Colored cellulose films, their preparation methods and applications

By constructing dome-structured colored cellulose films on the surface of cellulose-based functional materials, the problems of insufficient structural stability and color brightness in existing technologies have been solved, enabling large-area preparation and environmentally friendly colored film applications, which are applicable to multiple functional material fields.

CN117924805BActive Publication Date: 2026-11-17BEIHANG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211266227.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-17
Publication Date
2026-11-17
Estimated Expiration
2042-10-17

AI Technical Summary

Technical Problem

Existing colored cellulose membrane materials suffer from poor structural stability, low color brightness, and complex preparation processes that make large-scale production difficult.

Method used

By constructing a colored cellulose film with a dome structure on the surface of a cellulose-based functional material, structural color is generated using the dome structure. The cellulose-based functional material is then coated onto a large-area pit structure template using techniques such as etching and photolithography to prepare a uniform and bright structural color film.

Benefits of technology

It achieves color stability and brightness of colored thin films, avoids the use of chemical pigments, and is biocompatible and biodegradable. It is suitable for large-area preparation and can be applied in food, packaging, sensing/detection devices, catalysis and biomedical materials and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117924805B_ABST
    Figure CN117924805B_ABST
Patent Text Reader

Abstract

This invention relates to the field of structural color materials, and discloses a colored cellulose film, its preparation method, and its applications. The colored cellulose film contains cellulose-based functional materials and has a dome structure on its surface, which generates structural color. The colored cellulose film of this invention has a uniform and bright structural color, its color is stable and never fades, and it enables large-area preparation of colored films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of structural color materials, specifically to a colored cellulose film, its preparation method, and its application. Background Technology

[0002] Cellulose and its derivatives are among the earliest commercially available polymer materials, widely used in papermaking, textiles, plastics, food, energy, pharmaceuticals, and coatings. By bonding functional groups to the main chain through reactions such as esterification, etherification, oxidation, and graft copolymerization, cellulose can be endowed with various functions, including mechanical, electrical, optical, magnetic, sensing, detection, adsorption, separation and purification, catalysis, and antibacterial properties. These functions have broad application value in packaging, mechanical / optical / electrical / magnetic devices, sensing / detection devices, adsorption and separation materials, catalysis, biomedicine, and information storage. While cellulose and its derivatives are mostly colorless and transparent, they can be made to exhibit a wide range of colors by adding pigments or dyes. However, the synthesis of pigments or dyes causes significant wastewater pollution and poses problems such as heavy metal residues and photobleaching fading.

[0003] Structural colors are produced by the modulation of light (such as diffraction, interference, and scattering) by micro- or nano-scale microstructures (thin films, gratings, photonic crystals, etc.). They possess characteristics such as metallic luster, high saturation, controllable color, rich hues, resistance to light bleaching, and environmental friendliness, making them a good alternative to chemical pigments. Constructing structural color materials using environmentally friendly and biodegradable cellulose and its derivatives can endow cellulose materials with vibrant colors and maintain or enhance the functions of cellulose, making them applicable to various functional materials fields. Patents (CN107353704 A; CN111040225 B) and literature (Carbohydrate Polymers, 2017, 174, 39-47; Journal of Materials Chemistry C, 2016, 4, 9687-9696; Advanced Materials, 2017, 29, 1701469) report methods for preparing brightly colored cellulose membrane materials using the self-assembly of cellulose nanocrystals. Patent CN104198401A discloses a method for preparing colored alcohol-responsive cellulose-based photonic crystals using a three-dimensional photonic crystal as a template. Several methods for preparing functional cellulose-based photonic crystal detection materials using cellulose derivatives via a three-dimensional photonic crystal template method have also been reported in the literature (Nanoscale, 2018, 10, 2090-2098; Analytical Chemistry, 2016, 88, 5424-5429; Analyst, 2019, 144, 1892-1897; Sensors and Actuators B, 2015, 220, 222–226). Currently, the colored cellulose membrane materials reported in patents and literature suffer from poor structural stability and low color brightness. Furthermore, the construction methods are subject to problems such as complex process parameters, applicability to only one or a few materials, and difficulty in large-scale preparation. Summary of the Invention

[0004] To address the problems existing in the preparation of colored cellulose-based functional materials using existing technologies, this invention provides a colored cellulose film, its preparation method, and its application. This colored cellulose film has a uniform and bright structural color, its color is stable and never fades, and it enables the large-area preparation of colored films.

[0005] To achieve the above objectives, the present invention provides a colored cellulose film, wherein the colored cellulose film contains a cellulose-based functional material and has a dome structure on its surface, the dome structure being capable of producing structural color.

[0006] Preferably, the cellulose-based functional material is one or more of the following: pure cellulose functional material, cellulose composite material, cellulose ester, cellulose ether, cellulose graft copolymer, cellulose crosslink copolymer, and surface-modified cellulose functional material.

[0007] Preferably, the pure cellulose functional material refers to a functional material prepared using unmodified or regenerated cellulose material, wherein the cellulose material used is selected from one or more of cellulose nanocrystals, bacterial cellulose, and regenerated cellulose materials.

[0008] Preferably, the cellulose composite material refers to a functional material prepared by combining cellulose with other materials, and is selected from one or more of cellulose optoelectronic or piezoelectric composite materials, cellulose-based detection and adsorption materials, and cellulose-based biomedical composite materials.

[0009] Preferably, the cellulose ester is obtained by reacting the hydroxyl groups on the cellulose chain with an acid, acyl chloride, acyl halide, or acid anhydride.

[0010] Preferably, the cellulose ester is selected from one or more of cellulose acetate, cellulose butyrate, cellulose acetate butyrate, cellulose nitrate, cellulose benzoate, cellulose sulfate, and cellulose carbamate.

[0011] Preferably, the cellulose ether is obtained by reacting the hydroxyl groups on cellulose with alkyl halides or other etherifying agents under alkaline conditions.

[0012] Preferably, the cellulose ether is selected from one or more of methylcellulose, ethylcellulose, hydroxypropylcellulose, hydroxypropylmethylcellulose, carboxymethylcellulose, and cellulose triphenylmethyl ether.

[0013] Preferably, the cellulose graft copolymer is obtained by reacting hydroxyl groups on the cellulose chain with an initiator, and then polymerizing and grafting small molecule monomers onto the cellulose polymer chain through one or more of the following reactions: free radical polymerization, ring-opening polymerization, atom transfer radical polymerization, and reversible addition-fragmentation chain transfer polymerization.

[0014] Preferably, the cellulose graft copolymer is selected from one or more of the following: hydroxyethyl cellulose grafted poly(N-isopropylacrylamide), cellulose grafted poly(N-isopropylacrylamide)-poly(4-vinylpyridine) block copolymer, cellulose grafted poly(N,N-dimethylaminoethyl methacrylate), cellulose grafted poly(N-isopropylacrylamide), cellulose grafted polylactic acid, and cellulose grafted calixarene graft copolymer.

[0015] Preferably, the cellulose crosslinked copolymer is prepared by the interaction of cellulose with bifunctional molecules, resulting in a crosslinking reaction between cellulose polymers.

[0016] Preferably, the cellulose crosslinked copolymer is selected from one or more of formaldehyde crosslinked cellulose polymers, dialdehyde crosslinked cellulose polymers, dicarboxylic acid crosslinked cellulose polymers, and divinyl sulfone crosslinked polymers.

[0017] Preferably, the surface-modified cellulose functional material is a functional material obtained by physically or chemically treating the surface of a cellulose material;

[0018] Preferably, the surface-modified cellulose functional material is selected from one or more of superhydrophobic cellulose materials, antibacterial quaternary ammonium salt cellulose materials, TEMPO oxidized transparent cellulose materials, and silanized cellulose materials.

[0019] Preferably, there is one or more dome structures; more preferably, there are multiple dome structures; even more preferably, the dome structures are distributed in an array.

[0020] Preferably, when the dome structure array is distributed, the spacing between adjacent dome structures is 0-500 μm, and more preferably 0-10 μm.

[0021] Preferably, the diameter of the dome structure is 500nm-100μm, and more preferably 5-30μm.

[0022] Preferably, the curvature angle of the dome structure is 40-150°, more preferably 60-120°, and even more preferably 70-100°.

[0023] Preferably, the reflectance spectral peak position of the colored cellulose film material is in the range of 200-15000nm, more preferably 310-1050nm, and even more preferably 390-780nm.

[0024] According to a second aspect of the present invention, a method for preparing a colored cellulose film according to the first aspect of the present invention is provided, wherein the method includes the following steps:

[0025] 1) The steps for preparing a template with a pitted structure;

[0026] 2) The step of filling the pitted side of the template obtained in step 1) with cellulose-based functional material and then curing it;

[0027] 3) The step of separating the template from the cured cellulose-based functional material.

[0028] Preferably, the method for preparing the template with the pit structure is selected from one or more of the following: etching, breathing patterning, photolithography, nanoimprinting, electron beam etching, focused ion beam etching, two-photon polymerization, or microsphere assembly.

[0029] According to a third aspect of the present invention, the application of the colored cellulose film of the first aspect of the present invention in smart response detectors, colorful packaging, anti-counterfeiting patterns, and flexible displays is provided.

[0030] This invention obtains a functional colored cellulose film by constructing a dome structure. This film possesses a uniform, bright structural color that is stable and never fades. It requires no added pigments or dyes, reducing harm to the environment and humans. Using cellulose as a raw material to construct structural color materials results in good biocompatibility and biodegradability. Furthermore, various functions can be imparted to the material through physical composites or chemical bonds, making it applicable to food, packaging, sensing / detection devices, catalysis, and biomedical materials, among other fields, demonstrating significant application value. Moreover, the preparation method of this invention is simple to operate, with easily controllable conditions, and avoids complex and cumbersome procedures, making it highly practical.

[0031] Furthermore, cellulose and its derivative materials have good solution or melt processing properties, and can be used to construct large-area functional colored cellulose films with dome structures by methods such as roll-to-roll or direct coating on large-area pit structure templates. Attached Figure Description

[0032] Figure 1 In the diagram, 'a' represents a schematic diagram illustrating the mechanism by which the dome structure of the colored cellulose film of this invention interacts with light to generate structural colors. Figure 1 In the diagram, b is a schematic representation of the diameter of the dome structure marked in a.

[0033] Figure 2 This is a SEM image of the colored cellulose acetate film with a dome structure prepared in Example 1.

[0034] Figure 3 This is an optical image of the colored cellulose acetate film with a dome structure prepared in Example 1.

[0035] Figure 4 This is the scattering spectrum of the colored cellulose acetate film with a dome structure prepared in Example 1. Detailed Implementation

[0036] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0037] According to a first aspect of the present invention, a colored cellulose film is provided, wherein the colored cellulose film contains a cellulose-based functional material and has a dome structure on its surface, the dome structure being capable of producing structural color.

[0038] According to the present invention, preferably, the colored cellulose film is composed of a cellulose-based functional material and has a dome structure on its surface, the dome structure being capable of producing structural color.

[0039] According to the present invention, preferably, the cellulose-based functional material is one or more of pure cellulose functional materials, cellulose composite materials, cellulose esters, cellulose ethers, cellulose graft copolymers, cellulose crosslinking copolymers, and surface-modified cellulose functional materials.

[0040] In this invention, the pure cellulose functional material refers to a functional material prepared using unmodified or regenerated cellulose materials, including one or more of materials such as cellulose nanocrystals, bacterial cellulose, and regenerated cellulose.

[0041] In this invention, the cellulose composite material refers to a functional material prepared by combining cellulose with other materials, including one or more of the following materials: cellulose optoelectronic or piezoelectric composite materials, cellulose-based detection and adsorption materials, and cellulose-based biomedical composite materials.

[0042] In this invention, the cellulose ester can be obtained by reacting the hydroxyl groups on the cellulose chain with an acid, acyl chloride, acyl halide, or acid anhydride. The cellulose ester includes one or more of cellulose esters and their derivatives, such as cellulose acetate, cellulose butyrate, cellulose acetate butyrate, cellulose nitrate, cellulose benzoate, cellulose sulfate, and cellulose carbamate.

[0043] In this invention, the cellulose ether can be generated by reacting hydroxyl groups on cellulose with alkyl halides or other etherifying agents under alkaline conditions. The synthesis method can be selected from one or more of the Williamson etherification reaction, alkaline-catalyzed epoxide addition reaction, and alkaline-catalyzed addition reaction. Preferably, the cellulose ether includes one or more of cellulose ethers and their derivatives, such as methylcellulose, ethylcellulose, hydroxypropylcellulose, hydroxypropylmethylcellulose, carboxymethylcellulose, and cellulose triphenylmethyl ether.

[0044] In this invention, the cellulose graft copolymer is obtained by reacting hydroxyl groups on the cellulose chain with an initiator, and polymerizing and grafting small molecule monomers onto the cellulose polymer chain through one or more of the following reactions: free radical polymerization, ring-opening polymerization, atom transfer radical polymerization, and reversible addition-fragmentation chain transfer polymerization. Preferably, the cellulose graft copolymer includes one or more of the following: hydroxyethyl cellulose grafted poly(N-isopropylacrylamide), cellulose grafted poly(N-isopropylacrylamide)-poly(4-vinylpyridine) block copolymer, cellulose grafted poly(N,N-dimethylaminoethyl methacrylate), cellulose grafted poly(N-isopropylacrylamide), cellulose grafted polylactic acid, and cellulose grafted calixarene.

[0045] In this invention, the cellulose crosslinked copolymer is prepared by the interaction of cellulose with bifunctional molecules, resulting in a crosslinking reaction between cellulose polymers. Preferably, the cellulose crosslinked copolymer is selected from one or more of formaldehyde crosslinked cellulose polymers, dialdehyde crosslinked cellulose polymers, dicarboxylic acid crosslinked cellulose polymers, and divinyl sulfone crosslinked polymers.

[0046] In this invention, the surface-modified cellulose functional material refers to a functional material obtained by physically or chemically treating the surface of a cellulose material, including one or more of the following: superhydrophobic cellulose material, antibacterial quaternary ammonium salt cellulose material, TEMPO oxidized transparent cellulose material, and silanized cellulose material.

[0047] According to the present invention, there is one or more dome structures; preferably, there are multiple dome structures; more preferably, the dome structures are distributed in an array.

[0048] In this invention, the spacing between adjacent dome structures can be 0-500 μm, preferably 0-10 μm. By keeping the spacing within the above range, the structural color brightness of the film is higher.

[0049] According to the present invention, the diameter of the dome structure is 500 nm-100 μm; preferably, the diameter of the dome structure is 5-30 μm. In this invention, the "diameter of the dome structure" refers to the diameter of the sphere to which the dome structure belongs. Figure 1 In b, it is represented as D.

[0050] According to the present invention, the curvature angle of the dome structure can be 40-150°; preferably, the curvature angle of the dome structure is 60-120°; more preferably, the curvature angle of the dome structure is 70-100°. By keeping the curvature angle of the recess structure within the above range, the dome structure can exhibit a structural color.

[0051] According to the present invention, the thickness of the colored cellulose film can be 5-500 μm, preferably 10-150 μm.

[0052] According to the present invention, the reflectance spectral peak position range of the colored cellulose film is 200-15000 nm; preferably, the reflectance spectral peak position range is 310-1050 nm; more preferably, the reflectance spectral peak position range is 390-780 nm. By making the reflectance spectral peak position range of the colored cellulose film within the above range, the film has a bright structural color.

[0053] According to a second aspect of the present invention, a method for preparing a colored cellulose film having a dome structure on its surface, as described in the first aspect of the present invention, is provided, the method comprising the following steps:

[0054] 1) The steps for preparing a template with a pitted structure;

[0055] 2) The step of filling the pitted side of the template obtained in step 1) with cellulose-based functional material and then curing it;

[0056] 3) The step of separating the template from the cured cellulose-based functional material.

[0057] Preferably, the method for preparing the template with the pit structure is selected from one or more of the following: etching, breathing patterning, photolithography, nanoimprinting, electron beam etching, focused ion beam etching, two-photon polymerization, or microsphere assembly.

[0058] In this invention, the etching method selectively removes the portion of the substrate layer not masked by the resist using chemical, physical, or a combination of chemical and physical methods, thereby obtaining a pattern on the substrate that is completely identical to that on the resist film. Etching techniques are mainly divided into dry etching and wet etching. Dry etching primarily utilizes reactive gases and plasma for etching; wet etching primarily utilizes chemical reagents to react chemically with the material being etched for etching.

[0059] In this invention, the breathing pattern method is a method that uses water droplets as templates to obtain a honeycomb-like ordered porous structure through the orderly arrangement of water droplets. First, a polymer is dissolved in a low-boiling-point organic solvent (e.g., chloroform, carbon disulfide) that is immiscible with water. Then, in a high-humidity environment created by a humid airflow, the polymer solution is dropped onto a substrate. The rapid evaporation of the solvent in the solution causes a decrease in the surface temperature, resulting in water vapor condensing into tiny spherical droplets on the polymer solution surface. Under the influence of surface convection and thermocapillary forces, the droplets self-assemble into an ordered arrangement within the polymer solution. Due to the surface tension of water, as the solvent evaporates, the polymer adsorbs and precipitates at the water / organic solvent interface, replicating and fixing the ordered arrangement of the water droplets while preventing their aggregation. Finally, after the solvent and water have completely evaporated, an ordered honeycomb structure is formed on the surface of the polymer film.

[0060] In this invention, the photolithography method refers to the technique of transferring a pattern on a photomask onto a substrate using a photoresist (also known as photoresist) under illumination. The main process is as follows: First, ultraviolet light passes through the photomask and irradiates the surface of the substrate coated with a photoresist film, causing a chemical reaction in the exposed areas of the photoresist. Then, a development technique is used to dissolve and remove the photoresist from the exposed or unexposed areas (the former is called positive photoresist, and the latter is called negative photoresist), allowing the pattern on the photomask to be copied onto the photoresist film. Finally, an etching technique is used to transfer the pattern onto the substrate.

[0061] In this invention, the nanoimprint method is a technique for transferring micro- and nanostructures from a template onto a material to be processed. It generally involves two steps: the first step is template fabrication, typically using electron beam etching or similar methods to create the desired structure on silicon or other substrates as a template; the second step is pattern transfer, where the template is pressed onto the surface of the material to be processed, and pressure is applied to transfer the pattern to the material surface.

[0062] In this invention, the electron beam etching method is carried out under computer control. According to the pattern required for processing, a focused electron beam is used to expose the resist on the substrate, creating regions with different solubility properties in the resist. Based on the solubility characteristics of different regions, a selective developer is used for development. The highly soluble resist is removed, while the poorly soluble or insoluble parts are retained, thereby obtaining the desired resist pattern.

[0063] In this invention, the focused ion beam etching method focuses an ion beam to the submicron or even nanometer scale. By controlling the scanning motion of the ion beam through a deflection system and an acceleration system, it achieves the detection and analysis of micro / nano patterns and the maskless fabrication of micro / nano structures. The focused ion beam etching method typically consists of two steps: 1) preparing the sample to be processed, and then depositing a layer of Pt on the sample using a focused ion beam; 2) then precisely processing the area using the focused ion beam, or performing precise deposition or etching in conjunction with a specific gas injection system.

[0064] In this invention, the two-photon polymerization method utilizes the photopolymerization process initiated by the absorption of two photons by a material. By focusing a laser, the reaction area is confined to a very small area near the focal point. Furthermore, by moving the stage at the nanometer scale, the focal point is moved within the photosensitive material. Where the focused micro-nano spot passes, the photosensitive material undergoes denaturation and solidification, thus enabling the printing of 3D objects of arbitrary shapes.

[0065] In this invention, the microsphere assembly method refers to the self-assembly of colloidal microspheres into an ordered colloidal microsphere array under the influence of physicochemical processes. Specific methods for microsphere self-assembly include drop coating, dip-coating, spin coating, electrophoretic deposition, interfacial assembly, and unidirectional triboelectric assembly. Among them, drop coating involves the continuous self-assembly of randomly dispersed colloidal particles during liquid evaporation; dip coating involves the continuous assembly of colloidal microspheres on a vertical (or inclined), flat substrate when the liquid evaporation and lifting rates are precisely controlled; spin coating involves the rapid spontaneous assembly of colloidal microspheres when the solution is spread on a hydrophilic substrate at a high shear rate; electrophoretic deposition involves the confinement of colloidal microsphere suspension in a system with two electrode plates, and the charged colloidal microspheres spontaneously assemble on one side of the electrode plates when the plates are energized; interfacial assembly involves the dispersion of colloidal microsphere emulsions at the gas-liquid interface with a dispersant, and the spontaneous assembly of colloidal microspheres suspended at the gas-liquid interface as the liquid in the emulsion evaporates; and unidirectional frictional assembly involves the assembly of colloidal microspheres between two elastomers under unidirectional frictional force.

[0066] According to the present invention, the material used to prepare the template can be one or more of inorganic materials, organic materials, and composite materials.

[0067] Preferably, the inorganic material is one or more of glass, silicon, iron, copper, and stainless steel.

[0068] Preferably, the organic material is one or more of polystyrene, hydroxypropyl cellulose, polypropylene, block copolymers, polydimethylsiloxane, and polymethyl methacrylate.

[0069] Preferably, the composite material is one or more of PVA / SiO2 and polymethyl methacrylate / nano-SiO2 composite materials.

[0070] According to the present invention, the cellulose-based functional material is as described above.

[0071] According to a third aspect of the present invention, the application of the colored cellulose film of the first aspect of the present invention in smart response detectors, colorful packaging, anti-counterfeiting patterns, and flexible displays is provided.

[0072] The present invention will be described in detail below through embodiments, but the present invention is not limited to the following embodiments.

[0073] Example 1

[0074] 1) Prepare a 5cm×5cm glass slide and use chemical vapor grafting of hydrophobic molecules 1H,1H,2H,2H perfluorodecyltrimethoxysilane (PFOS) to prepare a hydrophobic substrate with an ink contact angle of 80°.

[0075] 2) The ink (prepared by dissolving polyethylene glycol in a mixed solvent of water and ethylene glycol with a mass ratio of polyethylene glycol, water and ethylene glycol of 5:38:57) was filtered using an oily filter with a pore size of 200 nm. The filtered transparent polymer ink was then dropped into an inkjet printer cartridge and a printhead with a droplet volume of 1 pL was installed to prepare a dome structure with a diameter of 16 μm and a curvature angle of 70°.

[0076] 3) After printing, the printed patterned substrate is subjected to ultraviolet irradiation (wavelength 380nm) for 30 minutes until it is completely cured.

[0077] 4) Place the glass with the dome structure obtained in 3) into a vacuum dryer, add 2 drops of fluorosilane, evacuate for 20 minutes, and then place it in an 80°C oven for 2 hours to perform hydrophobic treatment.

[0078] 5) Place the hydrophobic glass with a dome structure in a petri dish, pour in 15g of epoxy resin (purchased from EPOTEK, model OG142-87), remove air bubbles in a vacuum, and then heat in an 80℃ oven for 2 hours.

[0079] 6) Peel the epoxy resin off the glass template of the dome structure to obtain the epoxy resin pit template with the dome structure inverse structure.

[0080] 7) Dissolve an appropriate amount of cellulose acetate (CA) in N,N-dimethylformamide (DMF) and stir until completely dissolved to prepare a CA / DMF solution with a concentration of 10 wt%.

[0081] 8) The CA / DMF solution was filled into the epoxy resin pit template with the dome structure inverse structure. The solvent was evaporated at 60°C. After drying, the cellulose acetate film was peeled off from the template to obtain a colored cellulose acetate film with a dome structure and a thickness of 25 μm.

[0082] Images obtained through scanning electron microscopy (SEM) Figure 2 As can be seen, the film has a dome structure, and observation reveals that the film exhibits a bright structural color (see attached images). Figure 3 The scattering spectrum of the thin film was obtained using a macroscopic angle-resolved instrument. Figure 4 Therefore, a structural color thin film with a dome structure was obtained. Additionally, as... Figure 1 As shown in a, the mechanism by which the thin film generates structural color is that light traveling along different trajectories of total internal reflection at the concave optical interface produces color due to interference.

[0083] The cellulose acetate film prepared in this embodiment has a bright structural color and can be used for smart, colorful packaging.

[0084] Example 2

[0085] 1) Mix component A (prepolymer) and component B (curing agent) of Dow Corning Sylgard 184 at a mass ratio of 10:1 to prepare 20g of polydimethylsiloxane (PDMS). Then pour it into a square plastic petri dish, vacuum it, and put it in an 80℃ oven. After 2 hours, take it out to obtain PDMS sheets.

[0086] 2) Cut the PDMS into pieces measuring 5cm x 8cm. Use one piece of PDMS as the base and the other piece as the friction pad;

[0087] 3) Take 0.1g of dry powder of silica particles with a particle size of 10μm and place it on the PDMS substrate. By unidirectional friction of the PDMS rubbing pad on the PDMS substrate, the silica microspheres are tightly arranged on the PDMS substrate, forming a single layer of silica microsphere array.

[0088] 4) Place the PDMS substrate with monolayer silica microspheres obtained in 3) into a vacuum dryer, add 2-3 drops of fluorosilane, evacuate for 20 minutes, and then place it in an 80℃ oven for 2 hours to perform hydrophobic treatment.

[0089] 5) Place the hydrophobic PDMS substrate with monolayer silica microspheres in a petri dish, pour in 10g of polydimethylsiloxane prepared in the same way as in step 1), remove air bubbles in a vacuum, and heat in an 80℃ oven for 2 hours. Then, peel the PDMS sheet off the PDMS substrate with monolayer silica microspheres to obtain a PDMS template with a pitted structure.

[0090] 6) Dissolve hydroxypropyl cellulose in water and stir until completely dissolved to prepare a 5 wt% solution;

[0091] 7) The PDMS template with pitted structure in step 5) is subjected to plasma treatment (200W, 200s) to make it hydrophilic. Hydroxypropyl cellulose aqueous solution is filled into the PDMS template with pitted structure. The water is evaporated at 60℃. After drying, the hydroxypropyl cellulose film is peeled off from the PDMS template to obtain a colored hydroxypropyl cellulose film with dome structure and a thickness of 20um.

[0092] Scanning electron microscopy images revealed that the thin film possesses a dome structure. Observation showed that the film exhibited a bright structural color, and its scattering spectrum was obtained using a macroscopic angle-resolved microscope. Therefore, a structurally colored thin film with a dome structure was obtained. Furthermore, the mechanism by which this thin film generates structural color is that light traveling along different trajectories of total internal reflection at the concave optical interface produces color due to interference.

[0093] The hydroxypropyl cellulose film prepared in this embodiment contains hydrophilic hydroxyl groups, which can swell or shrink under different humidity levels, and can be used for environmental humidity detection.

[0094] Example 3

[0095] 1) Add chloroform to polystyrene and sonicate to dissolve it completely, to obtain a polystyrene solution (PS solution) with a content of 5% by weight;

[0096] 2) Add polystyrene solution to the glass slide inside the sealed container;

[0097] 3) A nitrogen gas stream containing water vapor at a fixed relative humidity of 65% is immediately blown over the PS solution, and the temperature throughout the process is 10℃;

[0098] 4) After the solvent and the water droplets that spontaneously condensed at the gas-liquid interface completely evaporated, a PS template with a pitted structure was obtained.

[0099] 5) Dissolve an appropriate amount of cellulose acetate butyrate (CAB) in N,N-dimethylformamide (DMF) and stir until completely dissolved to prepare a CAB / DMF solution with a concentration of 10 wt%.

[0100] 6) The CAB / DMF solution was filled into the PS template with a pitted structure, the solvent was evaporated at 60°C, and after drying, the CAB film was peeled off from the template to obtain a colored cellulose acetate butyrate film with a dome structure and a thickness of 20 μm.

[0101] Scanning electron microscopy images revealed that the thin film possesses a dome structure. Observation showed that the film exhibited a bright structural color, and its scattering spectrum was obtained using a macroscopic angle-resolved microscope. Therefore, a structurally colored thin film with a dome structure was obtained. Furthermore, the mechanism by which this thin film generates structural color is that light traveling along different trajectories of total internal reflection at the concave optical interface produces color due to interference.

[0102] The cellulose acetate butyrate film prepared by this invention has good flexibility and bright structural color, and can be used for intelligent colorful packaging.

[0103] Example 4

[0104] 1) Spin-coating positive photoresist S1813 onto a glass substrate at a speed of 2000 rpm and a temperature of 23°C.

[0105] 2) Heat the coated photoresist at 115℃ for 60s, cover the photoresist with a mask, and then expose it with an irradiation dose of 150mj / cm2. Change the mask and expose multiple times.

[0106] 3) The dome structure template was obtained by immersion and development using ZX-238 developer at a temperature of 21°C for 65 seconds, followed by rinsing with deionized water for 30 seconds and drying.

[0107] 4) Place the dome-shaped structure obtained in 3) into a vacuum dryer, add 2-3 drops of fluorosilane, evacuate for 20 minutes, and then place it in an 80°C oven for 2 hours to perform hydrophobic treatment.

[0108] 5) Place the hydrophobic dome structure template in a petri dish. Mix component A (prepolymer) and component B (curing agent) of Dow Corning Sylgard 184 at a mass ratio of 10:1 to prepare 20g of polydimethylsiloxane (PDMS). Pour the mixture into the petri dish, remove air bubbles in a vacuum, and then heat in an 80℃ oven for 2 hours.

[0109] 6) The PDMS was peeled off from the dome structure template, resulting in a PDMS template with a pitted structure;

[0110] 7) Dissolve an appropriate amount of cellulose acetate (CA) in N,N-dimethylformamide (DMF) and stir until completely dissolved to prepare a CA / DMF solution with a concentration of 8 wt%.

[0111] 8) The CA / DMF solution was filled into the PDMS template with a pitted structure, the solvent was evaporated at 60°C, and after drying, the cellulose acetate film was peeled off from the template to obtain a colored cellulose acetate film with a dome structure and a thickness of 20 μm.

[0112] Scanning electron microscopy images revealed that the thin film possesses a dome structure. Observation showed that the film exhibited a bright structural color, and its scattering spectrum was obtained using a macroscopic angle-resolved microscope. Therefore, a structurally colored thin film with a dome structure was obtained. Furthermore, the mechanism by which this thin film generates structural color is that light traveling along different trajectories of total internal reflection at the concave optical interface produces color due to interference.

[0113] The cellulose acetate film prepared in this embodiment has good flexibility and bright structural color, and can be used for intelligent colorful packaging.

[0114] Example 5

[0115] 1) Prepare a 2cm×2cm polished quartz glass slide, clean it with deionized water and then blow it dry with nitrogen;

[0116] 2) Use femtosecond lasers to perform single-point ablation on the quartz surface to form a micro-pit structure;

[0117] 3) Under ultrasonic assistance at 23℃, the sample with micro-pits was immersed in a 5% hydrofluoric acid solution for 30 minutes for etching treatment.

[0118] 4) The sample was then ultrasonically cleaned in acetone, ethanol and deionized water for 15 minutes respectively, and then dried in ambient air to obtain a quartz glass slide with a pitted structure.

[0119] 5) Take an appropriate amount of cellulose acetate rhodamine B derivative (CA-RhB, acetyl substitution degree of 2.0, rhodamine B substitution degree of 0.1) and dissolve it in N,N-dimethylformamide (DMF). Stir until it is completely dissolved to prepare a CA / DMF solution with a concentration of 5wt%.

[0120] 6) The CA-RhB / DMF solution was filled into a glass template with a dome-shaped inverse structure. The solvent was evaporated at 60°C. After drying, the CA-RhB film was peeled off from the template to obtain a fluorescent CA-RhB film with a dome structure and a thickness of 20 μm.

[0121] Scanning electron microscopy images revealed that the thin film possesses a dome structure. Observation showed that the film exhibited a bright structural color, and its scattering spectrum was obtained using a macroscopic angle-resolved microscope. Therefore, a structurally colored thin film with a dome structure was obtained. Furthermore, the mechanism by which this thin film generates structural color is that light traveling along different trajectories of total internal reflection at the concave optical interface produces color due to interference.

[0122] The fluorescent CA-RhB film prepared by this invention has good flexibility and exhibits red fluorescence under ultraviolet light, and can be used in the preparation of anti-counterfeiting products.

[0123] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A colored cellulose film, characterized in that, The colored cellulose film contains cellulose-based functional materials and has a dome structure on its surface, which can produce structural color; the cellulose-based functional materials are one or more of cellulose esters, cellulose ethers, and cellulose acetate rhodamine B derivatives. When the dome structure array is distributed, the spacing between adjacent dome structures is 0-10μm; the diameter of the dome structure is 5-30μm; and the curvature angle of the dome structure is 70-100°. The method for preparing the colored cellulose film includes the following steps: 1) The step of preparing a template with a pitted structure; 2) The step of filling the pitted side of the template obtained in step 1) with cellulose-based functional material and then curing it; 3) The step of separating the template from the cured cellulose-based functional material.

2. The colored cellulose film according to claim 1, wherein, The cellulose ester is obtained by reacting the hydroxyl groups on the cellulose chain with acids, acyl chlorides, acyl halides, or acid anhydrides.

3. The colored cellulose film according to claim 2, wherein, The cellulose ester is selected from one or more of cellulose acetate, cellulose butyrate, cellulose acetate butyrate, cellulose nitrate, cellulose benzoate, cellulose sulfate, cellulose carbamate and their derivatives.

4. The colored cellulose film according to claim 1, wherein, The cellulose ether is obtained by reacting the hydroxyl groups on cellulose with alkyl halides or other etherifying agents under alkaline conditions.

5. The colored cellulose film according to claim 4, wherein, The cellulose ether is selected from one or more of methylcellulose, ethylcellulose, hydroxypropylcellulose, hydroxypropylmethylcellulose, carboxymethylcellulose, cellulose triphenylmethyl ether and their derivatives.

6. The colored cellulose film according to claim 1, wherein, The dome structure is one or more.

7. The colored cellulose film according to claim 6, wherein, The dome structure consists of multiple structures.

8. The colored cellulose film according to claim 7, wherein, The dome structure array is distributed.

9. The colored cellulose film according to claim 1, wherein, The reflectance spectral peaks of the colored cellulose film material are located in the range of 200-15000 nm.

10. The colored cellulose film according to claim 9, wherein, The reflectance spectral peaks of the colored cellulose film material are located in the range of 310-1050 nm.

11. The colored cellulose film according to claim 10, wherein, The reflectance spectral peaks of the colored cellulose film material are located in the range of 390-780 nm.

12. A method for preparing a colored cellulose film according to any one of claims 1-11, characterized in that, The method includes the following steps: 1) The step of preparing a template with a pitted structure; 2) The step of filling the pitted side of the template obtained in step 1) with cellulose-based functional material and then curing it; 3) The step of separating the template from the cured cellulose-based functional material.

13. The method for preparing a colored cellulose film according to claim 12, wherein, The method for preparing the template with the pit structure is selected from one or more of the following: etching, breathing patterning, photolithography, nanoimprinting, two-photon polymerization, or microsphere assembly.

14. The method for preparing a colored cellulose film according to claim 13, wherein, The template with the pit structure is prepared by electron beam etching and / or focused ion beam etching.

15. The application of the colored cellulose film according to any one of claims 1-11 in smart response detectors, colorful packaging, anti-counterfeiting patterns, and flexible displays.

Citation Information

Patent Citations

  • Preparation of alcohol response cellulose photonic crystal film

    CN104198401A

  • Method for patterning cellulose photonic crystal

    CN107353704A

  • A rewritable anti-counterfeiting film based on photonic crystal structure color, its preparation method and application

    CN111040225B