A composite diaphragm coating, a modified diaphragm, and a preparation method and application thereof
By using a composite separator coating in the lithium-ion battery separator, combining a heat-resistant coating of cellulose fibrils and silica with a rubber coating of vegetable oil cellulose, the thermal stability and ion transport of the lithium-ion battery separator are solved. Performance issues, achieving higher battery cycle stability and thermal stability.
Patent Information
- Application Number
- CN202311716956.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-14
AI Technical Summary
Existing lithium-ion battery separators can easily cause thermal runaway and short circuit during high-rate charge and discharge processes, and the nanocellulose heat-resistant coating has poor ion transmission performance, resulting in poor battery cycle performance.
Composite separator coating is used, including heat-resistant coating and rubber coating. The heat-resistant coating is composed of cellulose fibrils and silica. The rubber coating is composed of vegetable oil and cellulose polymer. The combination improves the Thermal stability and ion transport properties of the separator.
It significantly improves the thermal stability and cycle stability of the battery, reduces the consistency of the internal resistance of the battery, enhances the transmission capacity of lithium ions or sodium ions, and improves the moisture absorption problem of the heat-resistant coating.
Smart Images

Figure CN117937054B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery diaphragms, and more specifically, to a composite diaphragm coating, a modified diaphragm, and a preparation method and application thereof. Background Art
[0002] At present, commercial lithium-ion batteries mainly use liquid electrolytes as electrolytes and are used in conjunction with diaphragms. The working principle is that during the charging process, due to the pressure of the external power source, lithium ions first enter the electrolyte from the positive electrode and then pass through the diaphragm to the negative electrode; during the discharge process, lithium ions are transferred from the negative electrode to the positive electrode through the diaphragm. Therefore, the diaphragm in lithium-ion batteries not only plays a role in blocking electrons between the positive and negative electrodes, but also has the function of transmitting lithium ions, and also affects the internal resistance and interface structure of the battery, which has an important impact on the cycle, capacity and safety performance of lithium-ion batteries.
[0003] The commonly used diaphragms are mainly polyolefin diaphragm materials with microporous structures, such as single-layer and multi-layer films of polyethylene or polypropylene; however, the polyolefin diaphragm itself has a large thermal shrinkage rate, and a large amount of heat will be generated during the high-rate charge and discharge process of the battery, which can easily cause the polyolefin diaphragm to deform and cause direct contact between the positive and negative electrodes, resulting in a short circuit and thermal runaway. In order to solve the heat resistance and safety problems of the above-mentioned polyolefin diaphragm, a uniform layer of ceramic powder is usually coated on one or both sides to form a heat-resistant layer, thereby improving the heat resistance of the diaphragm to reduce its shrinkage rate, and then effectively preventing thermal runaway caused by internal short circuits in the battery.
[0004] However, in actual use, it was found that the inorganic particles (ceramic powder) in the ceramic coating were easy to fall off and serious powder loss occurred. In order to solve the problem of ceramic coating falling off and powder loss, people began to look for other high-temperature resistant coatings to replace ceramic coatings. For example, the prior art discloses a high-temperature resistant coating composite diaphragm and its preparation method and application, which improves the heat resistance of polyolefin diaphragms by replacing ceramic powder with nanocellulose crystals with excellent thermal stability; however, since nanocellulose is prone to serious agglomeration during the drying process and blocks the micropores of the polyolefin diaphragm, it hinders ion transmission and causes poor battery cycle performance; at the same time, due to the presence of nanocellulose, the modified diaphragm is easy to absorb moisture, which is not conducive to its application in non-aqueous batteries such as lithium ion or sodium ion batteries. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects and shortcomings of the existing nanocellulose heat-resistant coating diaphragm, such as poor ion transport performance, which leads to poor battery cycle performance, and to provide a composite diaphragm coating.
[0006] Another object of the present invention is to provide a method for preparing the above-mentioned composite diaphragm coating.
[0007] Another object of the present invention is to provide an application of the above-mentioned composite diaphragm coating in a lithium ion battery or a sodium ion battery.
[0008] Another object of the present invention is to provide a modified diaphragm.
[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0010] The invention protects a composite diaphragm coating, which comprises a heat-resistant coating and a glue coating; the heat-resistant coating comprises cellulose fibrils and silicon dioxide; the glue coating comprises a polymer of vegetable oil and cellulose.
[0011] The present invention combines a heat-resistant coating and a glue coating to form a composite diaphragm coating, which can not only effectively improve the thermal stability of the polyolefin diaphragm to prevent it from shrinking due to heat, but also significantly improve the bonding performance between the polyolefin diaphragm and the pole piece, thereby improving the consistency of the battery's internal resistance to improve the battery's cycle stability; at the same time, the tendency of the polyolefin base film to shrink due to heat can be further suppressed by the rigidity of the pole piece. The silicon dioxide in the heat-resistant coating can effectively reduce the tendency of cellulose fibrils to agglomerate so that they are evenly dispersed to promote the transmission of lithium ions or sodium ions; moreover, it can also react with the hydrofluoric acid generated by the electrolyte during the circulation process to further improve the battery's cycle performance. The polymer formed by vegetable oils and cellulose as the main raw materials in the glue coating contains active groups, which can not only increase the bonding force between the polyolefin diaphragm and the pole piece, but also use cellulose to increase the compatibility between the glue coating and the heat-resistant coating, and can also effectively improve the heat-resistant coating's easy moisture absorption.
[0012] Optionally, the mass ratio of the cellulose fibrils to silica is (0.1-0.5):(2-3); the vegetable oil includes any one or more of an amide group, a double bond that can undergo polymerization reaction, or a carbonyl group; the double bond that can undergo polymerization reaction includes a carbon-oxygen double bond and a carbon-carbon double bond; the vegetable oil and amino alcohol are subjected to an ester exchange reaction to obtain a vegetable oil-based monomer; after the vegetable oil-based monomer is grafted with anhydride compounds, it is subjected to a polymerization reaction with the cellulose to obtain a polymer emulsion, and finally dried to obtain the glue coating.
[0013] Specifically, the cellulose fibrils in the heat-resistant coating can be cellulose nanofibrils, and the silicon dioxide can be nano-silicon dioxide particles; the cellulose in the glue coating can be cellulose nanocrystals, and the cellulose fibrils in the heat-resistant coating or the cellulose in the glue coating can be obtained by drying their suspensions. In addition, the heat-resistant coating and the glue coating are arranged adjacent to each other, that is, the composite diaphragm coating includes a heat-resistant coating and a glue coating stacked in sequence; the heat-resistant coating is obtained by drying a mixture of a cellulose nanofibril suspension and nano-silicon dioxide in a mass ratio of 50:(2-3);
[0014] The glue coating is obtained by drying a polymer emulsion; the polymer emulsion is obtained by grafting anhydride compounds onto plant oil-based monomers, forming an emulsion with a cellulose nanocrystal suspension, and then undergoing free radical polymerization; the plant oil-based monomer is obtained by an ester exchange reaction between plant oils and amino alcohols.
[0015] A mixture of cellulose nanofibril suspension and nano-silica is formed in a specific ratio, and the three-dimensional network structure of cellulose nanofibrils and nano-silica interact with each other, which can not only improve the dispersion uniformity and stability of the cellulose nanofibril suspension, but also reduce the agglomeration tendency of cellulose nanofibrils in the drying process, thereby effectively preventing the cellulose nanofibrils from agglomerating and clogging the microporous structure of the polyolefin-based membrane, thereby promoting the transmission of lithium ions or sodium ions; it can also allow the hydrofluoric acid generated by the electrolyte during the circulation process to react with the nano-silica to further improve the cycle performance of the battery.
[0016] The cellulose nanocrystals in the adhesive coating have a rod-like structure, which can not only increase the compatibility with the heat-resistant layer, but also work together with the cellulose nanofibrils in the heat-resistant layer to promote the transfer of lithium ions or sodium ions in the electrolyte by using the O in the -OH in cellulose; at the same time, the adhesive layer covering the surface of the heat-resistant layer contains amino groups, which can form intermolecular effects with the hydroxyl groups in cellulose to reduce the adsorption of moisture by the composite diaphragm coating; moreover, the adhesive coating can also improve the bonding performance between the modified diaphragm and the pole piece, which can not only improve the consistency of the battery internal resistance to improve the battery cycle stability, but also use the rigidity of the pole piece to suppress the tendency of the polyolefin base film to shrink due to heat, thereby further improving the thermal stability of the modified diaphragm.
[0017] It should also be noted that the average thickness of the heat-resistant coating can be specifically 0.15 to 0.3 μm, and the thickness of the adhesive coating is 0.8 to 1.2 μm. The solid content of the cellulose nanofibril suspension is 0.2wt% to 1wt%, and the solid content of the cellulose nanocrystal suspension is 0.1wt% to 0.5wt%. The cellulose nanofibril suspension or the cellulose nanocrystal suspension is a mixture of cellulose nanofibrils or cellulose nanocrystals and water, and its solid content mainly affects the viscosity of the system, and thus affects the coating effect of the heat-resistant coating or the adhesive coating. The cellulose nanofibril suspension and the cellulose nanocrystal suspension with the above solid content can make the system have a more suitable viscosity, thereby reducing the occurrence of missing coating during the coating process, and obtaining a more uniform and complete heat-resistant coating and adhesive coating.
[0018] Cellulose nanofibrils and cellulose nanocrystals have the same raw material source and are obtained through different processing methods. They can be purchased or made at home.
[0019] For example, cellulose nanofibrils are made from straw powder or wood powder, and lignin is removed by sodium sulfite under acidic conditions (the solution is adjusted to pH = 4-5 by glacial acetic acid), and then most of the hemicellulose is removed by 5wt% sodium hydroxide solution or potassium hydroxide solution to obtain purified cellulose; then the purified cellulose is added to deionized water to form a suspension, which is successively homogenized and centrifuged to obtain a stable suspension on the upper layer, which is a cellulose nanofibril solution; finally, the cellulose nanofibril solution is dried to obtain cellulose nanofibrils. For details, please refer to Wang Haiying. Preparation and crystal transformation of cellulose nanofibrils [D]. Nanjing: Nanjing Forestry University, 2014.
[0020] Cellulose nanocrystals are made from straw powder or wood powder by sulfuric acid hydrolysis. For details, please refer to Wu Kaili. Preparation of Nanocellulose Crystals and Their Application in Papermaking [D]. Shaanxi: Shaanxi University of Traditional Chinese Medicine, 2010.
[0021] The vegetable oil-based monomer is obtained by an ester exchange reaction between vegetable oil and amino alcohol, which may specifically include the following steps: after mixing the vegetable oil, amino alcohol and catalyst, reacting at 60-80° C. in an inert gas atmosphere (N2) for 6-8 hours, removing unreacted substances and catalyst to obtain the vegetable oil-based monomer.
[0022] The polymer emulsion is obtained by grafting anhydride compounds onto plant oil-based monomers, forming an emulsion with a cellulose nanocrystal suspension, and then undergoing free radical polymerization.
[0023] Specifically, the method may include the following steps: firstly, mixing a plant oil-based monomer and an acid anhydride compound, reacting them in an inert gas atmosphere (N2) at 60-80°C for 8-12 hours, removing unreacted materials and catalysts to obtain a reaction monomer; then, uniformly mixing the reaction monomer with a cellulose nanocrystal suspension to obtain a pre-emulsion, adding a free radical initiator, and reacting them in an inert gas atmosphere (N2) at 60-80°C for 6-10 hours to obtain a polymer emulsion.
[0024] The mass ratio of the reaction monomer to the cellulose nanocrystal suspension is (10-30):(0.1-0.3), preferably (15-25):(0.15-0.25), and more preferably 20:0.2.
[0025] Optionally, the mass ratio of the cellulose nanofibril suspension to silicon dioxide is 50:(2.2-2.8), preferably 50:(2.4-2.6), and more preferably 50:2.5.
[0026] Optionally, the mass ratio of the vegetable oil to the amino alcohol is (20-50):(1-8); specifically, it can be 20:2, 50:1 or 20:8.
[0027] Optionally, the mass ratio of the plant oil-based monomer to the acid anhydride compound is (10-30):(30-50); preferably (15-25):(35-45); specifically, it can be 20:40, 15:45 or 25:35.
[0028] Optionally, the vegetable oil is one or more of olive oil, rubber seed oil, castor oil, tung oil, soybean oil, sunflower seed oil, rapeseed oil, peanut oil and almond oil. The amino alcohol is at least one of ethanolamine, propanolamine or dimethylaminoethanol; and the acid anhydride compound is at least one of methacrylic anhydride, acetic anhydride or maleic anhydride.
[0029] In actual application, the heat-resistant coating in the composite diaphragm coating is arranged on the surface of the polyolefin base film. At this time, the particle size of the silicon dioxide needs to be adapted to the micropores of the polyolefin diaphragm. When the particle size of the silicon dioxide is small, it is easy to block the micropores of the polyolefin base film and cause excessive air permeability. Specifically, based on the micropores of the existing commonly used polyolefin base films, the suitable particle size of the silicon dioxide can be 60 to 100 nm. Specifically, it can be 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm or 100 nm.
[0030] The present invention also protects a method for preparing a composite diaphragm coating, comprising the following steps:
[0031] The polymer emulsion is applied to the surface of the heat-resistant coating and dried to obtain a composite diaphragm coating;
[0032] The heat-resistant coating is obtained by drying a mixture of a cellulose nanofibril suspension and nano-silicon dioxide in a mass ratio of 50:(2-3);
[0033] The adhesive coating is obtained by drying a polymer emulsion; the polymer emulsion is obtained by grafting an acrylic anhydride compound onto a plant oil-based monomer, forming an emulsion with a cellulose nanocrystal suspension, and then undergoing a free radical polymerization reaction; the plant oil-based monomer is obtained by an ester exchange reaction between plant oils and amino alcohols.
[0034] The use of the above-mentioned composite diaphragm coating in lithium-ion batteries or sodium-ion batteries is also within the protection scope of the present invention.
[0035] The present invention also protects a modified diaphragm, comprising a polyolefin base film and a coating coated on one side or both sides of the base film, wherein the coating is the composite diaphragm coating, and the heat-resistant coating is arranged between the polyolefin base film and the rubber coating.
[0036] Compared with the prior art, the present invention has the following beneficial technical effects:
[0037] The present invention combines a heat-resistant coating and a glue coating to form a composite diaphragm coating, which can not only effectively improve the thermal stability of the polyolefin diaphragm to prevent it from shrinking due to heat, but also significantly improve the bonding performance between the polyolefin diaphragm and the pole piece, thereby improving the consistency of the battery's internal resistance to improve the battery's cycle stability; at the same time, the tendency of the polyolefin base film to shrink due to heat can be further suppressed by the rigidity of the pole piece. The silicon dioxide in the heat-resistant coating can effectively reduce the tendency of cellulose fibrils to agglomerate so that they are evenly dispersed to promote the transmission of lithium ions or sodium ions; moreover, it can also react with the hydrofluoric acid generated by the electrolyte during the circulation process to further improve the battery's cycle performance. The polymer formed by vegetable oils and cellulose as the main raw materials in the glue coating contains active groups, which can not only increase the bonding force between the polyolefin diaphragm and the pole piece, but also use cellulose to increase the compatibility between the glue coating and the heat-resistant coating, and can also effectively improve the heat-resistant coating's easy moisture absorption.
[0038] The polymer emulsion formed by using vegetable oil and cellulose suspension as main raw materials in the present invention not only has high stability and can effectively prevent stratification during coating, but also can significantly improve the compatibility of the coating and the heat-resistant layer, and utilize the large number of active groups contained to improve the bonding strength with the pole piece. Moreover, compared with the petroleum-based materials currently used for the coating layer of lithium battery or sodium battery separator, it also has the advantages of being more environmentally friendly and lower cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Schematic diagram of the structure of the modified diaphragm in Examples 1 to 6.
[0040] Figure 2 This is a physical picture of the polymer emulsion dispersed in water in Example 1.
[0041] Figure 3 The graph is a graph showing the capacity retention rate of the battery assembled using the modified separator in Example 1 as a function of the number of cycles. DETAILED DESCRIPTION
[0042] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0043] Cellulose nanofibrils: 20 g of straw powder (60 mesh) was added to 150 g of deionized water and heated to 100°C, followed by adding 2 mL of glacial acetic acid, 4 g of sodium chlorite and 300 mL of a 5 wt% sodium hydroxide solution to form a mixed solution; the mixed solution was then added to 150 g of deionized water, diluted and added to a high-pressure homogenizer, treated at a pressure of 800 bar for 3 times, and then centrifuged at 5000 r / min to separate the suspension, taking the upper stable suspension as the cellulose nanofibril solution; finally, the cellulose nanofibril solution was dried to obtain cellulose nanofibrils.
[0044] Cellulose nanocrystals: Take 20g of straw powder (60 mesh) and 10g of sulfuric acid (64wt%) and hydrolyze at 45℃ for 4h, add 200g of deionized water to dilute to form a suspension, and then centrifuge the suspension at 5000r / min for 10min to remove excess acid. The resulting precipitate is repeatedly centrifuged and rinsed with deionized water until the supernatant becomes turbid; then the supernatant after centrifugation is dialyzed with deionized water to achieve a constant neutral pH, and the resulting suspension is the cellulose nanocrystal solution; finally, the cellulose nanocrystal solution is dried to obtain cellulose nanocrystals.
[0045] Example 1
[0046] A composite diaphragm coating comprises a heat-resistant coating (average thickness of 0.2 μm) and a glue coating (average thickness of 1.0 μm) stacked in sequence; the heat-resistant coating is obtained by drying a heat-resistant coating composite material, and the glue coating is obtained by drying a polymer emulsion.
[0047] The heat-resistant coating composite material is a mixture of cellulose nanofibril suspension (solid content of 0.5wt%) and nano silicon dioxide (average particle size of 60-100nm) in a mass ratio of 50:2.5.
[0048] The above polymer emulsion is prepared by the following preparation method:
[0049] S1. By weight, 20 parts of vegetable oil (olive oil), 2 parts of amino alcohol (dimethylaminoethanol) and 0.2 parts of catalyst (sodium methoxide) were reacted at 60 ° C in an inert gas atmosphere (N2) for 6 hours, and the unreacted product and the catalyst were removed to obtain a vegetable oil-based monomer;
[0050] S2. After 20 parts of the vegetable oil-based monomer in S1 and 40 parts of methacrylic anhydride were reacted at 60 ° C in an inert gas atmosphere (N2) for 8 hours, the unreacted product and the catalyst were removed to obtain a reaction monomer;
[0051] S3. Mix 20 parts of the reaction monomer in S2 with 0.2 parts of cellulose nanocrystal suspension (solid content is 1 wt%) and ultrasonically treat for 5 minutes to obtain a pre-emulsion, then add 0.008 parts of initiator (potassium persulfate), react at 65°C in an inert gas atmosphere (N2) for 6 hours to obtain a polymer emulsion.
[0052] Take an appropriate amount (5 drops) of the polymer emulsion obtained above and add it to water to observe its dispersion uniformity and stability in the aqueous solution. Figure 2 As shown, it can be found that the polymer emulsion is evenly dispersed in water, and no stratification phenomenon is found after 24 hours, that is, the polymer emulsion has good dispersion uniformity and stability in water, which is beneficial to improve the uniformity of the glue coating.
[0053] A method for preparing a composite diaphragm coating comprises the following steps:
[0054] First, the heat-resistant coating composite material is applied to the surface of the substrate and dried at 60°C for 1 min to obtain a heat-resistant coating; then, the polymer emulsion is applied to the surface of the heat-resistant coating and dried at 60°C for 1 min to obtain a composite diaphragm coating.
[0055] A modified diaphragm (such as Figure 1 As shown), it includes a polyolefin base film (PE film) and a heat-resistant coating and a glue coating sequentially stacked on the single-side surface of the polyolefin base film, and can be prepared by the following preparation method: first, the heat-resistant coating composite material is applied to the surface of the substrate, and the heat-resistant coating is obtained by drying; then, the polymer emulsion is applied to the surface of the heat-resistant coating, and the glue coating is formed by drying to obtain the modified diaphragm.
[0056] Example 2
[0057] A composite diaphragm coating comprises a heat-resistant coating (average thickness of 0.18 μm) and a glue coating (average thickness of 1.1 μm) stacked in sequence; the heat-resistant coating is obtained by drying a heat-resistant coating composite material, and the glue coating is obtained by drying a polymer emulsion.
[0058] The heat-resistant coating composite material is substantially the same as that in Example 1, except that the mass ratio of the cellulose nanofibril suspension to the nano-silicon dioxide is 50:2.
[0059] The preparation method of the above polymer emulsion is basically the same as that of Example 1, except that: in step S1, the olive oil is 50 parts and the amino alcohol is 1 part; in step S2, the plant oil-based monomer is 15 parts and the methacrylic anhydride is 45 parts.
[0060] A preparation method of a composite diaphragm coating comprises the following steps: firstly coating a heat-resistant coating composite material on a substrate surface, and drying at 60°C for 1 min to obtain a heat-resistant coating; then coating a polymer emulsion on the surface of the heat-resistant coating, and drying at 60°C for 1 min to obtain a composite diaphragm coating.
[0061] A modified diaphragm includes a polyolefin base film (PE film) and a heat-resistant coating and a glue coating sequentially stacked on a single side surface of the polyolefin base film. The diaphragm can be prepared by the following preparation method: firstly, the heat-resistant coating composite material is coated on the surface of a substrate, and the heat-resistant coating is obtained by drying; then, the polymer emulsion is coated on the surface of the heat-resistant coating, and the glue coating is formed by drying to obtain the modified diaphragm.
[0062] Example 3
[0063] A composite diaphragm coating comprises a heat-resistant coating (average thickness of 0.25 μm) and a glue coating (average thickness of 1.0 μm) stacked in sequence; the heat-resistant coating is obtained by drying a heat-resistant coating composite material, and the glue coating is obtained by drying a polymer emulsion.
[0064] The heat-resistant coating composite material is substantially the same as that in Example 1, except that the mass ratio of the cellulose nanofibril suspension to the nano-silicon dioxide is 50:3.
[0065] The preparation method of the above polymer emulsion is basically the same as that of Example 1, except that: in step S1, the olive oil is 20 parts and the amino alcohol is 8 parts; in step S2, the plant oil-based monomer is 25 parts and the methacrylic anhydride is 35 parts.
[0066] A preparation method of a composite diaphragm coating comprises the following steps: firstly coating a heat-resistant coating composite material on a substrate surface, and drying at 60°C for 1 min to obtain a heat-resistant coating; then coating a polymer emulsion on the surface of the heat-resistant coating, and drying at 60°C for 1 min to obtain a composite diaphragm coating.
[0067] A modified diaphragm includes a polyolefin base film (PE film) and a heat-resistant coating and a glue coating sequentially stacked on a single side surface of the polyolefin base film. The diaphragm can be prepared by the following preparation method: firstly, the heat-resistant coating composite material is coated on the surface of a substrate, and the heat-resistant coating is obtained by drying; then, the polymer emulsion is coated on the surface of the heat-resistant coating, and the glue coating is formed by drying to obtain the modified diaphragm.
[0068] Example 4
[0069] A composite diaphragm coating comprises a heat-resistant coating (average thickness of 0.2 μm) and a glue coating (average thickness of 1.0 μm) stacked in sequence; the heat-resistant coating is obtained by drying a heat-resistant coating composite material, and the glue coating is obtained by drying a polymer emulsion.
[0070] The preparation method of the polymer emulsion is substantially the same as that of Example 1, except that the vegetable oil in step S1 is castor oil, and the amino alcohol is ethanolamine (2-hydroxyethylamine).
[0071] A preparation method of a composite diaphragm coating comprises the following steps: firstly coating a heat-resistant coating composite material on a substrate surface, and drying at 60°C for 1 min to obtain a heat-resistant coating; then coating a polymer emulsion on the surface of the heat-resistant coating, and drying at 60°C for 1 min to obtain a composite diaphragm coating.
[0072] A modified diaphragm includes a polyolefin base film (PE film) and a heat-resistant coating and a glue coating sequentially stacked on a single side surface of the polyolefin base film. The diaphragm can be prepared by the following preparation method: firstly, the heat-resistant coating composite material is coated on the surface of a substrate, and the heat-resistant coating is obtained by drying; then, the polymer emulsion is coated on the surface of the heat-resistant coating, and the glue coating is formed by drying to obtain the modified diaphragm.
[0073] Example 5
[0074] A composite diaphragm coating comprises a heat-resistant coating (average thickness of 0.2 μm) and a glue coating (average thickness of 1.0 μm) stacked in sequence; the heat-resistant coating is obtained by drying a heat-resistant coating composite material, and the glue coating is obtained by drying a polymer emulsion.
[0075] The heat-resistant coating composite material is substantially the same as that in Example 1, except that the mass ratio of the cellulose nanofibril suspension to the nano-silicon dioxide is 50:0.5.
[0076] A preparation method of a composite diaphragm coating comprises the following steps: firstly coating a heat-resistant coating composite material on a substrate surface, and drying at 60°C for 1 min to obtain a heat-resistant coating; then coating a polymer emulsion on the surface of the heat-resistant coating, and drying at 60°C for 1 min to obtain a composite diaphragm coating.
[0077] A modified diaphragm includes a polyolefin base film (PE film) and a heat-resistant coating and a glue coating sequentially stacked on a single side surface of the polyolefin base film. The diaphragm can be prepared by the following preparation method: firstly, the heat-resistant coating composite material is coated on the surface of a substrate, and the heat-resistant coating is obtained by drying; then, the polymer emulsion is coated on the surface of the heat-resistant coating, and the glue coating is formed by drying to obtain the modified diaphragm.
[0078] Example 6
[0079] A composite diaphragm coating comprises a heat-resistant coating (average thickness of 0.2 μm) and a glue coating (average thickness of 1.0 μm) stacked in sequence; the heat-resistant coating is obtained by drying a heat-resistant coating composite material, and the glue coating is obtained by drying a polymer emulsion.
[0080] The heat-resistant coating composite material is substantially the same as that in Example 1, except that the mass ratio of the cellulose nanofibril suspension to the nano-silicon dioxide is 50:5.
[0081] A preparation method of a composite diaphragm coating comprises the following steps: firstly coating a heat-resistant coating composite material on a substrate surface, and drying at 60°C for 1 min to obtain a heat-resistant coating; then coating a polymer emulsion on the surface of the heat-resistant coating, and drying at 60°C for 1 min to obtain a composite diaphragm coating.
[0082] A modified diaphragm includes a polyolefin base film (PE film) and a heat-resistant coating and a glue coating sequentially stacked on a single side surface of the polyolefin base film. The diaphragm can be prepared by the following preparation method: firstly, the heat-resistant coating composite material is coated on the surface of a substrate, and the heat-resistant coating is obtained by drying; then, the polymer emulsion is coated on the surface of the heat-resistant coating, and the glue coating is formed by drying to obtain the modified diaphragm.
[0083] Comparative Example 1
[0084] A diaphragm coating with an average thickness of 1.2 μm is obtained by drying a heat-resistant coating composite material, wherein the heat-resistant coating composite material is the same as that in Example 1.
[0085] A modified diaphragm includes a polyolefin base film (PE film) and a heat-resistant coating arranged on one side of the polyolefin base film. The modified diaphragm can be prepared by the following preparation method: the heat-resistant coating composite material is coated on the surface of a substrate, and dried to form a heat-resistant coating to obtain the modified diaphragm.
[0086] Comparative Example 2
[0087] A diaphragm coating with an average thickness of 1.2 μm is obtained by drying a polymer emulsion, wherein the polymer emulsion is the same as that in Example 1.
[0088] A modified diaphragm includes a polyolefin base film (PE film) and a glue coating arranged on one side of the polyolefin base film. The modified diaphragm can be prepared by the following preparation method: the polymer emulsion is coated on the surface of the substrate, and dried to form a glue coating to obtain the modified diaphragm.
[0089] Performance Testing
[0090] (1) Increased air permeability: The air permeability value A of the modified membranes in Examples 1 to 6 and Comparative Examples 1 to 2 and the air permeability value B of the PE membrane were respectively tested using a Wang Yan type air permeometer, and the increased air permeability value = AB.
[0091] (2) Internal resistance test: The internal resistance of the battery assembled with the modified diaphragms in Examples 1 to 6 and Comparative Examples 1 to 2 was tested using an electrochemical workstation. Test conditions: AC disturbance voltage 10mv, frequency range: 1MH Z ~10000HZ .
[0092] (3) Heat resistance test: The modified separators in Examples 1 to 6 and Comparative Examples 1 to 2 were cut into samples of 100 mm*100 mm, and their longitudinal (MD) dimensions a1 and transverse (TD) dimensions b1 were measured. The marked samples were then placed in an oven at 130°C for 1 hour, and the longitudinal dimensions a2 and transverse dimensions b2 of the samples were measured. The longitudinal shrinkage and transverse shrinkage of the modified separator were calculated by the following formula to evaluate its heat resistance.
[0093] MD shrinkage (%) = (a1-a2) / a1*100%;
[0094] TD shrinkage (%) = (b1-b2) / b1*100%.
[0095] (4) Bonding strength test: The modified diaphragms in Examples 1 to 6 and Comparative Examples 1 to 2 were stacked on the positive electrode sheet respectively, and then subjected to hot pressing treatment using a hot press (hot pressing conditions: 3 MPa, 90 degrees, 60 seconds) to bond the modified diaphragm to the positive electrode sheet. The bonding strength between the modified diaphragm and the electrode sheet was then tested using a peeling tester. The test conditions were: the strip width was 30 mm, and the peeling speed was 300 mm / min.
[0096] (5) Battery test: The modified separators in Examples 1 to 6 and Comparative Examples 1 to 2 were respectively wound with positive electrode sheets (positive electrode material is MCN523) and negative electrode sheets (negative electrode material is graphite) to form batteries (electrolyte is ternary battery electrolyte), and then charged and discharged for 1000 cycles at 25±2°C and 1C rate, and the changes in battery capacity retention were recorded to evaluate the cyclic stability of the modified separator. The test results of the modified separator in Example 1 are as follows: Figure 3 As shown. Figure 3 It can be seen that the capacity retention rate of the modified membrane after 1000 cycles at room temperature reaches more than 90%. The capacity retention rates of the modified membranes in Examples 2 to 4 after 1000 cycles at room temperature are better than those of the modified membranes in Examples 5 and 6, but are all above 85%, meeting the requirements of the national standard GB / T31484-2015.
[0097] Table 1 Performance of modified diaphragms in various embodiments and comparative examples
[0098]
[0099]
[0100] According to the data in Table 1, the air permeability increase value of the modified diaphragm in Examples 1 to 6 is ≤109s / 100cc, and the battery internal resistance is ≤2.48Ω.cm 2At the same time, the MD shrinkage rate is ≤2.3% and the TD shrinkage rate is ≤2.9%, and the bonding strength reaches 5.8-8.2N / m (basically at the same level), indicating that the composite diaphragm coating of the present invention can effectively improve the thermal stability of the polyolefin diaphragm while maintaining a low internal resistance.
[0101] It can be seen from Example 5, Example 2, Example 1, Example 3 and Example 6 that with the increase of the amount of nano-silicon dioxide added in the heat-resistant coating, the increased permeability of the modified membrane gradually decreases, while the internal resistance shows a trend of first decreasing and then increasing. The main reason is that with the increase of the amount of nano-silicon dioxide added, it is more conducive to reducing the agglomeration of cellulose nanofibrils to promote their uniform dispersion, thereby reducing the increased permeability and reducing the internal resistance of the battery; but with the further increase of the amount of nano-silicon dioxide added, more nano-silicon dioxide will increase the internal resistance of the battery, that is, the appropriate amount of nano-silicon dioxide added is more conducive to promoting the ion transport of the modified membrane while reducing the internal resistance of the battery, thereby achieving better battery cycle.
[0102] It can be found from Example 1, Comparative Example 1 and Comparative Example 2 that when the heat-resistant layer is used alone as the diaphragm coating, the adhesion performance between the modified diaphragm and the pole piece is poor; and when the glue coating is used alone as the diaphragm coating, the thermal stability of the modified diaphragm is poor.
[0103] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A composite diaphragm coating, It is characterized in that It comprises a heat-resistant coating and a rubber coating; the heat-resistant coating comprises cellulose fibrils and silicon dioxide; the rubber coating comprises a polymer of plant oil and cellulose; The vegetable oil comprises any one or more of an amide group, a double bond capable of undergoing polymerization reaction, or a carbonyl group; the double bond capable of undergoing polymerization reaction comprises a carbon-oxygen double bond and a carbon-carbon double bond; The vegetable oil and amino alcohol are subjected to an ester exchange reaction to obtain a vegetable oil-based monomer; after the vegetable oil-based monomer is grafted with an anhydride compound, it is subjected to a polymerization reaction with the cellulose to obtain a polymer emulsion, and finally the adhesive coating is obtained by drying.
2. The composite diaphragm coating according to claim 1, It is characterized in that The mass ratio of the cellulose fibrils to silicon dioxide is (0.1-0.5):(2-3).
3. The composite diaphragm coating according to claim 1, It is characterized in that The mass ratio of the vegetable oil to the amino alcohol is (20-50):(1-8).
4. The composite diaphragm coating according to claim 1, It is characterized in that The mass ratio of the vegetable oil-based monomer to the acid anhydride compound is (10-30): (30-50).
5. The composite diaphragm coating according to claim 1, It is characterized in that The vegetable oil is at least one of olive oil, rubber seed oil, castor oil, tung oil, soybean oil, sunflower seed oil, rapeseed oil, peanut oil or almond oil.
6. The composite diaphragm coating according to claim 1, It is characterized in that The amino alcohol is at least one of ethanolamine, propanolamine or dimethylaminoethanol.
7. The composite diaphragm coating according to claim 1, It is characterized in that The acid anhydride compound is at least one of methacrylic anhydride, maleic anhydride or maleic anhydride.
8. The composite diaphragm coating according to claim 1, It is characterized in that The average particle size of the silicon dioxide is 60-100 nm.
9. A method for preparing a composite diaphragm coating, It is characterized in that The following steps are involved: The polymer emulsion is applied to the surface of the heat-resistant coating and dried to obtain a composite diaphragm coating; The heat-resistant coating is obtained by drying a mixture of a cellulose nanofibril suspension and nano-silicon dioxide in a mass ratio of 50:(2-3); The adhesive coating is obtained by drying a polymer emulsion; the polymer emulsion is obtained by grafting anhydride compounds onto plant oil-based monomers, forming an emulsion with a cellulose nanocrystal suspension, and then undergoing free radical polymerization; the plant oil-based monomers are obtained by transesterification of plant oils and amino alcohols; The vegetable oil comprises any one or more of an amide group, a double bond capable of undergoing polymerization reaction or a carbonyl group; the double bond capable of undergoing polymerization reaction comprises a carbon-oxygen double bond and a carbon-carbon double bond.
10. Use of the composite diaphragm coating according to any one of claims 1 to 8 in a lithium ion battery or a sodium ion battery.
11. A modified diaphragm, comprising a polyolefin base film and a coating applied to one or both sides of the base film, It is characterized in that The coating is the composite diaphragm coating according to any one of claims 1 to 8, and the heat-resistant coating is arranged between the polyolefin base film and the rubber coating.