plantarum 69-2 showing green fluorescence was still distributed outside the PVA / FUC fiber. The main reason for this phenomenon may be that although the sinking flow at the Taylor cone of the needle tip can make part of L.plantarum 69-2 flow out of the droplet. With the rapid evaporation of the external solvent, this part of L.plantarum 69-2 can be successfully encapsulated into the fiber. However, part of L.plantarum 69-2 remains outside the droplet. When the solvent evaporates rapidly and PVA / FUC forms a nanofiber structure, this part of L.plantarum 69-2 is blocked outside the nanofibers present in the nanofiber network.

[0150] 3.1.8 Effect of adding different types of polyphenols on the number of viable bacteria before and after electrospun fiber encapsulation

[0151] As shown in Table 2, the survival rate of L. plantarum 69-2 encapsulated by the blended solutions of different formulations was significantly lower than that before spinning (P<0.05). This is because during the electrospinning process, the high voltage electrostatic field, the rapid evaporation of water and the change of osmotic pressure caused damage to the strain, resulting in a decrease in the number of viable bacteria. Before electrospinning, the number of viable bacteria of L. plantarum 69-2 did not decrease significantly compared with the initial number of viable bacteria, whether in PVA / FUC or in the spinning solution with the addition of GA, CA, DMY and HES (P>0.05). The number of viable bacteria in the two groups of PVA / FUC / 69-2 / DMY and PVA / FUC / 69-2 / HES was significantly increased compared with the initial number of viable bacteria (P<0.05). PVA is biocompatible and is a recognized safe compound that can produce a high oxygen barrier when dried, thereby protecting the biological activity of bacteria. The addition of polyphenols not only did not affect the number of viable bacteria of L. plantarum 69-2, but also better protected its survival.

[0152] Table 2 Number of viable L. plantarum 69-2 encapsulated before and after spinning of different fibers

[0153]

[0154] Note: Different superscript lowercase letters indicate significant differences in the same column (P<0.05), and different superscript uppercase letters indicate significant differences in the same row (P<0.05).

[0155] 3.1.9 Antioxidant analysis of electrospun nanofibers with different types of polyphenols

[0156] The in vitro antioxidant capacity of electrospun nanofibers of different types of polyphenols was determined by DPPH and ABTS free radical scavenging tests. Fig.14 As shown (different lowercase letters in the figure indicate significant differences (P<0.05)). The scavenging rates of DPPH and ABTS free radicals of the electrospun nanofibers in the pure PVA group were 23.63±0.46% and 14.11±0.33%, respectively, which were significantly lower than those in the other groups (P<0.05). The antioxidant activity of the electrospun nanofibers with the addition of FUC and L.plantarum 69-2 was significantly improved compared with the pure PVA group (P<0.05). Among the electrospun nanofibers with the same amount of different types of polyphenols, the scavenging rate of ABTS free radicals of the electrospun nanofibers with the addition of GA, CA, and DMY was higher than that of the HES group (P<0.05), but there was no significant difference among the three groups (P>0.05). The scavenging rate of DPPH free radicals in the DMY group was significantly higher than that in the other three groups (P<0.05), and the scavenging rate of DPPH free radicals in the HES group was lower than that in the other three groups with the addition of polyphenols, but it was still higher than that in the group without the addition of polyphenols. This result indicated that the co-encapsulation of polyphenols and L. plantarum 69-2 could be achieved through electrospun nanofibers, and the antioxidant capacity of electrospun nanofibers could also be effectively improved.

[0157] 3.1.10 Analysis of the storage stability of electrospun nanofibers with different types of polyphenols

[0158] Table 3 records the changes in the number of viable bacteria of L. plantarum 69-2 encapsulated in nanofibers and not encapsulated at 4°C and 25°C for 21 days. Under 4°C storage conditions, the survival rates of L. plantarum 69-2 encapsulated in PVA / FUC / L. plantarum 69-2, PVA / FUC / L. plantarum69-2 / GA, PVA / FUC / L. plantarum 69-2 / CA, PVA / FUC / L. plantarum 69-2 / DMY and PVA / FUC / L. plantarum 69-2 / HES nanofibers were 81.77%, 85.06%, 81.40%, 88.77% and 82.37%, respectively, and the survival rate of L. plantarum 69-2 not encapsulated was 63.67% within 21 days of storage. Compared with unencapsulated L. plantarum 69-2, the survival rate of L. plantarum 69-2 was significantly improved after nanofiber encapsulation, and the number of viable bacteria could still be maintained above 7 log CFU / g after 21 days of storage.

[0159] Under storage conditions of 25℃, the survival rates of L.plantarum 69-2 encapsulated by PVA / FUC / L.plantarum 69-2, PVA / FUC / L.plantarum 69-2 / GA, PVA / FUC / L.plantarum 69-2 / CA, PVA / FUC / L.plantarum 69-2 / DMY and PVA / FUC / L.plantarum69-2 / HES nanofibers were 77.48%, 80.75%, 79.17%, 80.72% and 79.26%, respectively, within 21 days of storage, and the survival rate of unencapsulated L.plantarum 69-2 was 62.56% within 21 days of storage. The viable bacterial counts of L.plantarum 69-2 encapsulated and unencapsulated by nanofibers were lower than those under 4℃ conditions. Compared with 25 °C, the number of viable Lactobacillus rhamnosus 1.0320 encapsulated in nanofibers was relatively higher at 4 °C, indicating that the storage effect of PVA / PEC nanofibers encapsulated L. plantarum 69-2 was better under low temperature conditions. The results showed that PVA / FUC nanofibers with added polyphenols can help improve the storage stability of L. plantarum 69-2 and have potential for application in the preservation of probiotics.

[0160] Table 3 Changes in the number of viable cells of L. plantarum 69-2 encapsulated in nanofibers and not encapsulated at 4℃ and 25℃ for 21 days

[0161]

[0162]

[0163] Note: Different superscript lowercase letters indicate significant differences in the same column (P<0.05).

[0164] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing polyphenol and probiotic co-encapsulated nanofibers, characterized in that: The following steps are involved: Adding polyphenols to a mixed solution of polyvinyl alcohol and fucoidan to obtain a mixed solution of the three; Adding probiotics to the blended solution of the three and mixing evenly to obtain an electrospinning solution; Electrospinning the electrospinning solution to obtain polyphenol and probiotic co-encapsulated nanofibers; The polyphenol is at least one of gallic acid, chlorogenic acid, dihydromyricetin and hesperidin; The mass concentration of polyvinyl alcohol in the mixed solution of polyvinyl alcohol and fucoidan is 10%, and the mass concentration of fucoidan is 3%; The mass concentration of polyphenols in the mixed solution of the three is 0.04%; The probiotic is Lactobacillus plantarum.

2. The method for preparing polyphenol and probiotic co-encapsulated nanofibers according to claim 1, characterized in that: The probiotics also include the steps of culturing to the second generation and resuspending before being added into the three-component blend solution.

3. The method for preparing polyphenol and probiotic co-encapsulated nanofibers according to claim 1, characterized in that: The content of probiotics in the electrospinning solution is 9-10 log CFU / mL.

4. The method for preparing polyphenol and probiotic co-encapsulated nanofibers according to claim 1, characterized in that: The electrospinning parameters were set as follows: spinning voltage 12 kV, spinning distance 15 cm, and injection rate 0.6 mL / h.

5. The polyphenol and probiotic co-encapsulated nanofibers prepared according to the method for preparing polyphenol and probiotic co-encapsulated nanofibers according to any one of claims 1 to 4.

6. Use of the polyphenol and probiotic co-encapsulated nanofibers as claimed in claim 5 in the preparation of medicines and foods.

Citation Information

Patent Citations

  • Nanofiber membrane loaded with prebiotics and / or probiotics as well as preparation and application

    CN108589045A