A zinc-containing polyacid-based MOF material and its preparation method and application
By developing zinc-containing polyacid-based MOF materials, carbon dioxide and epoxy in the prior art are solved by using a three-dimensional network structure combining zinc ions, 2,5-bis(4-pyridyl)pyridine ligand and phosphotungstic anion combination. The problem of low activity and insufficient stability of the cyclic carbonate catalyst for compound preparation has achieved high efficiency and low toxicity.
Patent Information
- Application Number
- CN202311736753.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-12-18
AI Technical Summary
In the prior art, the catalyst for preparing cyclic carbonate with carbon dioxide and epoxy compounds has problems such as low catalytic activity, high toxicity, harsh reaction conditions, high energy consumption, and difficult catalyst recycling, which limits its large-scale production.
Develop a zinc-containing polyacid-based MOF material with a three-dimensional network structure formed by a combination of zinc ions, 2,5-bis(4-pyridyl)pyridine ligand, oxalic acid ligand and phosphotungstic anion, through one step of water Prepared by thermal synthesis method, used to catalyze the preparation of phenyl epoxy carbonate with carbon dioxide and phenyl ethylene oxide.
The material has high catalytic activity, good thermal stability, low toxicity, easy operation and good reproducibility, effectively overcomes the problems of traditional homogeneous catalytic efficiency, high operating cost, and difficult separation and recycling, and demonstrates excellent catalysis Performance and good stability.
Smart Images

Figure CN117924721B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new materials, and specifically relates to a zinc-containing polyacid-based MOF material and a preparation method and application thereof. Background Art
[0002] As human production and life activities intensify, the dependence on fossil energy is increasing, and the sharp increase in carbon dioxide emissions has made people aware of the severity of the problem due to global warming and the resulting environmental problems. Since the adoption of the Kyoto Protocol in 1997, carbon dioxide has become the most concerned greenhouse gas (GHG) due to the large changes in the spatial distribution of water vapor. How to achieve carbon dioxide emission reduction is gradually becoming a key issue in the development of today's society.
[0003] Carbon dioxide molecules have high chemical thermodynamic stability and are extremely difficult to be activated and utilized. In industrial production, high temperature, high pressure or catalysts are usually used to overcome their inertness. However, chemical fixation of carbon dioxide can be achieved by activating relatively active reaction substrates to combine with them, thereby reducing the demand for energy. Among them, the reaction of epoxy compounds with carbon dioxide to prepare cyclic carbonates is considered to be an important way to prepare high value-added chemical products by artificial fixation of carbon dioxide with high atom economy, green, safe and efficient. Cyclic carbonates can be used as monomers of polyester materials to prepare polymer materials through polymerization reactions, and can also be used to prepare medical sutures, drug sustained-release materials, etc. At present, homogeneous catalytic systems such as metal complexes and organic small molecule catalysis have been reported, but there are still many problems such as low catalytic activity, high toxicity, harsh reaction conditions, high energy consumption, and difficulty in recycling catalysts, which limit their large-scale production. Therefore, the development of heterogeneous catalysts to catalyze carbon dioxide and epoxy compounds to prepare cyclic carbonates is receiving increasing attention.
[0004] As a type of catalytic material with excellent performance, polyacid-based MOFs materials play an important role in the field of heterogeneous catalysis. Chemists combine polyacids with MOFs through independent assembly and crystal engineering methods to construct polyacid-based MOFs materials. Studies in recent years have found that MOFs materials can be used as catalysts to initiate the preparation of cyclic carbonates from carbon dioxide and epoxides, but the catalytic activity and stability of MOFs need to be further improved. The combination of polyacids and MOFs can not only improve the stability of the catalytic material, but also improve its catalytic activity. Therefore, it is urgent to develop applications of polyacid-based MOFs materials with high stability and activity to catalyze the preparation of cyclic carbonates from carbon dioxide and epoxides. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a zinc-containing polyacid-based MOF material.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a zinc-containing polyacid-based MOF material, characterized in that it includes a three-dimensional network structure composed of zinc ions, 2,5-bis(4-pyridyl)pyridine ligands, oxalic acid ligands and phosphotungstate anions, and its chemical formula is [Zn 9 (TPYD) 9 (OX) 6 (P 2 W 18 O 62 )(H 2 O) 6 ].
[0009] Among them, TPYD is a 2,5-bis(4-pyridyl)pyridine ligand, OX is an oxalic acid ligand, [P 2 W 18 O 62 ] is the phosphotungstate anion.
[0010] As a preferred embodiment of the preparation method of the present invention, the molecular formula of the zinc-containing polyacid-based MOF material is C 147 H 111 N 27 O 92 P 2 W 18 Zn 9 ; molecular weight is 7687.15; crystal system is trigonal; space group is P6 / m; unit cell parameters are α=90, β=90, γ=120, Z=1.
[0011] As a preferred embodiment of the preparation method of the present invention, phosphotungstic acid, metal zinc salt, oxalic acid and 2,5-bis(4-pyridyl)pyridine are dissolved in deionized water, and the pH value is adjusted to obtain a reaction solution;
[0012] The reaction solution after adjusting the pH value is added into a polytetrafluoroethylene reactor, and after the reaction, the temperature is cooled to room temperature to obtain colorless block crystals, that is, a zinc-containing polyacid-based MOF material.
[0013] As a preferred embodiment of the preparation method of the present invention, the molar ratio of the phosphotungstic acid to 2,5-bis(4-pyridyl)pyridine is 1:2 to 1:4.
[0014] As a preferred embodiment of the preparation method of the present invention, the molar ratio of phosphotungstic acid to metal zinc salt is 0.1:0.2 to 0.1:1.0, and the molar ratio of phosphotungstic acid to oxalic acid is 1:11 to 1:16.
[0015] As a preferred embodiment of the preparation method of the present invention, the metal zinc salt is zinc nitrate, zinc chloride or zinc acetate.
[0016] As a preferred embodiment of the preparation method of the present invention, wherein: the pH value is adjusted to obtain a reaction solution, wherein 1 mol / L NaOH solution and 1 mol / L HNO 3 The solution was adjusted to a pH of 3.0-4.0.
[0017] As a preferred embodiment of the preparation method of the present invention, the reaction solution after adjusting the pH value is added into a polytetrafluoroethylene reaction kettle, wherein the reaction temperature is 160° C. and the reaction time is 3 days.
[0018] Another object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a zinc-containing polyacid-based MOF material by catalyzing carbon dioxide and phenylethylene oxide to prepare phenyl epoxy carbonate using the product obtained by the method.
[0019] As a preferred embodiment of the method for preparing phenyl epoxy carbonate by catalyzing carbon dioxide and phenyl ethylene oxide of the present invention, the molar ratio of the zinc-containing polyacid-based MOF material to phenyl ethylene oxide is 1:500 to 1:4500, the reaction temperature is 25 to 120° C., and the reaction time is 10 to 60 hours.
[0020] Beneficial effects of the present invention:
[0021] (1) The zinc-containing polyacid-based MOF material disclosed in the present invention has high catalytic activity, good thermal stability and low toxicity, and its synthesis method is easy to operate and has good reproducibility.
[0022] (2) The present invention uses a one-step hydrothermal synthesis method to successfully synthesize a zinc-containing polyacid-based MOF material using phosphotungstic acid, zinc nitrate, oxalic acid and 2,5-bis(4-pyridyl)pyridine. The material has excellent catalytic performance and good stability in CO 2The potential application value is shown in the transformation.
[0023] (3) The present invention effectively overcomes the problems of low efficiency, high operating cost, and difficulty in separation and recycling of traditional homogeneous catalysis. Through independent assembly and crystal engineering methods, polyacids are combined with MOFs to construct zinc-containing polyacid-based MOF materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0025] Figure 1 This is a schematic diagram of the coordination of the zinc-containing polyacid-based MOF material prepared in Example 1. Figure 1 Among them, 1 is Zn, 2 is N, 3 is O, 4 is C, 5 is W, and 6 is P;
[0026] Figure 2 A schematic diagram of the three-dimensional structure of the zinc-containing polyacid-based MOF material prepared in Example 1;
[0027] Figure 3 This is a thermogravimetric curve of the zinc-containing polyacid-based MOF material prepared in Example 1;
[0028] Figure 4 This is an infrared graph of the zinc-containing polyacid-based MOF material prepared in Example 1;
[0029] Figure 5 This is the solid UV-visible absorption spectrum of the zinc-containing polyacid-based MOF material prepared in Example 1;
[0030] Figure 6 The PXRD pattern of the zinc-containing polyacid-based MOF material prepared in Example 1;
[0031] Figure 7 This is a schematic diagram of the conversion rate and reaction time of preparing phenyl epoxy carbonate by using the zinc-containing polyacid-based MOF material prepared in Example 1 to catalyze carbon dioxide and phenyl ethylene oxide;
[0032] Figure 8 These are the PXRD patterns of the zinc-containing polyacid-based MOF material prepared in Example 1 before and after catalysis. DETAILED DESCRIPTION
[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0034] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0035] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0036] Example 1
[0037] This embodiment 1 provides a method for preparing a zinc-containing polyacid-based MOF material:
[0038] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2 O (0.02 mmol), zinc nitrate (0.17 mmol), oxalic acid (0.28 mmol) and 2,5-bis(4-pyridyl)pyridine (0.05 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3 The solution adjusted the pH value of the reaction solution to 3.2, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 63% (based on 2,5-bis(4-pyridyl)pyridine).
[0039] The X-ray single crystal diffraction structure analysis data of a zinc-containing polyacid-based MOF material prepared in Example 1 is shown in Table 1. The instrument used is the ApexII single crystal diffractometer of Bruker Corporation;
[0040] Table 1
[0041]
[0042]
[0043] As shown in Table 1, X-ray single crystal diffraction analysis shows that the molecular formula of a zinc-containing polyacid-based MOF material prepared in Example 1 is C 147 H 111 N 27 O 92 P 2W 18 Zn 9 The zinc-containing polyacid-based MOF material prepared in Example 1 has a three-dimensional network structure. Figure 1 This is a coordination diagram of a zinc-containing polyacid-based MOF material prepared in Example 1, Figure 1 Where 1 is Zn, 2 is N, 3 is O, 4 is C, 5 is W, and 6 is P; the zinc ions of a zinc-containing polyacid-based MOF material prepared in Example 1 are connected with oxalic acid and TPYD organic ligands to form a three-dimensional cationic pore structure, and each pore is loaded with an anionic polyacid [P 2 W 18 O 62 ] 6- Forming a zinc-containing three-dimensional polyacid-based MOFs structure (such as Figure 2 shown), Figure 2 A schematic diagram of the three-dimensional structure of a zinc-containing polyacid-based MOF material prepared in Example 1; Figure 3 This is a thermogravimetric curve of a zinc-containing polyacid-based MOF material prepared in Example 1. Figure 3 It can be seen that a zinc-containing polyacid-based MOF material has good thermal stability below 400 °C; Figure 4 This is the infrared curve of the zinc-containing polyacid-based MOF material prepared in Example 1. Figure 4 It can be seen that the infrared spectrum of a zinc-containing polyacid-based MOF material is 1091, 960, 907 and 791 cm -1 The characteristic peaks near [P 2 W 18 O 62 ] 6- ν(P–O), ν(W=Ot), ν in anions as (W–Ob–W) stretching vibration, 1673–1234 cm -1 The characteristic peaks in the range are attributed to the vibration peaks of TPYD and OX ligands, 3391 cm -1 The characteristic peaks are attributed to the vibration peaks of water; Figure 5 This is a solid UV-visible absorption spectrum of a zinc-containing polyacid-based MOF material prepared in Example 1. Figure 5 It can be seen that a zinc-containing polyacid-based MOF material shows a UV-visible absorption peak with the center of the UV absorption peak at 300nm, which is attributed to the heteropolyacid [P 2 W 18 O 62 ] 6- The ultraviolet absorption peak of Figure 6 The PXRD pattern of a zinc-containing polyacid-based MOF material prepared in Example 1 is shown in FIG. Figure 6It can be seen that by comparing the X-ray powder diffraction simulation spectrum and the X-ray powder diffraction experimental spectrum of a zinc-containing polyacid-based MOF material prepared in Example 1 (1 is the simulated peak position, 2 is the experimental peak position), the experimental peak position and the simulated peak position of the compound in the PXRD spectrum are basically consistent, indicating that the purity of the zinc-containing polyacid-based MOF material prepared in Example 1 is good.
[0044] In summary, this embodiment uses a one-step hydrothermal synthesis method to successfully synthesize a zinc-containing polyacid-based MOF material using phosphotungstic acid, zinc nitrate, oxalic acid and 2,5-bis(4-pyridyl)pyridine.
[0045] The main steps of applying the zinc-containing polyacid-based MOF material prepared in Example 1 to catalyze carbon dioxide and phenylethylene oxide to prepare phenyl epoxy carbonate are:
[0046] In Example 1 of the present invention, a zinc-containing polyacid-based MOF material in an amount of 20 μmoL, tetrabutylammonium bromide co-catalyst (0.3 mmol), and phenyl oxirane (20 mmol) were added sequentially into a 10 mL reaction tube, and carbon dioxide gas (0.1 MPa) was introduced to supply the reaction system. The reaction temperature was 100°C and the reaction time was 24 hours to obtain phenyl epoxy carbonate with a yield of 99% (yield = (amount of phenyl epoxy carbonate substance after reaction / amount of phenyl oxirane substance before reaction) × 100%).
[0047] Figure 7 This is a schematic diagram of the conversion rate and reaction time of preparing phenyl epoxy carbonate by catalyzing carbon dioxide and phenyl ethylene oxide using the zinc-containing polyacid-based MOF material prepared in Example 1. Figure 7 It can be seen that by adding a large excess of phenyl oxirane (90 mmol) at one time while keeping the catalyst dosage and other reaction conditions unchanged, the substrate was completely converted into phenyl epoxy carbonate after 60 hours with a yield of 99%. The experimental results prove that zinc-containing polyacid-based MOF materials have good recycling capabilities.
[0048] Figure 8 The PXRD patterns of the zinc-containing polyacid-based MOF material prepared in Example 1 before and after catalysis are shown in Table 1. Figure 6 It can be seen that by comparing the X-ray powder diffraction experimental spectrum of the zinc-containing polyacid-based MOF material prepared in Example 1 with the X-ray powder diffraction spectrum after catalysis (1 is the experimental peak position, 2 is the peak position after catalysis), the experimental peak position of the compound in the PXRD spectrum and the peak position after catalysis are basically consistent, indicating that the zinc-containing polyacid-based MOF material prepared in Example 1 has good stability.
[0049] In summary, Example 1 uses a one-step hydrothermal synthesis method to successfully synthesize a zinc-containing polyacid-based MOF material using phosphotungstic acid, zinc nitrate, oxalic acid and 2,5-bis(4-pyridyl)pyridine. The material has excellent catalytic performance and good stability in CO 2 The potential application value is shown in the transformation.
[0050] Example 2
[0051] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2 O (0.02 mmol), zinc chloride (0.17 mmol), oxalic acid (0.28 mmol) and 2,5-bis(4-pyridyl)pyridine (0.05 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3 The solution adjusted the pH value of the reaction solution to 3.2, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 51% (based on 2,5-bis(4-pyridyl)pyridine).
[0052] Example 3
[0053] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2 O (0.02 mmol), zinc acetate (0.17 mmol), oxalic acid (0.28 mmol) and 2,5-bis(4-pyridyl)pyridine (0.05 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3 The solution adjusted the pH value of the reaction solution to 3.2, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 37% (based on 2,5-bis(4-pyridyl)pyridine).
[0054] Example 4
[0055] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2O (0.02 mmol), zinc nitrate (0.20 mmol), oxalic acid (0.32 mmol) and 2,5-bis(4-pyridyl)pyridine (0.08 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3 The solution adjusted the pH value of the reaction solution to 3.2, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 55% (based on 2,5-bis(4-pyridyl)pyridine).
[0056] Example 5
[0057] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2 O (0.02 mmol), zinc nitrate (0.04 mmol), oxalic acid (0.22 mmol) and 2,5-bis(4-pyridyl)pyridine (0.04 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3 The solution adjusted the pH value of the reaction solution to 3.2, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 39% (based on 2,5-bis(4-pyridyl)pyridine).
[0058] Example 6
[0059] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2 O (0.02 mmol), zinc nitrate (0.10 mmol), oxalic acid (0.24 mmol) and 2,5-bis(4-pyridyl)pyridine (0.05 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3 The solution adjusted the pH value of the reaction solution to 3.2, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 43% (based on 2,5-bis(4-pyridyl)pyridine).
[0060] Example 7
[0061] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2 O (0.02 mmol), zinc nitrate (0.18 mmol), oxalic acid (0.30 mmol) and 2,5-bis(4-pyridyl)pyridine (0.06 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3 The solution adjusted the pH value of the reaction solution to 3.2, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 49% (based on 2,5-bis(4-pyridyl)pyridine).
[0062] Example 8
[0063] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2 O (0.02 mmol), zinc nitrate (0.17 mmol), oxalic acid (0.28 mmol) and 2,5-bis(4-pyridyl)pyridine (0.05 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3 The solution adjusted the pH value of the reaction solution to 3.0, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 53% (based on 2,5-bis(4-pyridyl)pyridine).
[0064] Example 9
[0065] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2 O (0.02 mmol), zinc nitrate (0.17 mmol), oxalic acid (0.28 mmol) and 2,5-bis(4-pyridyl)pyridine (0.05 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3The solution adjusted the pH value of the reaction solution to 3.5, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 46% (based on 2,5-bis(4-pyridyl)pyridine).
[0066] Example 10
[0067] Phosphotungstic acid K 6 [P 2 W 18 O 62 ]·14H 2 O (0.02 mmol), zinc nitrate (0.17 mmol), oxalic acid (0.28 mmol) and 2,5-bis(4-pyridyl)pyridine (0.05 mmol) were dissolved in deionized water (8 mL) to obtain a reaction solution (pH < 3); 1 mol / L NaOH solution was used first and then 1 mol / L HNO 3 The solution adjusted the pH value of the reaction solution to 4.0, and the reaction solution was added into a polytetrafluoroethylene reactor, reacted at 160°C for 3 days, and cooled to room temperature to obtain colorless block crystals, i.e., a zinc-containing polyacid-based MOF material, with a yield of 38% (based on 2,5-bis(4-pyridyl)pyridine).
[0068] Embodiment 11
[0069] The zinc-containing polyacid-based MOF material prepared in Example 1 catalyzes carbon dioxide and phenylethylene oxide to prepare phenyl epoxy carbonate.
[0070] A zinc-containing polyacid-based MOF material in an amount of 20 μmoL, tetrabutylammonium bromide co-catalyst (0.3 mmol), and phenyl oxirane (10 mmol) were added sequentially into a 10 mL reaction tube, and carbon dioxide gas (0.1 MPa) was introduced to supply the reaction system. The reaction temperature was 100°C and the reaction time was 10 hours to obtain phenyl epoxy carbonate with a yield of 93% (yield = (amount of phenyl epoxy carbonate substance after reaction / amount of phenyl oxirane substance before reaction) × 100%).
[0071] Example 12
[0072] A zinc-containing polyacid-based MOF material provided in Example 1 was used in an amount of 20 μmoL, tetrabutylammonium bromide co-catalyst (0.3 mmol), and phenyl oxirane (85 mmol) were added sequentially into a 10 mL reaction tube, and carbon dioxide gas (0.1 MPa) was introduced to supply the reaction system. The reaction temperature was 100°C and the reaction time was 55 hours to obtain phenyl epoxy carbonate with a yield of 99% (yield = (amount of phenyl epoxy carbonate substance after reaction / amount of phenyl oxirane substance before reaction) × 100%).
[0073] Example 13
[0074] A zinc-containing polyacid-based MOF material provided in Example 1 was used in an amount of 20 μmoL, tetrabutylammonium bromide co-catalyst (0.3 mmol), and phenyl oxirane (20 mmol) were added sequentially into a 10 mL reaction tube, and carbon dioxide gas (0.1 MPa) was introduced to supply the reaction system. The reaction temperature was 25°C and the reaction time was 24 hours to obtain phenyl epoxy carbonate with a yield of 13% (yield = (amount of phenyl epoxy carbonate substance after reaction / amount of phenyl oxirane substance before reaction) × 100%).
[0075] Embodiment 14
[0076] A zinc-containing polyacid-based MOF material provided in Example 1 was used in an amount of 20 μmoL, tetrabutylammonium bromide co-catalyst (0.3 mmol), and phenyl oxirane (90 mmol) were added sequentially into a 10 mL reaction tube, and carbon dioxide gas (0.1 MPa) was introduced to supply the reaction system. The reaction temperature was 100°C and the reaction time was 60 hours to obtain phenyl epoxy carbonate with a yield of 99% (yield = (amount of phenyl epoxy carbonate substance after reaction / amount of phenyl oxirane substance before reaction) × 100%).
[0077] Embodiment 15
[0078] A zinc-containing polyacid-based MOF material provided in Example 1 was used in an amount of 20 μmoL, tetrabutylammonium bromide co-catalyst (0.3 mmol), and phenyl oxirane (20 mmol) were added into a 10 mL reaction tube in sequence, and carbon dioxide gas (0.1 MPa) was introduced to supply the reaction system. The reaction temperature was 80°C and the reaction time was 24 hours to obtain phenyl epoxy carbonate with a yield of 88% (yield = (amount of phenyl epoxy carbonate substance after reaction / amount of phenyl oxirane substance before reaction) × 100%).
[0079] Example 16
[0080] A zinc-containing polyacid-based MOF material provided in Example 1 was used in an amount of 20 μmoL, tetrabutylammonium bromide co-catalyst (0.3 mmol), and phenyl oxirane (20 mmol) were added into a 10 mL reaction tube in sequence, and carbon dioxide gas (0.1 MPa) was introduced to supply the reaction system. The reaction temperature was 120°C and the reaction time was 24 hours to obtain phenyl epoxy carbonate with a yield of 99% (yield = (amount of phenyl epoxy carbonate substance after reaction / amount of phenyl oxirane substance before reaction) × 100%).
[0081] Comparative Example 1
[0082] Phosphotungstic acid K6 [P 2 W 18 O 62 ]·14H 2 O is replaced by other phosphotungstic acids (such as K 3 PW 12 O 40 Or Na 3 PW 12 O 40 ), and the other aspects were the same as in Example 1, and all that was obtained was amorphous powder, and no crystalline sample suitable for X-ray single crystal analysis was obtained.
[0083] Comparative Example 2
[0084] The metal zinc salt was replaced with other metal salts (such as silver nitrate, nickel chloride, copper acetate or cadmium nitrate) except zinc nitrate, zinc chloride and zinc acetate, and the other conditions were the same as in Example 1. All the obtained materials were amorphous powders, and no crystalline samples suitable for X-ray single crystal analysis were obtained.
[0085] Comparative Example 3
[0086] When oxalic acid was replaced with other acidic substances (such as malonic acid, succinic acid or tartaric acid), and the other conditions were the same as those in Example 1, amorphous powders were obtained, and no crystalline samples suitable for X-ray single crystal analysis were obtained.
[0087] Comparative Example 4
[0088] When 2,5-di(pyridin-4-yl)pyridine was replaced with other nitrogen heterocyclic ligands (such as imidazole, benzimidazole, pyridine or pyrrole), and the other conditions were the same as in Example 1, amorphous powders were obtained, and no crystalline samples suitable for X-ray single crystal analysis were obtained.
[0089] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. An application of a zinc-containing polyacid-based MOF material, characterized in that: Application of the zinc-containing polyacid-based MOF material to catalyze carbon dioxide and phenylethylene oxide to prepare phenyl epoxy carbonate at a reaction temperature; The zinc-containing polyacid-based MOF material includes a three-dimensional network structure composed of zinc ions, 2,5-bis(4-pyridyl)pyridine ligands, oxalic acid ligands and phosphotungstate anions, and its chemical formula is [Zn9(TPYD)9(OX)6(P2W 18 O 62 )(H2O)6];TPYD is 2,5-bis(4-pyridyl)pyridine ligand, OX is oxalic acid ligand, [P2W 18 O 62 ] is the phosphotungstate anion; The molecular formula of the zinc-containing polyacid-based MOF material is C 147 H 111 N 27 O 92 P2W 18 Zn9; molecular weight is 7687.15; crystal system is trigonal; space group is P6 / m; unit cell parameters are a=18.785(5)Å, b=18.785(5)Å, c=15.527(5)Å, V =4745.047Å3, α=90, β=90, γ=120, Z =1.
2. The use according to claim 1, characterized in that: The molar ratio of the zinc-containing polyacid-based MOF material to phenylethylene oxide is 1:500 to 1:4500, wherein the reaction temperature is 25 to 120° C. and the reaction time is 10 to 60 hours.
3. The use according to claim 1, characterized in that: The preparation method of the zinc-containing polyacid-based MOF material comprises: Dissolve phosphotungstic acid, metal zinc salt, oxalic acid and 2,5-bis(4-pyridyl)pyridine in deionized water, and adjust the pH value to obtain a reaction solution; The reaction solution after adjusting the pH value is added into a polytetrafluoroethylene reactor, and after the reaction, the temperature is cooled to room temperature to obtain colorless block crystals, that is, a zinc-containing polyacid-based MOF material.
4. The use according to claim 3, characterized in that: The molar ratio of the phosphotungstic acid to 2,5-bis(4-pyridyl)pyridine is 1:2-1:
4.
5. The use according to claim 4, characterized in that: The molar ratio of the phosphotungstic acid to the metal zinc salt is 0.1:0.2-0.1:1.0, and the molar ratio of the phosphotungstic acid to the oxalic acid is 1:11-1:
16.
6. The use according to claim 5, characterized in that: The metal zinc salt is zinc nitrate, zinc chloride or zinc acetate.
7. The use according to claim 1, characterized in that: The pH value is adjusted to obtain a reaction solution, wherein the pH value is adjusted to 3.0-4.0 using 1 mol / L NaOH solution and 1 mol / L HNO3 solution.
8. The use according to claim 7, characterized in that: The reaction solution after adjusting the pH value is added into a polytetrafluoroethylene reactor, wherein the reaction temperature is 160° C. and the reaction time is 3 days.
Citation Information
Patent Citations
Resist base material, resist composition, and method for forming resist pattern
CN107533290A
Synthesis of copper compound and application of copper compound in photodegradation of organic dye methyl violet
CN113214492A
Cobalt-containing phosphotungstic acid-based metal organic framework material as well as preparation method and application thereof
CN117964909A