Carbon paper for fuel cell and preparation method thereof
By performing vapor deposition on the carbon paper precursor and multiple low-concentration resin impregnation treatments, the crack problem of carbon paper during pyrolysis at high temperature is solved, and its conductive and mechanical properties are improved.
Patent Information
- Application Number
- CN202410094007.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-01-23
AI Technical Summary
The resin reacts violently during high temperature pyrolysis, resulting in cracks in carbon paper and reducing its conductive and mechanical properties.
The vapor deposition method is used to deposit carbon on the surface of carbon fibers, connecting breakpoints and reducing the proportion of resin. Through multiple low-concentration resin impregnation and hot pressing treatments, a uniform three-dimensional network structure is formed, reducing the violentness of the resin pyrolysis reaction.
It improves the conductive and mechanical properties of carbon paper, reduces the occurrence of cracks, and enhances the structural integrity and pore uniformity of carbon paper.
Smart Images

Figure BDA0004677913010000081 
Figure BDA0004677913010000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fuel cell carbon paper, and in particular to a carbon paper for fuel cells and a preparation method thereof. Background Art
[0002] Fuel cells are energy conversion devices that directly and efficiently convert the chemical energy of fuel and oxidant into electrical energy. Their competitive advantage of clean power generation makes them at the forefront of research and application in various fields. Among the many types of fuel cells, proton exchange membrane fuel cells have attracted widespread attention due to their high energy conversion efficiency, fast startup, simple design and environmental friendliness. They are considered to be an emerging power source for transportation, fixed and portable applications. The gas diffusion layer (GDL) in proton exchange membrane fuel cells supports the catalyst layer, collects current and provides a path for the reaction gas and product. Therefore, it is required to have excellent mechanical properties, conductivity, pore structure and uniformity. When the design of GDL is unreasonable, the water generated by the reaction will not be able to be discharged from the battery normally, forcing the battery to stop working. Therefore, the design and optimization of GDL plays an important role in improving and enhancing the water management ability and gas transmission efficiency of the battery.
[0003] GDL is usually composed of a porous substrate (MPS) and a microporous layer (MPL). MPS is generally made of carbon fiber paper (abbreviated as carbon paper), carbon fiber woven cloth, non-woven fabric, and carbon black paper; MPL is usually a mixture of carbon black and polytetrafluoroethylene (PTFE) coated on the surface of MPS. Carbon fiber paper is the first choice for substrate material due to its mature manufacturing process, stable performance, relatively low cost, and strong reprocessing adaptability.
[0004] At present, the main method for preparing carbon paper is wet preparation. The main process is to mix short-cut carbon fibers of the same or different lengths, dispersants, and binders to make paper, liquid phase impregnation resin and hot pressing and curing, and finally carbonization and graphitization high temperature treatment.
[0005] The related art discloses a method for preparing carbon paper, which includes the following steps: mixing a plurality of carbon fibers of different lengths with a dispersion liquid respectively, and then making paper to obtain a plurality of carbon fiber felts with carbon fibers of different lengths; impregnating the plurality of carbon fiber felts with resin respectively and drying them, and then stacking the dried plurality of carbon fiber felts in sequence according to the length of the carbon fibers, and hot pressing them at 0.1 MPa to 5 MPa to obtain a carbon paper preform; and sequentially carbonizing and graphitizing the carbon paper preform to obtain carbon paper.
[0006] Regarding the above-mentioned related technologies, since the carbon fiber felt needs to be impregnated with a resin with a large load, the resin reacts violently during high-temperature pyrolysis, causing cracks in the carbon paper, thereby reducing the conductive and mechanical properties of the carbon paper. Summary of the invention
[0007] In order to improve the electrical conductivity and mechanical properties of carbon paper, the present application provides a carbon paper for a fuel cell and a preparation method thereof.
[0008] In a first aspect, the present application provides a method for preparing carbon paper for a fuel cell, using the following technical solution:
[0009] A method for preparing carbon paper for a fuel cell comprises the following steps:
[0010] Pyrolytic carbon deposition: The carbon paper precursor is vapor deposited to obtain deposited carbon paper;
[0011] Loading resin: Thermosetting resin is loaded on the deposited carbon paper, and then subjected to low-temperature pre-curing, hot pressing and carbonization treatments to obtain densified carbon paper;
[0012] Impregnation treatment: prepare a thermosetting resin ethanol solution, impregnate the densified carbon paper in the thermosetting resin ethanol solution, and sequentially undergo low-temperature pre-curing, hot pressing and carbonization treatments;
[0013] Repeated impregnation: Repeat the impregnation treatment step more than once, and the concentration of the thermosetting resin ethanol solution used for each impregnation is gradually reduced to obtain carbonized carbon paper;
[0014] Graphitization treatment: The carbonized carbon paper is subjected to high-temperature graphitization treatment to obtain carbon paper for fuel cells.
[0015] By adopting the above-mentioned technical scheme, since the present application first performs vapor deposition on the carbon paper precursor, the deposited carbon is wrapped on the surface of the carbon fiber and connects the breakpoints of the carbon fiber, which plays a structural strengthening role on the carbon fiber network. In addition, the introduced deposited carbon can reduce the proportion of resin carbon and reduce the probability of carbon paper cracking due to excessive carbonization and pyrolysis of the resin; and then through multiple impregnation treatments, the three-dimensional network structure is enhanced by resin bonding, and the resin shrinks and fills large gaps when carbonized at high temperature, which can strengthen the gaps between the carbon fibers, making the carbon paper pores more uniform and the conductive path more complete. The resin is impregnated in small amounts and multiple times, so that the resin will not react too violently during carbonization and pyrolysis, reducing the probability of carbon paper cracking and improving the conductive properties and mechanical properties of the carbon paper.
[0016] Optionally, in the pyrolytic carbon deposition step, the vapor deposition temperature is 900-1300° C., the time is 0.7-3 h, and the carbon source gas flow rate is 600-1000 mL / min.
[0017] By adopting the above technical solution, sufficient deposited carbon can be deposited on the carbon paper precursor within the above parameter range.
[0018] Optionally, in the repeated impregnation step, the impregnation treatment step is repeated twice, the concentration of the thermosetting resin ethanol solution used in the first time is 7-10wt%, and the impregnation time is 1-4min, the concentration of the thermosetting resin ethanol solution used in the second time is 4-6wt%, and the impregnation time is 5-8min, and the concentration of the thermosetting resin ethanol solution used in the third time is 1-3wt%, and the impregnation time is 9-12min.
[0019] By adopting the above technical solution, the concentration of thermosetting resin decreases gradually, which can fill the large pores to form small pores more gently, and improve the conductive properties and mechanical properties of carbon paper as much as possible while ensuring the porosity.
[0020] Optionally, in the resin loading step, the low temperature pre-curing temperature is 80-100° C., the low temperature pre-curing time is 1-1.5 h; the hot pressing temperature is 130-180° C., the hot pressing pressure is 1-8 MPa, and the hot pressing time is 40-60 min;
[0021] The carbonization temperature is 900-1400°C and the carbonization time is 3-4h.
[0022] By adopting the above technical solution, within the above parameter range, the resin in the resin loading step can be fully combined with the carbon fibers and carbonized to form resin carbon.
[0023] Optionally, in the dipping step, the low-temperature pre-curing temperature is 80-100° C., and the low-temperature pre-curing time is 40-60 min;
[0024] The hot pressing temperature is 130-180°C, the hot pressing pressure is 1-8MPa, and the hot pressing time is 10-30min;
[0025] The carbonization temperature is 900-1400°C and the carbonization time is 1-2h.
[0026] By adopting the above technical solution, within the above parameter range, the resin in the impregnation step can fill the large pores and gaps of the carbon fiber and slowly undergo pyrolysis reaction, thereby reducing the probability of cracks in the carbon paper and improving the electrical conductivity and mechanical properties of the carbon paper.
[0027] Optionally, in the impregnation step, the densified carbon paper is immersed in a thermosetting resin ethanol solution and evacuated to below -0.1 MPa.
[0028] By adopting the above technical solution, vacuuming is conducive to the escape of gas inside the dense carbon paper, forming gaps and channels, which is conducive to the infiltration and diffusion of thermosetting resin, improves the conductive channel of carbon paper, and enhances the three-dimensional structural strength of carbon fiber.
[0029] Optionally, the carbon paper precursor has a thickness of 0.4-0.5 mm and a gram weight of 20-60 g / m2 .
[0030] By adopting the above technical solution and controlling the thickness and grammage of the carbon paper precursor, the performance of the final carbon paper is made more stable.
[0031] Optionally, the thermosetting resin is selected from any one of furan resin, phenolic resin and furfural resin.
[0032] By adopting the above technical solution, the above resins are all high carbon residue resins, which produce less gaseous matter during high-temperature carbonization, have a small resin shrinkage rate, and produce fewer cracks on carbon paper, thereby improving the structural integrity of the carbon paper.
[0033] In a second aspect, the present application provides a carbon paper for a fuel cell, which adopts the following technical solution:
[0034] A carbon paper for fuel cells is prepared by adopting the preparation method of the carbon paper for fuel cells mentioned above.
[0035] In a third aspect, the present application provides a gas diffusion layer, which adopts the following technical solution:
[0036] A gas diffusion layer comprises a microporous layer and a base layer which are stacked in sequence, wherein the material of the base layer comprises the above-mentioned carbon paper for fuel cells.
[0037] In a fourth aspect, the present application provides a fuel cell, which adopts the following technical solution:
[0038] A fuel cell comprises the above-mentioned gas diffusion layer.
[0039] In summary, this application has the following beneficial effects:
[0040] 1. Since the present application first performs vapor deposition on the carbon paper precursor, it plays a structural strengthening role on the carbon fiber network. In addition, the introduced deposited carbon can reduce the proportion of resin carbon, and reduce the probability of carbon paper cracking due to excessive carbonization and pyrolysis of the resin; then through multiple impregnation treatments, the three-dimensional network structure is enhanced by resin bonding, and the conductive path is more complete. The resin is impregnated in small amounts and multiple times, so that the resin will not react too violently during carbonization and pyrolysis, reducing the probability of carbon paper cracking, and improving the conductive properties and mechanical properties of carbon paper.
[0041] 2. In the present application, vacuum impregnation is preferably used. Vacuuming is conducive to the escape of gas inside the carbon paper, forming gaps and channels, which is conducive to the infiltration and diffusion of thermosetting resin, improving the conductive channel of carbon paper, and enhancing the three-dimensional structural strength of carbon fiber.
[0042] 3. By optimizing the low-temperature thermal curing, hot pressing and carbonization parameters, the present application can enable the resin in the impregnation step to fill the large pores and gaps of the carbon fibers and slowly carry out the pyrolysis reaction, thereby reducing the probability of cracks in the carbon paper and improving the electrical conductivity and mechanical properties of the carbon paper. DETAILED DESCRIPTION
[0043] The present application is further described in detail below with reference to the embodiments.
[0044] The carbon paper precursor of the present application can be a commercially available product or a homemade product. The following example illustrates the preparation method of the homemade carbon paper precursor. The thickness of the carbon paper precursor is 0.4-0.5 mm and the weight is 20-60 g / m 2 .
[0045] Preparation Example
[0046] Preparation Example 1
[0047] A method for preparing a carbon paper precursor comprises the following steps:
[0048] (1) mixing sodium carboxymethyl cellulose and water and stirring them uniformly to obtain a dispersion with a mass concentration of 0.3 wt %;
[0049] (2) adding carbon fibers with a diameter of 7 μm and a length of 3-10 mm into the dispersion and stirring evenly, wherein the mass concentration of the carbon fibers in the dispersion is 3 wt %, to obtain a carbon fiber papermaking slurry;
[0050] (3) Making paper from the carbon fiber papermaking slurry to obtain a carbon fiber wet paper web, which is then pressed and dried to obtain a carbon paper precursor.
[0051] Example
[0052] Example 1
[0053] A method for preparing carbon paper for a fuel cell comprises the following steps:
[0054] Pyrolytic carbon deposition: The thickness of the carbon deposit prepared in Example 1 is 0.45 mm and the weight is 20 g / m 2 The carbon paper precursor is subjected to vapor deposition at a vapor deposition temperature of 900°C for 3 hours, the carbon source gas is methane, and the carbon source gas flow rate is 600 mL / min to obtain deposited carbon paper;
[0055] Loading resin: The thermosetting resin is loaded on the deposited carbon paper by screen printing. The thermosetting resin is a furan resin with a solid content of 60%. The viscosity of the furan resin (25°C) is 200mPa·s. The loading amount of the furan resin on 100g of the deposited carbon paper is 30g. The paper is subjected to low-temperature pre-curing, hot pressing and carbonization treatment in sequence. The low-temperature pre-curing temperature is 80°C and the low-temperature pre-curing time is 1.5h; the hot pressing temperature is 130°C, the hot pressing pressure is 8MPa, and the hot pressing time is 40min; the carbonization temperature is 900°C and the carbonization time is 4h to obtain a densified carbon paper;
[0056] Impregnation treatment: prepare a thermosetting resin ethanol solution, the thermosetting resin uses furan resin with a solid content of 60%, impregnate the densified carbon paper in the thermosetting resin ethanol solution, and then perform low-temperature pre-curing, hot pressing and carbonization treatments in sequence;
[0057] Repeated impregnation: repeat the impregnation treatment step once, the concentration of the thermosetting resin ethanol solution used for the first time is 10wt%, the impregnation time is 1min, the concentration of the thermosetting resin ethanol solution used for the second time is 6wt%, the impregnation time is 5min, the low-temperature pre-curing temperature for the two times in the impregnation treatment and repeated impregnation steps is 80°C, and the low-temperature pre-curing time is 60min; the hot pressing temperature is 130°C, the hot pressing pressure is 8MPa, and the hot pressing time is 10min; the carbonization temperature is 900°C, and the carbonization time is 2h to obtain carbonized carbon paper;
[0058] Graphitization treatment: The carbonized carbon paper is subjected to high-temperature graphitization treatment, the graphitization temperature is 2200° C., and the graphitization time is 3 h to obtain carbon paper for fuel cells.
[0059] Example 2
[0060] A method for preparing carbon paper for a fuel cell comprises the following steps:
[0061] Pyrolytic carbon deposition: The thickness of the carbon deposit prepared in Example 1 is 0.45 mm and the weight is 40 g / m 2 The carbon paper precursor is subjected to vapor deposition at a vapor deposition temperature of 1100°C for 1.5 hours, the carbon source gas is propane, and the carbon source gas flow rate is 800 mL / min to obtain deposited carbon paper;
[0062] Loading resin: The thermosetting resin is loaded on the deposited carbon paper by screen printing. The thermosetting resin is a phenolic resin with a solid content of 60%. The viscosity of the phenolic resin (25°C) is 200mPa·s. The loading amount of the phenolic resin on 100g of the deposited carbon paper is 30g. The paper is subjected to low-temperature pre-curing, hot pressing and carbonization treatment in sequence. The low-temperature pre-curing temperature is 90°C, and the low-temperature pre-curing time is 1.2h; the hot pressing temperature is 150°C, the hot pressing pressure is 5MPa, and the hot pressing time is 50min; the carbonization temperature is 1100°C, and the carbonization time is 3.5h to obtain a densified carbon paper;
[0063] Impregnation treatment: prepare a thermosetting resin ethanol solution, the thermosetting resin uses a phenolic resin with a solid content of 60%, impregnate the densified carbon paper in the thermosetting resin ethanol solution, and then perform low-temperature pre-curing, hot pressing and carbonization treatments in sequence;
[0064] Repeated impregnation: repeat the impregnation treatment step once, the concentration of the thermosetting resin ethanol solution used for the first time is 10wt%, the impregnation time is 1min, the concentration of the thermosetting resin ethanol solution used for the second time is 6wt%, the impregnation time is 5min, the low-temperature pre-curing temperature for the two times in the impregnation treatment and repeated impregnation steps is 90°C, and the low-temperature pre-curing time is 50min; the hot pressing temperature is 150°C, the hot pressing pressure is 5MPa, and the hot pressing time is 20min; the carbonization temperature is 1100°C, and the carbonization time is 1.5h to obtain carbonized carbon paper;
[0065] Graphitization treatment: The carbonized carbon paper is subjected to high-temperature graphitization treatment, the graphitization temperature is 2500° C., and the graphitization time is 2 h to obtain carbon paper for fuel cells.
[0066] Example 3
[0067] A method for preparing carbon paper for a fuel cell comprises the following steps:
[0068] Pyrolytic carbon deposition: The thickness of the carbon deposit prepared in Example 1 is 0.45 mm and the weight is 40 g / m 2 The carbon paper precursor is subjected to vapor deposition at a vapor deposition temperature of 1300°C for 0.7 h, the carbon source gas is natural gas, and the carbon source gas flow rate is 1000 mL / min to obtain deposited carbon paper;
[0069] Loading resin: The thermosetting resin is loaded on the deposited carbon paper by screen printing, the thermosetting resin is furfural resin with a solid content of 60%, the viscosity of furfural resin (25°C) is 300mPa·s, the loading amount of phenolic resin on 100g of deposited carbon paper is 30g, and low-temperature pre-curing, hot pressing and carbonization treatment are sequentially performed, the low-temperature pre-curing temperature is 100°C, the low-temperature pre-curing time is 1h; the hot pressing temperature is 180°C, the hot pressing pressure is 1MPa, and the hot pressing time is 60min; the carbonization temperature is 1400°C, and the carbonization time is 3h, to obtain a densified carbon paper;
[0070] Impregnation treatment: prepare a thermosetting resin ethanol solution, the thermosetting resin adopts furfural resin with a solid content of 60%, impregnate the densified carbon paper in the thermosetting resin ethanol solution, and then perform low-temperature pre-curing, hot pressing and carbonization treatment in sequence;
[0071] Repeated impregnation: repeat the impregnation treatment step once, the concentration of the thermosetting resin ethanol solution used for the first time is 10wt%, the impregnation time is 1min, the concentration of the thermosetting resin ethanol solution used for the second time is 6wt%, the impregnation time is 5min, the low-temperature pre-curing temperature for the two times in the impregnation treatment and repeated impregnation steps is 100°C, and the low-temperature pre-curing time is 40min; the hot pressing temperature is 180°C, the hot pressing pressure is 1MPa, and the hot pressing time is 30min; the carbonization temperature is 1400°C, and the carbonization time is 1h, to obtain carbonized carbon paper;
[0072] Graphitization treatment: The carbonized carbon paper is subjected to high-temperature graphitization treatment, the graphitization temperature is 2700° C., and the graphitization time is 1 h to obtain carbon paper for fuel cells.
[0073] Example 4
[0074] The difference from Example 2 is that the immersion treatment step is repeated twice, the concentration of the thermosetting resin ethanol solution used in the third time is 3 wt %, and the immersion time is 9 minutes.
[0075] Example 5
[0076] The difference from Example 4 is that the immersion treatment step is repeated 4 times, the concentration of the thermosetting resin ethanol solution used in the fourth time is 0.5 wt %, and the immersion time is 20 min.
[0077] Example 6
[0078] The difference from Example 4 is that the concentration of the thermosetting resin ethanol solution used for the first time is 8.5wt%, and the immersion time is 2.5min, the concentration of the thermosetting resin ethanol solution used for the second time is 5wt%, and the immersion time is 6.5min, and the concentration of the thermosetting resin ethanol solution used for the third time is 2wt%, and the immersion time is 10min.
[0079] Example 7
[0080] The difference from Example 4 is that the concentration of the thermosetting resin ethanol solution used in the first time is 7wt%, and the immersion time is 4min, the concentration of the thermosetting resin ethanol solution used in the second time is 4wt%, and the immersion time is 5min, and the concentration of the thermosetting resin ethanol solution used in the third time is 1wt%, and the immersion time is 12min.
[0081] Example 8
[0082] The difference from Example 4 is that the concentration of the thermosetting resin ethanol solution used in the first, second and third times is 15 wt %.
[0083] Example 9
[0084] The difference from Example 4 is that the concentration of the thermosetting resin ethanol solution used in the first, second and third times is 5 wt %.
[0085] Example 10
[0086] The difference from Example 6 is that the impregnation step adopts vacuum impregnation, the densified carbon paper is impregnated in the thermosetting resin ethanol solution, and the vacuum is evacuated to -0.1 MPa.
[0087] Comparative Example
[0088] Comparative Example 1
[0089] A method for preparing carbon paper for a fuel cell comprises the following steps:
[0090] Loaded resin: The thickness of the resin prepared in Preparation Example 1 is 0.45 mm and the weight is 40 g / m 2 A carbon paper precursor is prepared, and a thermosetting resin is loaded on the carbon paper precursor by an impregnation method, wherein the thermosetting resin is a phenolic resin with a solid content of 60%, the viscosity of the phenolic resin (25°C) is 200mPa·s, and the loading amount of the phenolic resin on 100g of the carbon paper precursor is 30g. The carbon paper precursor is subjected to low-temperature pre-curing, hot pressing and carbonization treatments in sequence, wherein the low-temperature pre-curing temperature is 90°C, the low-temperature pre-curing time is 1.2h; the hot pressing temperature is 150°C, the hot pressing pressure is 5MPa, and the hot pressing time is 50min; the carbonization temperature is 1100°C, and the carbonization time is 3.5h, to obtain a densified carbon paper;
[0091] Graphitization treatment: The densified carbon paper is subjected to high-temperature graphitization treatment, the graphitization temperature is 2500° C., and the graphitization time is 2 h to obtain carbon paper for fuel cells.
[0092] Comparative Example 2
[0093] A method for preparing carbon paper for a fuel cell comprises the following steps:
[0094] Pyrolytic carbon deposition: The thickness of the carbon deposit prepared in Example 1 is 0.45 mm and the weight is 40 g / m 2 The carbon paper precursor is subjected to vapor deposition at a vapor deposition temperature of 1100°C for 1.5 hours, the carbon source gas is propane, and the carbon source gas flow rate is 800 mL / min to obtain deposited carbon paper;
[0095] Loading resin: The thermosetting resin is loaded on the deposited carbon paper by screen printing. The thermosetting resin is a phenolic resin with a solid content of 60%. The viscosity of the phenolic resin (25°C) is 200mPa·s. The loading amount of the phenolic resin on 100g of the deposited carbon paper is 30g. The paper is subjected to low-temperature pre-curing, hot pressing and carbonization treatment in sequence. The low-temperature pre-curing temperature is 90°C, and the low-temperature pre-curing time is 1.2h; the hot pressing temperature is 150°C, the hot pressing pressure is 5MPa, and the hot pressing time is 50min; the carbonization temperature is 1100°C, and the carbonization time is 3.5h to obtain a densified carbon paper;
[0096] Graphitization treatment: The densified carbon paper is subjected to high-temperature graphitization treatment at a graphitization temperature of 2500° C. for a graphitization time of 2 h to obtain carbon paper for fuel cells.
[0097] Comparative Example 3
[0098] A method for preparing carbon paper for a fuel cell comprises the following steps:
[0099] Loaded resin: The thickness of the resin prepared in Example 1 is 0.45 mm and the weight is 40 g / m 2 A carbon paper precursor is prepared, and a thermosetting resin is loaded on the carbon paper precursor by an impregnation method, wherein the thermosetting resin is a phenolic resin with a solid content of 60%, the viscosity of the phenolic resin (25°C) is 200mPa·s, and the loading amount of the phenolic resin on 100g of the carbon paper precursor is 30g. The carbon paper precursor is subjected to low-temperature pre-curing, hot pressing and carbonization treatments in sequence, wherein the low-temperature pre-curing temperature is 90°C, the low-temperature pre-curing time is 1.2h; the hot pressing temperature is 150°C, the hot pressing pressure is 5MPa, and the hot pressing time is 50min; the carbonization temperature is 1100°C, and the carbonization time is 3.5h, to obtain a densified carbon paper;
[0100] Impregnation treatment: prepare a thermosetting resin ethanol solution, the thermosetting resin adopts a phenolic resin with a solid content of 60%, impregnate the densified carbon paper in the thermosetting resin ethanol solution, and then perform low-temperature pre-curing, hot pressing and carbonization treatments in sequence;
[0101] Repeated impregnation: the impregnation treatment step is repeated once, the concentration of the thermosetting resin ethanol solution used twice is 10wt%, the impregnation time is 1min, the low-temperature pre-curing temperature twice in the impregnation treatment and repeated impregnation steps is 90°C, and the low-temperature pre-curing time is 50min; the hot pressing temperature is 150°C, the hot pressing pressure is 5MPa, and the hot pressing time is 20min; the carbonization temperature is 1100°C, and the carbonization time is 1.5h to obtain carbonized carbon paper;
[0102] Graphitization treatment: The carbonized carbon paper is subjected to high-temperature graphitization treatment, the graphitization temperature is 2500° C., and the graphitization time is 2 h to obtain carbon paper for fuel cells.
[0103] Performance testing
[0104] The performance requirements of carbon paper are as follows:
[0105] Resistivity 0.04-0.3Ω·mm, tensile strength ≥20MPa, porosity ≥70%.
[0106] Detection Methods
[0107] (1) The carbon papers prepared in Examples 1-10 and Comparative Examples 1-3 were subjected to performance tests. The test method adopted the method specified in GB / T20042.7-2014 Proton Exchange Membrane Fuel Cell Part 7: Carbon Paper Property Test Method. The test items included: resistivity (in plane direction), tensile strength, and porosity.
[0108] Table 1 Test results
[0109]
[0110]
[0111] Combining Examples 1-3 and Comparative Examples 1-3 and Table 1, it can be seen that Comparative Example 1 does not perform vapor deposition, and only impregnates with high-concentration resin once when loading the resin. The resistivity of the carbon paper is high and the tensile strength is low, indicating that the carbon paper obtained by the conventional resin impregnation method has poor conductivity and mechanical properties; Comparative Example 2 first performs vapor deposition on the carbon paper precursor on the basis of Comparative Example 1, and the resistivity of the obtained carbon paper decreases and the tensile strength increases, indicating that vapor deposition of the carbon paper precursor first can improve the conductivity and mechanical properties of the carbon paper; Comparative Example 3 adds two low-concentration resin impregnation steps on the basis of Comparative Example 1, and the resistivity of the obtained carbon paper decreases and the tensile strength increases, indicating that multiple impregnations with low-concentration resin can improve the conductivity and mechanical properties of the carbon paper; Examples 1-3 simultaneously use vapor deposition and multiple impregnations with low-concentration resin, and the resistivity of the obtained carbon paper decreases and the tensile strength increases, indicating that the present application uses vapor deposition and multiple impregnations with low-concentration resin to improve the conductivity and mechanical properties of the carbon paper, among which Example 2 has a better effect.
[0112] Combining Examples 4-10 and Table 1, it can be seen that Examples 4 and 5 increase the number of impregnation treatment steps in turn. The resistivity of the carbon paper obtained in Example 4 decreases, and the tensile strength increases. Compared with Example 4, the resistivity of the carbon paper in Example 5 decreases slightly, and the tensile strength increases slightly. Taking all factors into consideration, Example 4 has a better effect. Examples 6-7 change the resin concentration and the impregnation time. Taking all factors into consideration, Example 6 has a better effect. Examples 8-9 use larger and smaller concentrations of resin for impregnation, respectively, and the resistivity of the carbon paper increases, while the tensile strength decreases, indicating that the resin concentration preferably adopts the range of this application. Example 10 uses vacuum impregnation, and the resistivity of the carbon paper decreases, while the tensile strength increases, indicating that vacuum impregnation is beneficial for the resin to penetrate into the pores of the carbon paper, enhance the three-dimensional network structure, and further improve the conductive properties and mechanical properties of the carbon paper.
[0113] Since carbon paper needs to meet the ventilation and drainage requirements of the fuel cell, the porosity of the carbon paper must be greater than or equal to 70%. The porosity of the carbon paper prepared in Examples 1-10 is greater than 70%, indicating that the present application can improve the conductive properties and mechanical properties of carbon paper while ensuring that the porosity of the carbon paper meets the requirements.
[0114] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for preparing carbon paper for fuel cells, Features: The following steps are involved: Pyrolytic carbon deposition: The carbon paper precursor is vapor deposited to obtain deposited carbon paper; Loading resin: Thermosetting resin is loaded on the deposited carbon paper, and then subjected to low-temperature pre-curing, hot pressing and carbonization treatments to obtain densified carbon paper; Impregnation treatment: prepare a thermosetting resin ethanol solution, impregnate the densified carbon paper in the thermosetting resin ethanol solution, and sequentially undergo low-temperature pre-curing, hot pressing and carbonization treatments; Repeated impregnation: Repeat the impregnation treatment step more than once, and the concentration of the thermosetting resin ethanol solution used for each impregnation is gradually reduced to obtain carbonized carbon paper; Graphitization treatment: subjecting the carbonized carbon paper to high-temperature graphitization treatment to obtain carbon paper for fuel cells; In the repeated impregnation step, the impregnation treatment step is repeated twice, the concentration of the thermosetting resin ethanol solution used in the first step is 7-10wt%, the impregnation time is 1-4min, the concentration of the thermosetting resin ethanol solution used in the second step is 4-6wt%, the impregnation time is 5-8min, and the concentration of the thermosetting resin ethanol solution used in the third step is 1-3wt%, and the impregnation time is 9-12min; The thermosetting resin is selected from any one of furan resin, phenolic resin and furfural resin.
2. The method for preparing carbon paper for fuel cells according to claim 1, Features: In the pyrolytic carbon deposition step, the vapor deposition temperature is 900-1300° C., the time is 0.7-3 h, and the carbon source gas flow rate is 600-1000 mL / min.
3. The method for preparing carbon paper for fuel cells according to claim 1, Features: In the resin loading step, the low-temperature pre-curing temperature is 80-100°C, and the low-temperature pre-curing time is 1-1.5h; the hot pressing temperature is 130-180°C, the hot pressing pressure is 1-8MPa, and the hot pressing time is 40-60min; the carbonization temperature is 900-1400°C, and the carbonization time is 3-4h.
4. The method for preparing carbon paper for fuel cells according to claim 3, Features: In the impregnation treatment step, the low-temperature pre-curing temperature is 80-100°C, and the low-temperature pre-curing time is 40-60min; the hot pressing temperature is 130-180°C, the hot pressing pressure is 1-8MPa, and the hot pressing time is 10-30min; the carbonization temperature is 900-1400°C, and the carbonization time is 1-2h.
5. The method for preparing carbon paper for fuel cells according to claim 4, Features: In the impregnation step, the densified carbon paper is impregnated in a thermosetting resin ethanol solution and evacuated to below -0.1 MPa.
6. The method for preparing carbon paper for fuel cells according to claim 1, Features: The thickness of the carbon paper precursor is 0.4-0.5 mm, and the weight is 20-60 g / m 2 .
7. A carbon paper for a fuel cell, Features: The carbon paper is prepared by the method for preparing carbon paper for fuel cells according to any one of claims 1 to 6.
8. A gas diffusion layer, Features: The invention comprises a microporous layer and a base layer which are stacked in sequence, wherein the material of the base layer comprises the carbon paper for fuel cells as claimed in claim 7.
9. A fuel cell, Features: Comprising the gas diffusion layer as claimed in claim 8.
Citation Information
Patent Citations
PEM fuel cell, gas diffusion layer porous carbon paper and preparation method of gas diffusion layer porous carbon paper
CN113066996A
Carbon paper and preparation method thereof, gas diffusion layer and fuel cell
CN115262265A