Preparation method of multifunctional polyethylene blown film and multifunctional polyethylene blown film
A blend of specific additives and processing techniques in polyethylene films addresses the challenges of antistatic, gas barrier, and mechanical properties, achieving durable performance and cost-effectiveness in polyethylene films.
Patent Information
- Application Number
- CN202411395811.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-12-03
AI Technical Summary
Existing polyethylene films face challenges in achieving simultaneous improvements in antistatic properties, gas barrier properties, mechanical properties, and maintaining good processing performance while avoiding issues like filler agglomeration, migration of antistatic agents, and increased production costs.
A preparation method involving a blend of polyethylene matrix, polyethylene glycol monostearate, organically modified layered silicate, maleic anhydride grafted polyethylene, triacetin, antioxidant, and light stabilizer, processed through twin-screw extrusion and film blowing, to create a multifunctional polyethylene blown film.
The method results in durable antistatic performance, enhanced gas barrier properties, improved mechanical properties, high transparency, and cost-effective production without significant cost increase, with potential improvements in processing performance and thermal stability.
Smart Images

Figure BDA0005073726990000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyethylene blown films, in particular to a preparation method of a multifunctional polyethylene blown film and the multifunctional polyethylene blown film. Background Art
[0002] Polyethylene film is widely used in the packaging field due to its excellent processing performance, mechanical properties and chemical stability. However, with the development of industry and technology, the performance requirements of polyethylene film are constantly increasing, especially in terms of antistatic properties, gas barrier properties and comprehensive mechanical properties.
[0003] The existing technology mainly improves the performance of polyethylene film by the following methods:
[0004] 1. Add antistatic agent: Commonly used antistatic agents are cationic, anionic and nonionic. However, these antistatic agents often have the problems of strong migration and poor durability, resulting in unstable long-term antistatic performance of the film.
[0005] 2. Introducing inorganic fillers: such as montmorillonite and silica, to improve gas barrier properties. However, inorganic fillers have poor dispersibility in the polyethylene matrix and are prone to agglomeration, which affects the transparency and mechanical properties of the film.
[0006] 3. Use compatibilizers: such as maleic anhydride grafted polyethylene, to improve the dispersion of fillers. However, using a compatibilizer alone is difficult to achieve both antistatic and gas barrier properties.
[0007] 4. Multi-layer co-extrusion technology: The combination of different functions is achieved through a multi-layer structure, but this method increases production costs and process complexity.
[0008] The main problems of the existing technology:
[0009] 1. Insufficient antistatic performance and durability: Traditional antistatic agents are easy to migrate, resulting in long-term performance degradation and may affect other properties of the film.
[0010] 2. The improvement of gas barrier performance is limited: simply adding inorganic fillers is difficult to form an effective barrier structure and can easily affect the transparency of the film.
[0011] 3. Poor filler dispersion: Inorganic fillers are easy to agglomerate in the polyethylene matrix, affecting the mechanical and optical properties of the film.
[0012] 4. Multifunctionality is difficult to achieve: Existing technologies make it difficult to maintain the basic properties of the film while improving the antistatic properties, gas barrier properties and mechanical properties.
[0013] 5. Balance between processing performance and final performance: Improving certain properties often affects the processing performance or other important properties of the film.
[0014] 6. Trade-off between cost and performance: High-performance additives or complex production processes often significantly increase production costs.
[0015] Based on the above problems, it is of great practical significance and market demand to develop a polyethylene film formula that can simultaneously improve antistatic properties, gas barrier properties and mechanical properties while maintaining good processing performance and cost-effectiveness. Summary of the invention
[0016] In view of the above problems, it is of great practical significance and urgent need to develop a preparation method for multifunctional polyethylene blown film that can simultaneously solve these technical problems.
[0017] The method for preparing a functional polyethylene blown film comprises the following steps:
[0018] (1) Mix the following components:
[0019] 100 parts by weight of polyethylene matrix,
[0020] 0.5-2.0 parts by weight of polyethylene glycol monostearate,
[0021] 1.0-3.0 parts by weight of organic modified layered silicate,
[0022] Maleic anhydride grafted polyethylene 0.3-1.0 parts by weight,
[0023] 0.2-0.8 parts by weight of triacetin,
[0024] Antioxidant 0.05-0.15 parts by weight,
[0025] Light stabilizer 0.05-0.15 parts by weight;
[0026] (2) melt-blending the mixture in step (1) through a twin-screw extruder;
[0027] (3) granulating the molten blend;
[0028] (4) The film is prepared by the film blowing method.
[0029] Preferably, the polyethylene matrix comprises:
[0030] 60-90 parts by weight of linear low-density polyethylene, density 0.918-0.922 g / cm 3 , melt index (190℃ / 2.16kg) is 0.8-1.2g / 10min;
[0031] 10-40 parts by weight of low-density polyethylene, density 0.917-0.921 g / cm 3 , the melt index (190℃ / 2.16kg) is 1.8-2.2g / 10min.
[0032] Preferably, the average molecular weight of the polyethylene glycol monostearate is 1000-2000 g / mol.
[0033] Preferably, the organically modified layered silicate is quaternary ammonium salt-modified montmorillonite, and the organic content is 25-30%.
[0034] Preferably, the maleic anhydride grafted polyethylene has a maleic anhydride grafting rate of 0.5-1.5% and a melt index (190°C / 2.16kg) of 3-5g / 10min.
[0035] Preferably, the antioxidant is Irganox 1010.
[0036] Preferably, the light stabilizer is Tinuvin 770.
[0037] Preferably, the specific steps of melt blending in step (2) are:
[0038] (a) premixing a polyethylene matrix, an organically modified layered silicate, a maleic anhydride grafted polyethylene, an antioxidant and a light stabilizer;
[0039] (b) melt blending the premixed materials through a twin-screw extruder, wherein the temperatures of the extruder are set to 135-140° C., 150-155° C., 165-170° C., 175-180° C., 170-175° C., and 165-170° C. from the feed zone to the die head;
[0040] (c) adding a mixture of polyethylene glycol monostearate and triacetin to a second section feed port of the extruder;
[0041] (d) The screw speed is controlled to be 80-100 rpm and the residence time is 2-3 minutes.
[0042] Preferably, the specific steps of film blowing in step (4) are:
[0043] (a) drying the granulated material to a moisture content of less than 100 ppm;
[0044] (b) preparing the film by a film blowing method, wherein the die temperature is 165-175° C., the die gap is 0.8-1.2 mm, the blow-up ratio is 2.5:1-3.5:1, the pulling speed is 15-25 m / min, and the cooling ring temperature is 15-20° C.;
[0045] (c) The final thickness of the film is controlled to be 25-35 μm.
[0046] The multifunctional polyethylene blown film is prepared by the method.
[0047] Compared with the prior art, the present invention can achieve the following beneficial effects:
[0048] 1. Excellent antistatic performance and its durability: By introducing the synergistic effect of polyethylene glycol monostearate (PEG-SS) and triacetin, a stable hydrophilic layer is formed on the surface of the film, achieving a durable antistatic effect. The long chain structure of PEG-SS has good compatibility with the polyethylene matrix, reducing migration, and the presence of triacetin further enhances this effect.
[0049] 2. Significantly improved gas barrier performance: Organically modified layered silicates form a highly dispersed nanolayer structure in the polyethylene matrix, greatly extending the diffusion path of gas molecules. At the same time, the polar groups of PEG-SS may fill the tiny gaps between the nanolayers, further enhancing the barrier effect.
[0050] 3. Improved mechanical properties: Maleic anhydride grafted polyethylene (PE-g-MAH) as a compatibilizer significantly improves the dispersibility of organically modified layered silicates in the polyethylene matrix, reduces stress concentration points, and improves the tensile strength and elongation at break of the film.
[0051] 4. Excellent transparency: By finely controlling the ratio of each component and improving the dispersibility of the filler, the present invention maintains high transparency of the film while improving functionality.
[0052] 5. Improved thermal stability: The network structure formed between the components enhances the intermolecular interactions and unexpectedly improves the thermal stability of the film, which is of great significance for the service life and high-temperature applications of the film.
[0053] 6. Potential improvement in processing performance: Although not directly tested, it can be inferred from the improvement in mechanical properties and thermal stability that the present invention may improve the processing performance of the film, such as improving melt strength, which is of great significance for bubble stability and product quality consistency during the film blowing process.
[0054] 7. Cost-effectiveness: Through clever formula design, the present invention uses common and relatively economical raw materials, and achieves simultaneous improvement of multiple performances without significantly increasing costs.
[0055] 8. Environmentally friendly: The additives used in the present invention are mostly food grade or biocompatible materials, which reduces the potential risks to the environment and human health.
[0056] In summary, the present invention has achieved breakthroughs in antistatic properties, gas barrier properties, mechanical properties, etc. through unique formula design and synergistic effects between components, providing new ideas and directions for the development of high-performance polyethylene films, and has important theoretical significance and application value. DETAILED DESCRIPTION
[0057] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0058] Example 1
[0059] The method for preparing a functional polyethylene blown film comprises the following steps:
[0060] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0061] 1. Polyethylene matrix: 100 parts by weight
[0062] Linear low-density polyethylene (LLDPE): 60 parts by weight
[0063] Density: 0.918g / cm 3 , Melt index (190℃ / 2.16kg): 0.8g / 10min
[0064] Low-density polyethylene (LDPE): 40 parts by weight
[0065] Density: 0.917 g / cm 3 , Melt index (190℃ / 2.16kg): 1.8g / 10min
[0066] 2. Polyethylene glycol monostearate (PEG-SS): 0.5 parts by weight
[0067] Average molecular weight: 1000 g / mol
[0068] 3. Organic modified layered silicate: 1.0 parts by weight
[0069] Quaternary ammonium salt modified montmorillonite, organic content 25%
[0070] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 0.3 parts by weight
[0071] Maleic anhydride grafting rate: 0.5%, melt index (190℃ / 2.16kg): 3g / 10min
[0072] 5. Triacetin: 0.2 parts by weight
[0073] 6. Antioxidant: 0.05 parts by weight, the antioxidant is Irganox 1010.
[0074] 7. Light stabilizer: 0.05 parts by weight, the light stabilizer Tinuvin 770.
[0075] Preparation method:
[0076] 1. Premixing: Add LLDPE, LDPE, organically modified layered silicate, PE-g-MAH, antioxidant and light stabilizer into a high-speed mixer and mix at 2000 rpm for 5 minutes.
[0077] 2. Melt blending:
[0078] (1) The premixed materials are melt blended through a twin-screw extruder. The temperatures of the extruder are set to 135°C, 150°C, 165°C, 175°C, 170°C, and 165°C from the feed zone to the die head;
[0079] (2) adding a mixture of PEG-SS and triacetin to the second feeding port of the extruder;
[0080] (3) The screw speed was set to 80 rpm and the residence time was controlled at 2 minutes.
[0081] 3. Granulation: The molten blend is granulated by water-cooled strand drawing.
[0082] 4. Film blowing:
[0083] (1) Dry the pelletized material to a moisture content of less than 100 ppm.
[0084] (2) Film preparation by film blowing method:
[0085] Die temperature: 165℃
[0086] Die gap: 0.8mm
[0087] Blowing ratio: 2.5:1
[0088] Traction speed: 15m / min
[0089] Cooling ring temperature: 15°C
[0090] (3) The final thickness of the film is controlled to be 25 μm.
[0091] Example 2
[0092] The method for preparing a functional polyethylene blown film comprises the following steps:
[0093] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0094] 1. Polyethylene matrix: 100 parts by weight
[0095] Linear low-density polyethylene (LLDPE): 75 parts by weight
[0096] Density: 0.920g / cm 3 , Melt index (190℃ / 2.16kg): 1.0g / 10min
[0097] Low-density polyethylene (LDPE): 25 parts by weight
[0098] Density: 0.919 g / cm 3 , Melt index (190℃ / 2.16kg): 2.0g / 10min
[0099] 2. Polyethylene glycol monostearate (PEG-SS): 1.25 parts by weight
[0100] Average molecular weight: 1500 g / mol
[0101] 3. Organic modified layered silicate: 2.0 parts by weight
[0102] Quaternary ammonium salt modified montmorillonite, organic content 27.5%
[0103] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 0.65 parts by weight
[0104] Maleic anhydride grafting rate: 1.0%, melt index (190℃ / 2.16kg): 4g / 10min
[0105] 5. Glyceryl triacetate: 0.5 parts by weight
[0106] 6. Antioxidant: 0.1 parts by weight
[0107] 7. Light stabilizer: 0.1 parts by weight
[0108] Preparation method:
[0109] 1. Premixing: Add LLDPE, LDPE, organically modified layered silicate, PE-g-MAH, antioxidant and light stabilizer into a high-speed mixer and mix at 2250 rpm for 6 minutes.
[0110] 2. Melt blending:
[0111] (1) The premixed materials are melt blended through a twin-screw extruder. The temperatures of the extruder are set to 137.5°C, 152.5°C, 167.5°C, 177.5°C, 172.5°C, and 167.5°C from the feed zone to the die head;
[0112] (2) Add a mixture of PEG-SS and triacetin to the second feeding port of the extruder.
[0113] (3) The screw speed was set to 90 rpm and the residence time was controlled at 2.5 minutes.
[0114] 3. Granulation: The molten blend is granulated by water-cooled strand drawing.
[0115] 4. Film blowing:
[0116] (1) Dry the pelletized material to a moisture content of less than 100 ppm.
[0117] (2) Film preparation by film blowing method:
[0118] Die temperature: 170℃
[0119] Die gap: 1.0mm
[0120] Blowing ratio: 3:1
[0121] Traction speed: 20m / min
[0122] Cooling ring temperature: 17.5℃
[0123] (3) The final thickness of the film is controlled to be 30 μm.
[0124] Example 3
[0125] The method for preparing a functional polyethylene blown film comprises the following steps:
[0126] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0127] 1. Polyethylene matrix: 100 parts by weight
[0128] Linear low-density polyethylene (LLDPE): 90 parts by weight
[0129] Density: 0.922g / cm 3 , Melt index (190℃ / 2.16kg): 1.2g / 10min
[0130] Low-density polyethylene (LDPE): 10 parts by weight
[0131] Density: 0.921 g / cm 3 , Melt index (190℃ / 2.16kg): 2.2g / 10min
[0132] 2. Polyethylene glycol monostearate (PEG-SS): 2.0 parts by weight
[0133] Average molecular weight: 2000g / mol
[0134] 3. Organic modified layered silicate: 3.0 parts by weight
[0135] Quaternary ammonium salt modified montmorillonite, organic content 30%
[0136] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 1.0 parts by weight
[0137] Maleic anhydride grafting rate: 1.5%, melt index (190℃ / 2.16kg): 5g / 10min
[0138] 5. Triacetin: 0.8 parts by weight
[0139] 6. Antioxidant: 0.15 parts by weight
[0140] 7. Light stabilizer: 0.15 parts by weight
[0141] Preparation method:
[0142] 1. Premixing: Add LLDPE, LDPE, organically modified layered silicate, PE-g-MAH, antioxidant and light stabilizer into a high-speed mixer and mix at 2500 rpm for 7 minutes.
[0143] 2. Melt blending:
[0144] (1) The premixed materials are melt blended through a twin-screw extruder. The temperatures of the extruder are set as follows from the feed zone to the die: 140°C, 155°C, 170°C, 180°C, 175°C, 170°C
[0145] (2) Add a mixture of PEG-SS and triacetin to the second feeding port of the extruder.
[0146] (3) The screw speed was set to 100 rpm and the residence time was controlled at 3 minutes.
[0147] 3. Granulation: The molten blend is granulated by water-cooled strand drawing.
[0148] 4. Film blowing:
[0149] (1) Dry the pelletized material to a moisture content of less than 100 ppm.
[0150] (2) Film preparation by film blowing method:
[0151] Die temperature: 175℃
[0152] Die gap: 1.2mm
[0153] Blowing ratio: 3.5:1
[0154] Traction speed: 25m / min
[0155] Cooling ring temperature: 20℃
[0156] (3) The final thickness of the film is controlled to be 35 μm.
[0157] Example 4
[0158] The method for preparing a functional polyethylene blown film comprises the following steps:
[0159] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0160] 1. Polyethylene matrix: 100 parts by weight
[0161] Linear low-density polyethylene (LLDPE): 80 parts by weight
[0162] Density: 0.920g / cm 3 , Melt index (190℃ / 2.16kg): 1.0g / 10min
[0163] Low-density polyethylene (LDPE): 20 parts by weight
[0164] Density: 0.919 g / cm 3 , Melt index (190℃ / 2.16kg): 2.0g / 10min
[0165] 2. Polyethylene glycol monostearate (PEG-SS): 1.5 parts by weight
[0166] Average molecular weight: 1500 g / mol
[0167] 3. Organic modified layered silicate: 2.5 parts by weight
[0168] Quaternary ammonium salt modified montmorillonite, organic content 27.5%
[0169] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 0.8 parts by weight
[0170] Maleic anhydride grafting rate: 1.0%, melt index (190℃ / 2.16kg): 4g / 10min
[0171] 5. Glycerol triacetate: 0.6 parts by weight
[0172] 6. Antioxidant: 0.12 parts by weight
[0173] 7. Light stabilizer: 0.12 parts by weight
[0174] Preparation method:
[0175] 1. Premixing: Add LLDPE, LDPE, organically modified layered silicate, PE-g-MAH, antioxidant and light stabilizer into a high-speed mixer and mix at 2350 rpm for 6.5 minutes.
[0176] 2. Melt blending:
[0177] (1) The premixed materials were melt blended through a twin-screw extruder. The temperatures of the extruder were set from the feed zone to the die head as follows: 138°C, 153°C, 168°C, 178°C, 173°C, 168°C
[0178] (2) Add a mixture of PEG-SS and triacetin to the second feeding port of the extruder.
[0179] (3) The screw speed was set to 95 rpm and the residence time was controlled at 2.7 minutes.
[0180] 3. Granulation: The molten blend is granulated by water-cooled strand drawing.
[0181] 4. Film blowing:
[0182] (1) Dry the pelletized material to a moisture content of less than 100 ppm.
[0183] (2) Film preparation by film blowing method:
[0184] Die temperature: 172°C
[0185] Die gap: 1.1mm
[0186] Blowing ratio: 3.2:1
[0187] Traction speed: 22m / min
[0188] Cooling ring temperature: 18°C
[0189] (3) The final thickness of the film is controlled to be 32 μm.
[0190] Comparative Example 1 (corresponding to Example 1, lacking polyethylene glycol monostearate):
[0191] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0192] 1. Polyethylene matrix: 100 parts by weight (same as Example 1)
[0193] 2. Polyethylene glycol monostearate (PEG-SS): 0 parts by weight
[0194] 3. Organic modified layered silicate: 1.0 part by weight (same as in Example 1)
[0195] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 0.3 parts by weight (same as Example 1)
[0196] 5. Glycerol triacetate: 0.2 parts by weight (same as in Example 1)
[0197] 6. Antioxidant: 0.05 parts by weight (same as Example 1)
[0198] 7. Light stabilizer: 0.05 parts by weight (same as Example 1)
[0199] Preparation method:
[0200] Same as Example 1, but without adding PEG-SS in the melt blending step.
[0201] Comparative Example 2 (corresponding to Example 2, replacing the organically modified layered silicate with ordinary montmorillonite):
[0202] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0203] 1. Polyethylene matrix: 100 parts by weight (same as Example 2)
[0204] 2. Polyethylene glycol monostearate (PEG-SS): 1.25 parts by weight (same as Example 2)
[0205] 3. Ordinary montmorillonite: 2.0 parts by weight
[0206] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 0.65 parts by weight (same as Example 2)
[0207] 5. Glycerol triacetate: 0.5 parts by weight (same as in Example 2)
[0208] 6. Antioxidant: 0.1 parts by weight (same as Example 2)
[0209] 7. Light stabilizer: 0.1 parts by weight (same as Example 2)
[0210] Preparation method:
[0211] Same as Example 2, but using ordinary montmorillonite instead of the organically modified layered silicate.
[0212] Comparative Example 3 (corresponding to Example 3, lacking maleic anhydride grafted polyethylene):
[0213] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0214] 1. Polyethylene matrix: 100 parts by weight (same as Example 3)
[0215] 2. Polyethylene glycol monostearate (PEG-SS): 2.0 parts by weight (same as Example 3)
[0216] 3. Organic modified layered silicate: 3.0 parts by weight (same as Example 3)
[0217] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 0 parts by weight
[0218] 5. Glycerol triacetate: 0.8 parts by weight (same as in Example 3)
[0219] 6. Antioxidant: 0.15 parts by weight (same as Example 3)
[0220] 7. Light stabilizer: 0.15 parts by weight (same as Example 3)
[0221] Preparation method:
[0222] Same as Example 3, but without adding PE-g-MAH.
[0223] Comparative Example 4 (corresponding to Example 4, increasing the content of polyethylene glycol monostearate):
[0224] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0225] 1. Polyethylene matrix: 100 parts by weight (same as Example 4)
[0226] 2. Polyethylene glycol monostearate (PEG-SS): 3.0 parts by weight
[0227] 3. Organic modified layered silicate: 2.5 parts by weight (same as Example 4)
[0228] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 0.8 parts by weight (same as Example 4)
[0229] 5. Triacetin: 0.6 parts by weight (same as in Example 4)
[0230] 6. Antioxidant: 0.12 parts by weight (same as Example 4)
[0231] 7. Light stabilizer: 0.12 parts by weight (same as Example 4)
[0232] Preparation method:
[0233] Same as Example 4, but the amount of PEG-SS added was increased to 3.0 parts by weight.
[0234] Comparative Example 5 (corresponding to Example 1, lacking triacetin):
[0235] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0236] 1. Polyethylene matrix: 100 parts by weight (same as Example 1)
[0237] 2. Polyethylene glycol monostearate (PEG-SS): 0.5 parts by weight (same as Example 1)
[0238] 3. Organic modified layered silicate: 1.0 part by weight (same as in Example 1)
[0239] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 0.3 parts by weight (same as Example 1)
[0240] 5. Glyceryl triacetate: 0 parts by weight
[0241] 6. Antioxidant: 0.05 parts by weight (same as Example 1)
[0242] 7. Light stabilizer: 0.05 parts by weight (same as Example 1)
[0243] Preparation method:
[0244] Same as Example 1, but without adding triacetin.
[0245] Comparative Example 6 (corresponding to Example 2, reducing the content of organically modified layered silicate):
[0246] Raw material components (based on 100 parts by weight of polyethylene matrix):
[0247] 1. Polyethylene matrix: 100 parts by weight (same as Example 2)
[0248] 2. Polyethylene glycol monostearate (PEG-SS): 1.25 parts by weight (same as Example 2)
[0249] 3. Organic modified layered silicate: 0.5 parts by weight
[0250] 4. Maleic anhydride grafted polyethylene (PE-g-MAH): 0.65 parts by weight (same as Example 2)
[0251] 5. Glycerol triacetate: 0.5 parts by weight (same as in Example 2)
[0252] 6. Antioxidant: 0.1 parts by weight (same as Example 2)
[0253] 7. Light stabilizer: 0.1 parts by weight (same as Example 2)
[0254] Preparation method:
[0255] The same as Example 2, but the amount of organically modified layered silicate added was reduced to 0.5 parts by weight.
[0256] 1. Comparative Example 1 verifies the key role of PEG-SS in improving antistatic properties.
[0257] 2. Comparative Example 2 demonstrates the advantages of organically modified layered silicate in improving gas barrier properties compared to ordinary montmorillonite.
[0258] 3. Comparative Example 3 demonstrates the importance of PE-g-MAH as a compatibilizer, especially in improving filler dispersibility.
[0259] 4. Comparative Example 4 demonstrates the negative effects that may be caused by excessive PEG-SS content.
[0260] 5. Comparative Example 5 verifies the role of triacetin in improving film flexibility and synergistic antistatic effect.
[0261] 6. Comparative Example 6 shows that insufficient content of organically modified layered silicate may lead to decreased gas barrier properties.
[0262] In order to verify the effectiveness of the present invention, the applicant designed the following test model to evaluate the effectiveness of the solution:
[0263] 1. Antistatic performance test
[0264] Experimental conditions: temperature 23±2℃, relative humidity 50±5%
[0265] Experimental method: According to ASTM D257 standard, the surface resistivity of the film was measured using a high resistance meter.
[0266] 2. Gas barrier performance test
[0267] Experimental conditions: temperature 23±2℃, relative humidity 0%
[0268] Experimental method: According to ASTM D3985 standard, the oxygen permeability of the film was measured using an oxygen permeability tester.
[0269] 3. Mechanical properties test
[0270] Experimental conditions: temperature 23±2℃, relative humidity 50±5%
[0271] Experimental method: According to ASTM D882 standard, the tensile strength and elongation at break of the film were measured using a universal testing machine.
[0272] 4. Transparency test
[0273] Experimental conditions: temperature 23±2℃
[0274] Experimental method: According to ASTM D1003 standard, the haze of the film is measured using a haze meter.
[0275] 5. Dispersion Assessment
[0276] Experimental method: Transmission electron microscopy (TEM) was used to observe the cross-sectional morphology of the film and evaluate the dispersion state of the filler.
[0277] 6. Thermal stability test
[0278] Experimental conditions: nitrogen atmosphere, heating rate 10℃ / min
[0279] Experimental method: The thermal decomposition temperature of the film (Td,5%, the temperature at which 5% mass loss) was measured using a thermogravimetric analyzer (TGA)
[0280] The test results are shown in the following table:
[0281]
[0282] According to the test results, Example 3 exhibits the best comprehensive performance and can be regarded as the best embodiment of the present invention.
[0283] Analysis and discussion:
[0284] 1. Antistatic performance: The surface resistivity of Examples 1-4 is all lower than 1011Ω / sq, showing excellent antistatic performance. Comparative Example 1 lacks PEG-SS, resulting in significantly reduced antistatic performance. This demonstrates the key role of PEG-SS in providing antistatic performance.
[0285] 2. Gas barrier properties: The oxygen permeability of Examples 1-4 is significantly lower than that of the comparative examples, especially comparative example 2 (using ordinary montmorillonite) and comparative example 6 (insufficient content of organically modified layered silicate). This shows the importance of organically modified layered silicate in improving gas barrier properties.
[0286] 3. Mechanical properties: The tensile strength and elongation at break of Examples 1-4 are better than those of the comparative examples, especially comparative example 3 (lacking PE-g-MAH). This demonstrates the role of PE-g-MAH as a compatibilizer in improving filler dispersion and enhancing film mechanical properties.
[0287] 4. Transparency: Examples 1-4 have lower haze values, indicating good transparency. Comparative Examples 3 and 4 have higher haze values, indicating that the lack of PE-g-MAH and the high content of PEG-SS affect the transparency of the film.
[0288] 5. Thermal stability: The thermal decomposition temperatures of Examples 1-4 are higher than those of the comparative example, indicating that the formulation of the present invention improves the thermal stability of the film.
[0289] Unexpected technical effects:
[0290] 1. Synergistic antistatic effect: The combination of PEG-SS and triacetin not only provides excellent antistatic performance, but also maintains low haze. This synergistic effect may be due to the special microstructure formed by the two additives on the film surface, which can effectively dissipate static electricity without affecting the transmission of light.
[0291] 2. Enhanced gas barrier properties: The combination of organically modified layered silicate, PE-g-MAH and PEG-SS produced a gas barrier effect beyond expectations. This may be because PE-g-MAH promoted the exfoliation of organically modified layered silicate, while PEG-SS filled the gaps between nanolayers, forming a more complex gas diffusion path.
[0292] 3. Simultaneous improvement of mechanical properties and thermal stability: The formulation of the present invention not only improves the mechanical properties of the film, but also unexpectedly improves the thermal stability. This may be due to the formation of a more stable network structure between the components, which enhances the interaction between molecules.
[0293] 4. Improvement in processing performance: Although not directly tested, it can be inferred from the improvement in mechanical properties and thermal stability that the formulation of the present invention may also improve the processing performance of the film, such as improving melt strength and thermal stability, which is of great significance for bubble stability and product quality consistency during the film blowing process.
[0294] 5. Long-term performance stability: Although this test does not involve long-term performance, it can be inferred from the balanced improvement of various indicators that the film of the present invention may have better long-term performance stability, such as the durability of antistatic performance and the long-term retention of barrier performance.
[0295] These unexpected technical effects fully demonstrate the innovation of the invention in formula design and the synergy between the components, and provide new ideas and directions for the development of high-performance polyethylene films.
Claims
1. A method for preparing a multifunctional polyethylene blown film, characterized in that: The following steps are involved: (1) Mix the following components: 100 parts by weight of polyethylene matrix, 0.5-2.0 parts by weight of polyethylene glycol monostearate, 1.0-3.0 parts by weight of organic modified layered silicate, Maleic anhydride grafted polyethylene 0.3-1.0 parts by weight, 0.2-0.8 parts by weight of triacetin, Antioxidant 0.05-0.15 parts by weight, Light stabilizer 0.05-0.15 parts by weight; (2) melt-blending the mixture in step (1) through a twin-screw extruder; (3) granulating the molten blend; (4) The film is prepared by the film blowing method.
2. The preparation method according to claim 1, characterized in that: The polyethylene matrix comprises: 60-90 parts by weight of linear low-density polyethylene, density 0.918-0.922 g / cm 3 , melt index (190℃ / 2.16kg) is 0.8-1.2g / 10min; 10-40 parts by weight of low-density polyethylene, density 0.917-0.921 g / cm 3 , the melt index (190℃ / 2.16kg) is 1.8-2.2g / 10min.
3. The preparation method according to claim 1, characterized in that: The average molecular weight of the polyethylene glycol monostearate is 1000-2000 g / mol.
4. The preparation method according to claim 1, characterized in that: The organic modified layered silicate is quaternary ammonium salt modified montmorillonite, and the organic content is 25-30%.
5. The preparation method according to claim 1, characterized in that: The maleic anhydride grafted polyethylene has a maleic anhydride grafting rate of 0.5-1.5% and a melt index (190°C / 2.16kg) of 3-5g / 10min.
6. The preparation method according to claim 1, characterized in that: The antioxidant is Irganox1010.
7. The preparation method according to claim 1, characterized in that: The light stabilizer is Tinuvin770.
8. The preparation method according to claim 1, characterized in that: The specific steps of melt blending in step (2) are: (a) premixing a polyethylene matrix, an organically modified layered silicate, a maleic anhydride grafted polyethylene, an antioxidant and a light stabilizer; (b) melt blending the premixed materials through a twin-screw extruder, wherein the temperatures of the extruder are set to 135-140° C., 150-155° C., 165-170° C., 175-180° C., 170-175° C., and 165-170° C. from the feed zone to the die head; (c) adding a mixture of polyethylene glycol monostearate and triacetin to a second section feed port of the extruder; (d) The screw speed is controlled to be 80-100 rpm and the residence time is 2-3 minutes.
9. The preparation method according to claim 1, characterized in that: The specific steps of film blowing in step (4) are: (a) drying the granulated material to a moisture content of less than 100 ppm; (b) preparing the film by a film blowing method, wherein the die temperature is 165-175° C., the die gap is 0.8-1.2 mm, the blow-up ratio is 2.5:1-3.5:1, the pulling speed is 15-25 m / min, and the cooling ring temperature is 15-20° C.; (c) The final thickness of the film is controlled to be 25-35 μm.
10. A multifunctional polyethylene blown film prepared by the method according to any one of claims 1 to 9.
Citation Information
Cited By
Multi-layer co-extrusion modified composite film as well as preparation method and application thereof
CN121181956A
A method for preparing an antistatic scratch-resistant regenerated film by in-situ capacity modification of recycled packaging bag waste and a regenerated film
CN122978358A