A kind of ultra-high strength plasticity ultra-fine bainite finish-rolled threaded steel and preparation method thereof

Through austenitization treatment and multi-stage cooling, ultrafine bainite structure is formed, which solves the problem of poor strength and stability of traditional rebar, and achieves high-strength rebar of PSB1200 and above, reducing brittleness and hydrogen embrittlement sensitivity , improves the performance stability and corrosion resistance of rebar.

CN117925963BActive Publication Date: 2024-12-03NORTH CHINA UNIVERSITY OF SCIENCE AND TECHNOLOGY +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311718017.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2024-12-03
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

Traditional fine-rolled rebar has high strength but low plasticity, poor corrosion resistance, and microsegregation of alloy elements, resulting in high brittleness and hydrogen embrittlement sensitivity, making it difficult to achieve the performance stability of the PSB1200 level.

Method used

Through austenitization treatment, multi-stage cooling and stabilization tempering treatment, ultrafine bainite structure is formed, chemical composition and cooling speed are controlled, high-content bainite and nano-size second phase are generated, and austenite content is reduced. and carbon supersaturation to improve the strength and stability of rebar.

Benefits of technology

Ultra-high strength rebar of PSB1200 and above has been achieved, which significantly reduces brittleness and hydrogen embrittlement sensitivity, and improves the performance stability and corrosion resistance of rebar.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117925963B_ABST
    Figure CN117925963B_ABST
Patent Text Reader

Abstract

The invention discloses an ultra-high strength and plasticity ultra-fine bainite finish-rolled threaded steel and a preparation method thereof, belonging to the technical field of metallurgy, and comprising the following steps: austenitizing the threaded steel to be processed, and then cooling to a first preset temperature at a first cooling rate, the first cooling rate is 1°C / s-20°C / s, and the first preset temperature is 450°C-500°C; cooling to a second preset temperature at a second cooling rate, the second cooling rate is 0.1°C / s-5°C / s, the second preset temperature is Ms+100°C-Ms°C, cooling to a third preset temperature at a third cooling rate, the third cooling rate is 0.01°C / s-0.3°C / s, the third preset temperature is Ms+5°C-Ms-80°C, and Ms is the starting temperature of martensitic transformation; air cooling to room temperature, and tempering the threaded steel cooled to room temperature to obtain ultra-high strength threaded steel of PSB1200 level and above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to an ultra-high strength and plastic ultra-fine bainite finish-rolled threaded steel and a preparation method thereof. Background Art

[0002] The production process of traditional fine-rolled rebar is water quenching + high-temperature tempering and quenching to obtain rebars of different strength levels. This kind of rebar has high strength, but low plasticity. At the same time, the corrosion resistance of the rebar is also poor, and the surface of the rebar is also very easy to form a shrinkage rust layer. The strength level of bainite fine-rolled rebar currently produced by air cooling + tempering process can reach PSB1080, and it is difficult to reach PSB1200 level. Limited by the overall rebar production process, there is a large micro-segregation of alloy elements in the rebar currently produced, such as Mn, Cr, Mo and other elements. The segregation of these elements leads to the presence of more ultra-high strength but very brittle areas inside the high-strength rebar, which significantly increases the brittleness of the rebar. At the same time, these areas also have a higher sensitivity to hydrogen embrittlement. As a result, the performance stability of the rebar is poor, especially for PSB1200 level rebar, brittle fracture often occurs. Summary of the invention

[0003] In order to solve the above technical problems, the present invention proposes an ultra-high strength and plastic ultra-fine bainite finish-rolled threaded steel and a preparation method thereof. The method of the present invention can obtain ultra-high strength threaded steel of PSB1200 level and above.

[0004] To achieve the above object, the present invention provides a method for preparing ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel, comprising the following steps:

[0005] The rebar to be processed is subjected to austenitizing treatment, and then hot-rolled;

[0006] The hot-rolled rebar is cooled to a first preset temperature at a first cooling rate, wherein the first cooling rate is 1°C / s to 20°C / s, and the first preset temperature is 450°C to 500°C; the first cooling rate is relatively large, and rapid cooling is performed during the process to avoid the formation of ferrite.

[0007] Cooling to a second preset temperature at a second cooling rate, wherein the second cooling rate is 0.1°C / s to 5°C / s, and the second preset temperature is Ms°C to Ms+100°C, where Ms is the starting temperature of martensite transformation, and a small amount of austenite is controlled to transform into bainite during this process, and finally a bainite content of <35 vol.% is generated;

[0008] Cooling to a third preset temperature at a third cooling rate, wherein the third cooling rate is 0.01°C / s to 0.3°C / s, and the third preset temperature is Ms-80°C to Ms+5°C, where Ms is the starting temperature of martensite transformation, and most of the bainite structure is generated in this process, and the final bainite content is >50 vol.%, the remaining untransformed austenite content is <20 vol.%, and the average C content is >1.0 wt.%;

[0009] Air cooling to room temperature, that is, naturally cooling the rebar at the third preset temperature to room temperature in air;

[0010] The rebar cooled to room temperature is tempered. During the tempering process, stress is reduced, the supersaturated carbon content in the bainitic ferrite is reduced, and a nano-sized second phase is precipitated.

[0011] The present invention firstly performs hot working controlled forming on the threaded steel to be processed, so that the threaded steel forms fine austenite grains; the threaded steel with fine austenite grains is subjected to multi-stage controlled cooling treatment, and an ultrafine bainite structure is formed by controlling the cooling rate; the ultrafine bainite threaded steel is subjected to stabilization heat treatment (i.e., tempering treatment) to further stabilize the threaded steel structure, so as to obtain ultra-high strength and plasticity ultrafine bainite finish-rolled threaded steel.

[0012] Furthermore, the mass percentage of the chemical composition of the ultrafine bainite finish-rolled threaded steel is: C: 0.25% to 0.45%, Mn: 0.5% to 2.0%, Al+Si: 1.3% to 2.5%, Cr: <1.0%, Mo+Ni<0.5%, V+B: 0.06% to 0.18%, P<0.02%, S<0.02%, O<0.0015%, N<0.008%, H<0.0001%, and the balance is Fe and unavoidable impurities.

[0013] Furthermore, the mass percentages of the chemical components of the ultrafine bainite finish-rolled threaded steel are: C: 0.30% to 0.36%, Al+Si: 1.42% to 2.13%, Mn: 1.30% to 2.05%, Cr+Mo+Ni: 0.95% to 1.40%, V+B: 0.12% to 0.16%, O: 0.0010% to 0.0012%, H: 0.00007% to 0.00009%, N: 0.004% to 0.005%, P: 0.01% and S: 0.01%, and the balance is Fe and unavoidable impurities.

[0014] Furthermore, during the hot rolling treatment, the initial rolling temperature is 1100° C. to 1200° C., the final rolling temperature is controlled at 850° C. to 900° C., and the final rolling deformation is controlled at 30% to 50% to form fine austenite grains.

[0015] Furthermore, the initial rolling temperature is 1100° C. to 1150° C., the final rolling temperature is controlled at 850° C. to 880° C., and the final rolling deformation is controlled at 35% to 45%.

[0016] Furthermore, the first cooling rate is 5°C / s to 10°C / s, and the first preset temperature is 450°C to 480°C.

[0017] Furthermore, the second preset temperature is Ms+50°C to Ms°C, and in the process of cooling the threaded steel to the second preset temperature at a second cooling rate, continuous cooling and transformation are performed to generate bainite with a content of <35 vol.%.

[0018] Furthermore, the third preset temperature is Ms+5°C to Ms-30°C, and the bainite content generated by continuous cooling and transformation of the threaded steel to be processed to the third preset temperature at a third cooling rate is >50vol.%, the remaining untransformed austenite content is <20vol.%, and the average C content is >1.0wt.%.

[0019] Furthermore, during the tempering treatment, the tempering temperature is 300°C to 450°C, and the holding time is 15h to 60h.

[0020] An ultra-high strength and plastic ultra-fine bainite finish-rolled threaded steel prepared according to the above preparation method, wherein the residual austenite content is ≤15.1wt.%, the average C content is 1.21wt.%~1.52wt.%, the yield strength is 1200MPa~1350MPa, the tensile strength is 1480MPa~1645MPa, the uniform elongation is 5%~7%, and the total elongation is 12%~15.2%.

[0021] Compared with the prior art, the present invention has the following advantages and technical effects:

[0022] (1) In order to solve the serious segregation problem in traditional fine-rolled threaded steel, the present invention utilizes the C element strengthening and the precipitation dispersion strengthening of the nano-precipitated VC second phase, as well as the effect of trace V segregating at the grain boundary to improve the hardenability, thereby significantly reducing the content of Mn, Cr and other elements in the threaded steel that are traditionally used to improve the hardenability and strengthen the steel but are prone to segregation.

[0023] (2) In view of the poor performance stability of traditional ultra-high strength fine-rolled rebar, the present invention achieves precise control of the rebar structure through multi-stage controlled cooling. At the same time, through high-temperature stabilization tempering treatment, the content of supersaturated C in the bainitic ferrite is reduced, achieving precise control of the rebar microstructure and stable control of the mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0025] Figure 1 This is a scanning electron microscope micrograph of the ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel bar after treatment in Example 1;

[0026] Figure 2 This is the transmission electron microscope organization diagram of the ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel after treatment in Example 1;

[0027] Figure 3 This is the transmission electron microscope organization diagram of the ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel after treatment in Example 3. DETAILED DESCRIPTION

[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0029] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0031] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0032] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0033] The room temperature in the embodiments of the present invention, unless otherwise specified, is 25±2°C.

[0034] Unless otherwise specified, the percentages in the embodiments of the present invention are all by mass.

[0035] The performance test standard in the embodiment of the present invention is GB / T 20065-2016.

[0036] Example 1

[0037] The chemical composition mass percentage of the ultrafine bainite finish-rolled threaded steel to be processed is C: 0.36%, Al+Si: 1.58%, Mn: 1.40%, Cr: <1.0%, Mo+Ni<0.5%, V+B: 0.12%, O: 0.0012%, H: 0.00009%, N: 0.004%, P: 0.01%, S: 0.01%, and the balance is Fe and unavoidable impurities. The corresponding steel Ms temperature is 310℃. The rebar billet is heated and hot rolled into a rebar with a diameter of 40 mm. The final rolling temperature is controlled to be 890°C, the final deformation is 35%, and then cooled to 480°C at a first cooling rate of 10°C / s, and further cooled to 360°C at a second cooling rate of 2°C / s. In this process, 20wt.% of bainite is generated, and then cooled to 255°C at a third cooling rate of 0.2°C / s, and then naturally cooled to room temperature. Finally, it is tempered at 300°C for 50 hours. The scanning electron microscope structure diagram of the ultra-high strength and plastic ultra-fine bainite finish-rolled rebar treated by this method is shown in the figure Figure 1 As shown in the transmission electron microscope diagram Figure 2 As shown, it is an ultrafine bainite structure with a retained austenite content of 12.2wt.%, an average C content of 1.31wt.%, a yield strength of 1230MPa, a tensile strength of 1550MPa, a uniform elongation of 5.9%, and a total elongation (i.e., elongation after fracture) of 12%.

[0038] Example 2

[0039] The chemical composition mass percentage of the ultrafine bainite finish-rolled threaded steel to be processed is C: 0.33%, Al+Si: 1.42%, Mn: 1.30%, Cr: <1.0%, Mo+Ni<0.5%, V+B: 0.16%, O: 0.0011%, H: 0.00008%, N: 0.005%, P: 0.01%, S: 0.01%, and the balance is Fe and unavoidable impurities. The corresponding steel Ms temperature is 331°C. The rebar billet is heated and hot rolled into a rebar with a diameter of 30 mm. The final rolling temperature is controlled to be 890°C, the final deformation is 40%, and then cooled to 500°C at a first cooling rate of 18°C / s, and further cooled to 340°C at a second cooling rate of 1.2°C / s. In this process, 15wt.% of bainite is generated, and then cooled to 260°C at a third cooling rate of 0.1°C / s, and then naturally cooled to room temperature. Finally, it is tempered at 400°C for 50h. After being treated by this method, the residual austenite content in the ultra-high strength and plastic ultra-fine bainite finishing rebar structure is 10.5wt.%, the average C content is 1.21wt.%, the yield strength is 1250MPa, the tensile strength is 1590MPa, the uniform elongation is 6.2%, and the total elongation is 13.5%.

[0040] Example 3

[0041] The chemical composition mass percentage of the ultrafine bainite finish-rolled threaded steel to be processed is C: 0.30%, Al+Si: 1.72%, Mn: 1.70%, Cr: <1.0%, Mo+Ni<0.5%, V+B: 0.15%, O: 0.0011%, H: 0.00008%, N: 0.005%, P: 0.01%, S: 0.01%, and the balance is Fe and unavoidable impurities. The corresponding steel Ms temperature is 320℃. The rebar billet is heated and hot rolled into a rebar with a diameter of 20 mm. The final rolling temperature is controlled to be 870°C, the final deformation is 40%, and then cooled to 480°C at a first cooling rate of 6°C / s, and further cooled to 340°C at a second cooling rate of 3°C / s. In this process, 18wt.% bainite is generated, and then cooled to 270°C at a third cooling rate of 0.05°C / s, and then naturally cooled to room temperature. Finally, it is tempered at 430°C for 15h. After being treated by this method, the microstructure of the ultra-high strength and plastic ultra-fine bainite finished rolled rebar is as follows Figure 3 As shown, a large amount of nano-sized VC precipitates in the structure, the residual austenite content in the structure is 9.2wt.%, the average C content is 1.25wt.%, the yield strength of the steel is 1220MPa, the tensile strength is 1480MPa, the uniform elongation is 6.8%, and the total elongation is 15.2%.

[0042] Example 4

[0043] The chemical composition mass percentage of the ultrafine bainite finish-rolled threaded steel to be processed is C: 0.35%, Al+Si: 2.13%, Mn: 2.05%, Cr: <1.0%, Mo+Ni<0.5%, V+B: 0.11%, O: 0.0010%, H: 0.00007%, N: 0.005%, P: 0.01%, S: 0.01%, and the balance is Fe and unavoidable impurities. The corresponding steel Ms temperature is 275°C. The rebar billet is heated and hot rolled into a rebar with a diameter of 50 mm. The final rolling temperature is controlled to be 885°C, the final deformation is 35%, and then cooled to 455°C at a first cooling rate of 3°C / s, and further cooled to 320°C at a second cooling rate of 0.8°C / s. In this process, 23wt.% of bainite is generated, and then cooled to 220°C at a third cooling rate of 0.06°C / s, and then naturally cooled to room temperature. Finally, it is tempered at 360°C for 30h. After being treated by this method, the residual austenite content in the ultra-high strength and plastic ultra-fine bainite finishing rebar structure is 15.1wt.%, of which the average C content is 1.52wt.%, the yield strength of the steel is 1350MPa, the tensile strength is 1645MPa, the uniform elongation is 5.4%, and the total elongation is 12.8%.

[0044] It can be seen from the above embodiments that the ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel bars obtained by the method of the present invention can all reach the PSB1200 grade.

[0045] The above are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel, characterized in that: The following steps are involved: The rebar to be processed is subjected to austenitizing treatment, and then hot-rolled; Cooling the hot-rolled rebar to a first preset temperature at a first cooling rate, wherein the first cooling rate is 1°C / s to 20°C / s, and the first preset temperature is 450°C to 500°C; Cooling to a second preset temperature at a second cooling rate, wherein the second cooling rate is 0.1°C / s to 5°C / s, and the second preset temperature is Ms to Ms+100°C, where Ms is the starting temperature of martensitic transformation; Cooling to a third preset temperature at a third cooling rate, wherein the third cooling rate is 0.01°C / s to 0.3°C / s, and the third preset temperature is Ms-80°C to Ms+5°C, where Ms is the starting temperature of martensitic transformation; Air cool to room temperature; The rebar cooled to room temperature is tempered; The mass percentage of the chemical composition of the ultrafine bainite finish-rolled threaded steel is: C: 0.25% to 0.45%, Mn: 0.5% to 2.0%, Al+Si: 1.3% to 2.5%, Cr: <1.0%, Mo+Ni<0.5%, V+B: 0.06% to 0.18%, P<0.02%, S<0.02%, O<0.0015%, N<0.008%, H<0.0001%, and the balance is Fe and unavoidable impurities.

2. The method for preparing the ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel according to claim 1, characterized in that: During hot rolling, the initial rolling temperature is 1100°C to 1200°C, the final rolling temperature is controlled at 850°C to 900°C, and the final rolling deformation is controlled at 30% to 50%.

3. The method for preparing the ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel according to claim 2, characterized in that: The initial rolling temperature is 1100°C ~ 1150°C, the final rolling temperature is controlled at 850°C ~ 880°C, and the final rolling deformation is controlled at 35% ~ 45%.

4. The method for preparing ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel according to claim 1, characterized in that: The first cooling rate is 5°C / s to 10°C / s, and the first preset temperature is 450°C to 480°C.

5. The method for preparing ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel according to claim 1, characterized in that: The second preset temperature is Ms+50°C to Ms°C, and in the process of cooling the thread steel to be processed to the second preset temperature at a second cooling rate, continuous cooling transformation is performed to generate bainite with a content of <35 vol.%.

6. The method for preparing ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel according to claim 1, characterized in that: The third preset temperature is Ms+5°C to Ms-30°C, and the bainite content generated by continuous cooling and transformation of the threaded steel to be processed to the third preset temperature at a third cooling rate is >50vol.%, the remaining untransformed austenite content is <20vol.%, and the average C content is >1.0wt.%.

7. The method for preparing ultra-high strength and ductility ultra-fine bainite finish-rolled threaded steel according to claim 1, characterized in that: During tempering treatment, the tempering temperature is 300℃~450℃, and the holding time is 15h~60h.

8. An ultra-high strength and ductile ultra-fine bainite finish-rolled threaded steel bar, characterized in that: The preparation method according to any one of claims 1 to 7 has a retained austenite content of ≤15.1wt.%, an average C content of 1.21wt.% to 1.52wt.%, a yield strength of 1200MPa to 1350MPa, a tensile strength of 1480MPa to 1645MPa, a uniform elongation of 5% to 7%, and a total elongation of 12% to 15.2%.