A composite material with tunable exciton emission intensity and valley polarization and preparation method thereof
By constructing a composite material of two-dimensional heterojunction and flexible substrate, the torsion angle controls interlayer coupling and spin coating process, the problem of interlayer exciton emission intensity quenching is solved, and high-efficiency strain-tuning exciton energy and improving emission is achieved. The strength and valley polarization significantly improves the compatibility and performance of the material.
Patent Information
- Application Number
- CN202311655107.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-12-05
AI Technical Summary
When the prior art regulates the photon energy of interlayer excitons of two-dimensional transition metal chalcogenide compounds (TMDCs), the emission intensity is prone to quenching, and the lack of interlayer van der Waals force leads to interlayer sliding, making it difficult to effectively regulate. Optical properties of interlayer excitons.
By constructing a composite material based on two-dimensional heterojunction and flexible substrate, using torsion angle control interlayer coupling, the heterojunction structure is transferred to the flexible substrate by spin coating process, ensuring no slip contact and achieving high-efficiency strain tuning Exciton energy and increase emission intensity with valley polarization.
The emission intensity and valley polarization of the composite material are significantly improved at room temperature and low temperature, solving the problem of interlayer exciton emission intensity quenching, and enhancing the compatibility of the material for complex working conditions, achieving emission energy modulation up to 70meV The effect of the valley polarization is modulated from 0% to 20%.
Smart Images

Figure CN117976737B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a tunable two-dimensional heterojunction composite material, and in particular to a composite material with tunable exciton emission intensity and valley polarization and a preparation method thereof, belonging to the technical field of regulating the exciton luminescence performance of two-dimensional semiconductors and heterojunction materials. Background Art
[0002] Two-dimensional (2D) transition metal dichalcogenides (TMDCs) have unique electronic and optical properties, such as strong light-matter interaction, large exciton binding energy, and valley selectivity, providing a promising platform for the study of exciton many-body effects and optoelectronic device applications. Effective modulation of the electronic and optical properties of 2D TMDCs is crucial for the design and application of optoelectronic devices with different functions. Due to the atomic-scale thickness and high mechanical deformation tolerance of 2D TMDCs, their band structure, carrier mobility, and optical properties can be effectively controlled by strain engineering.
[0003] Van der Waals heterostructures formed by stacking different 2D TMDCs inherit the properties of single-layer materials and generate unique physical processes, such as the formation of interlayer excitons where electrons and holes are located in different layers. Compared with intralayer excitons, interlayer excitons have ultrafast formation processes, long lifetimes, and out-of-plane electric dipole moments, which expand the potential of excitons in optoelectronic device applications. In addition, the layer degree of freedom is directly related to the electronic band structure of TMDCs heterostructures, providing an effective way to form interlayer engineered excitons. Interlayer excitons are very sensitive to interlayer coupling and can be externally modulated by adjusting the lattice parameters and band structure. Recently, it has been reported that the optical properties of interlayer excitons in TMDCs heterostructures can be tuned by strain or high pressure. However, the PL emission intensity of interlayer excitons is severely quenched with the modulation of the emitted photon energy, which may be due to the atomic interlayer sliding caused by the weak interlayer van der Waals forces during the tuning process. Therefore, it is very necessary to develop a new method or mechanism to enhance the emission intensity while tuning the emission energy of interlayer excitons, which is crucial for the practical application of optoelectronic devices. Summary of the invention
[0004] In response to the problems existing in the prior art, the present invention provides a composite material with tunable exciton emission intensity and valley polarization. Based on the stacking structural characteristics between the layers of the composite material and the slip-free contact between the heterojunction structure and the flexible material, the composite material achieves the technical effects of efficient strain tuning of the exciton energy, improving the emission intensity and valley polarization of the composite material. The composite material can work effectively at both room temperature and low temperature, greatly improving the compatibility of the material with complex working conditions.
[0005] The second purpose of the present invention is to provide a method for preparing a composite material with tunable exciton emission intensity and valley polarization. The method realizes high-strength coupling between layers by controlling the torsion angle between layers in a two-dimensional heterojunction. Furthermore, a spin coating process is used to transfer the heterojunction structure to a flexible substrate, thereby avoiding external force damage to the heterojunction during the transfer process. Through the above steps, stable contact is achieved in the heterojunction structure of the composite material and between the heterojunction structure and the flexible substrate, thereby solving the slip problem of layered materials.
[0006] In order to achieve the above technical objectives, the present invention provides a composite material with tunable exciton emission intensity and valley polarization, which is composed of a two-dimensional heterojunction material and a flexible substrate; the two-dimensional heterojunction material includes 1 to 3 layers of stacked two-dimensional transition metal sulfide with a thickness of 0.7 to 3 nm, and there is no slip between the flexible substrate and the two-dimensional heterojunction material;
[0007] The transition metal sulfide has a general chemical formula of MX2, wherein M is one of Ti, In, Ta, Mo, W, Re and Te, and X is S or Se.
[0008] As a preferred solution, the torsion angles between the layers of the stacked two-dimensional transition metal sulfide are the same, which is 0.1 to 4°.
[0009] As a preferred solution, the two-dimensional heterojunction material further includes a two-dimensional semi-metal layer with a thickness of 0.3 to 1.5 nm.
[0010] As a preferred solution, the two-dimensional semi-metal layer is one of graphene, black phosphorus, silicon, arsenic and boron.
[0011] As a preferred solution, the flexible substrate is a single-layer or multi-layer material. When the flexible substrate is a multi-layer composite material, the layers starting from contact with the two-dimensional heterojunction material are a high-viscosity film, a flexible adhesive and a flexible thermoplastic resin.
[0012] The present invention also provides a method for preparing a composite material with tunable exciton emission intensity and valley polarization, wherein all single-layer two-dimensional transition metal sulfides are obtained by mechanical stripping, and are transferred to a silicon-based substrate according to the torsion angle, and a heterojunction precursor is obtained by annealing; a flexible substrate is spin-coated on the surface of the heterojunction precursor, and the composite material is cured, packaged and separated from the silicon-based substrate in sequence to obtain the composite material.
[0013] As a preferred solution, the annealing treatment conditions are: vacuum degree of 0.8×10 -4 mbar~4.2×10 -5 mbar, temperature is 120~180℃, time is 4~8h. Annealing can enhance the interface coupling between heterojunction layers of the material and ensure the formation of interlayer excitons in the material.
[0014] As a preferred solution, the spin coating conditions are: a rotation speed of 4000 to 6000 rpm and a time of 30 to 50 s.
[0015] As a preferred solution, when the flexible substrate is a multi-layer material, the high-viscosity film is PVA, the flexible adhesive is silicone, and the flexible thermoplastic resin is PET and / or PETG, wherein the high-viscosity film and the flexible thermoplastic resin need to be heated and baked when bonded, and the baking temperature is 60-70°C and the baking time is 1-3 minutes.
[0016] As a preferred solution, when the high-viscosity film is PVA, the preparation process of its spin coating liquid is: stir solid PVA particles and water at 100-130°C and 800-900 rpm for 3-4 hours to obtain a PVA spin coating liquid with a PVA concentration of 3-20wt%.
[0017] As a preferred solution, the PVA spin coating liquid needs to be heated at 50-80° C. for 1-3 minutes to remove moisture after spin coating, and the thickness of the obtained PVA film is 20-40 μm.
[0018] As a preferred solution, the thickness of the silica gel layer is 40 to 60 μm.
[0019] Compared with the prior art, the beneficial technical effects of the present invention are:
[0020] 1) The composite material provided by the present invention realizes efficient strain of the whole material by encapsulating the two-dimensional heterojunction with flexible materials, that is, the strain process can effectively act on the lattice of the heterojunction material, avoiding the sliding effect of the two-dimensional heterojunction during the bending process; in addition, the two-dimensional transition metal sulfide material stacked according to a specific twist angle can effectively adjust the emission energy, intensity and valley polarization of the excitons during the strain process, thereby effectively solving the problem of PL intensity quenching of the heterojunction material under stress.
[0021] 2) In the preparation method provided by the present invention, high-strength coupling between layers is achieved by controlling the torsion angle between each layer in the two-dimensional heterojunction. Furthermore, the heterojunction structure is transferred to a flexible substrate by a spin coating process, thereby avoiding external force damage to the heterojunction during the transfer process. Through the above steps, stable contact is achieved in the heterojunction structure of the composite material and between the heterojunction structure and the flexible substrate, thereby solving the slip problem of layered materials.
[0022] 3) In the technical solution provided by the present invention, the material is endowed with efficient strain characteristics based on the stable characteristics of the material. The composite material can work effectively at room temperature and low temperature of about 10K. According to the test, the composite material achieves emission energy modulation of up to 70meV by applying controllable flexible strain, which increases the PL intensity of interlayer excitons by 2.6 times at room temperature. In addition, under non-resonant excitation, the valley polarization of interlayer excitons is modulated from nearly 0% to about 20% at 10K. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the process of preparing the heterojunction precursor in Example 1;
[0024] Figure 2 This is a schematic diagram of the heterojunction precursor spin coating packaging process in Example 1;
[0025] Figure 3 This is a schematic diagram of the flexible substrate used in Example 1;
[0026] Figure 4 The morphology characterization results of the two-dimensional heterojunction structure in the composite material obtained in Example 1;
[0027] in, Figure 4 a is an optical photograph; Figure 4 b is SHG Mapping and polarization resolution image; Figure 4 c is a high-resolution STM image; Figure 4 d is TEM image;
[0028] Figure 5 The composite material provided in Example 1 has different number of layers of WSe. 2 / WS 2 Room temperature strain-dependent PL spectra in heterojunctions;
[0029] in, Figure 5 a. Figure 5 f and Figure 5 k is 1L WSe 2 / 1L WS 2 、2L WSe 2 / 1L WS 2 and 1L WSe 2 / 2L WS 2 Heterojunction strain-dependent PL spectra; Figure 5 b. Figure 5 g and Figure 5 l is the 1L WSe under different strains 2 / 1L WS 2 、2L WSe 2 / 1LWS 2 and 1L WSe 2 / 2L WS 2 The intensity ratio of exciton emission with and without strain extracted from the PL spectrum of the heterostructure; Figure 5 c. Figure 5 h and Figure 5 m is the exciton peak energy of the three heterostructures under different strains; Figure 5 d. Figure 5 i and Figure 5 n is the calculated exciton peak energy versus applied strain; Figure 5 e. Figure 5 j and Figure 5 o is the band structure of the three heterostructures in the strain range from -1% to 1%;
[0030] Figure 6 The composite material provided in Example 1 has different number of layers of WSe. 2 / WS 2 Raman spectra of heterojunctions with and without strain;
[0031] Figure 7 1L WS in two-dimensional transition metal sulfides 2 、1L WSe 2 Strain-dependent PL spectroscopy results;
[0032] in, Figure 7 a and Figure 7 b is 1L WS 2 and 1L WSe 2 PL spectra as a function of strain; Figure 7 c and Figure 7 d is from Figure 7 a. Figure 7 b The PL peak energy and fitted strain modulation efficiency S under different strains extracted ΔEg ;
[0033] Figure 8 2L WS in two-dimensional transition metal sulfides 2 、2L WSe 2 Strain-dependent PL spectroscopy results;
[0034] in, Figure 8 a and Figure 8 b is 2L WS under tensile strain 2 and 2L WSe 2 PL spectrum changes; Figure 8 c and Figure 8 d is the PL peak energy and the fitted strain modulation efficiency S that vary with strain ΔEg .
[0035] Fig. 9is the circular polarization resolved PL spectrum of the composite material provided in Example 1 at 10K with or without strain;
[0036] in, Fig. 9 a. Fig. 9 b and Fig. 9 c are single layer WSe 2 、1L WSe 2 / 1L WS 2 、2L WSe 2 / 1L WS 2 and 1LWSe 2 / 2L WS 2 Circularly polarized PL spectra of the heterostructure under unstrained and 0.5% tensile strain; Figures eh are the energy dependence of the valley polarization degree corresponding to the circularly polarized PL spectra under 0.5% tensile strain;
[0037] Fig.10 is the WS in the composite material provided in Example 2 2 / MoS 2 Strain-dependent PL spectra in heterojunctions;
[0038] in, Fig.10 a. Fig.10 b and Fig.10 c are single-layer MoS 2 , 1L WS 2 / 1L MoS 2 and 2L WS 2 / 1L MoS 2 PL spectra under different strains; Fig.10 d. Fig.10 e and Fig.10 f is a single layer of MoS 2 , 1L WS 2 / 1L MoS 2 and 2L WS 2 / 1L MoS 2 The strain-dependent PL peak energy;
[0039] Fig.11 is the WS in the composite material provided in Example 2 2 / MoS 2 Strain-dependent Raman spectroscopy of heterojunctions;
[0040] in, Fig.11 a. Fig.11 b and Fig.11 c are single-layer MoS 2 , 1L WS 2 / 1L MoS 2 and 2L WS 2 / 1L MoS 2 Raman spectra under different strains.
[0041] Fig.12 The WSe in the composite material provided in Example 2 2 / WS 2 Heterojunction strain-dependent PL spectra;
[0042] in, Fig.12 a is 1L WSe in Comparative Example 2 2 / 1L WS 2 Strain-dependent PL spectra of heterojunctions; Fig.12 b is the peak energy extracted under different strains;
[0043] Fig.13 The WSe in the composite material provided in Comparative Example 4 2 / WS 2 Heterojunction strain-dependent PL spectra;
[0044] in, Fig.13 a is 1L WSe in Comparative Example 4 2 / 1L WS 2 Strain-dependent PL spectra of heterojunctions; Fig.13 b is the peak energy extracted under different strains;
[0045] Fig.14 The weakly coupled WSe in the composite material provided in Example 5 2 / WS 2 PL spectra of the heterojunction with strain dependence;
[0046] in, Fig.14 a and Fig.14 b: 1L WSe with weak interlayer coupling 2 / 1L WS 2 and 1L WSe 2 / 2L WS 2 PL spectrum evolution of heterostructures under tensile and compressive strain; Fig.14 c and Fig.14 d is the strain-dependent exciton PL peak energy and strain modulation efficiency extracted from the spectrum. DETAILED DESCRIPTION
[0047] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively with reference to specific implementation examples below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0049] Example 1
[0050] This embodiment provides a composite material with tunable exciton emission intensity and valley polarization, and the preparation process is as follows:
[0051] 1) Mechanical exfoliation from bulk WSe using adhesive tape 2 , WS 2 Peel off a thin layer of material from the source, then fold the tape in half and tear it apart three times to dissociate an even thinner material. Stick a 1×1cm PDMS film on one side of the glass slide, and then stick the tape with the material on the PDMS film; press the tape gently with your fingers to ensure that the material on the surface and the PDMS are in even and close contact, wait for 3-5 minutes, then peel off the tape from one side of the PDMS, and a portion of the dissociated sample will remain on the PDMS surface. Use a knife to cut off the excess part around the PDMS with the target sample containing the single-layer and double-layer areas;
[0052] 2) The target sample on the PDMS surface was transferred to the 300nm SiO2 layer through a three-dimensional transfer platform under a microscope. 2 / Si substrate, and then stacked another atomic layer sample together to form 1L WSe 2 / 1L WS 2 、2L WSe 2 / 1L WS 2 and 1L WSe 2 / 2L WS 2 In order to ensure that each region has the same twist angle, the angle of the long sides of the upper and lower samples is used as a reference. The angle of the long sides of the upper and lower samples can be precisely controlled by rotating the angle of the three-dimensional transfer platform. Finally, the prepared target heterojunction sample is placed in a vacuum annealing furnace for annealing to reduce interlayer bubbles and impurities to enhance interlayer coupling. The vacuum degree in the furnace is maintained at 3.0×10 -5 mbar, and the temperature was maintained at 130°C for 6 hours to obtain a heterojunction precursor;
[0053] 3) Use a pipette to suck an appropriate amount of PVA solution and drop it on the surface of the target sample on the silicon wafer, then place the sample on a spin coater, set the speed to 5000 rpm and the time to 40 s, spin coat a layer of PVA solution on the substrate attached with the target sample and dry it at 70-80 ° C for 1 minute, then apply a layer of quick-drying silica gel water, adhere it to PET and heat it at 70 ° C for 2 minutes, finally use tweezers to gently separate the PVA from the silicon substrate, thus forming a heterojunction precursor-PVA-silica gel-PET overall flexible substrate with a thickness of about 200 μm ( Figure 3 ), the heterojunction maintained high-quality and complete morphology after being transferred to PVA, and there was no damage when further transferred to PET.
[0054] Example 2
[0055] The preparation method of this embodiment is exactly the same as that of embodiment 1, except that the heterojunction structure in the prepared composite material is 1L MoS 2 , 1L WS 2 / 1L MoS 2 and 2L WS 2 / 1L MoS 2 .
[0056] Comparative Example 1
[0057] The preparation process of this comparative example is exactly the same as that of Example 1, except that the mechanically exfoliated two-dimensional material is directly transferred to the prepared PVA film. The specific operation steps are as follows:
[0058] First, in blank SiO 2 The PVA solution was spin-coated on a Si / Si substrate, the coated substrate was placed on a heating table and heated for 3-5 minutes to remove residual water vapor, and then the previously peeled two-dimensional material was transferred to the solidified PVA surface layer by dry transfer, and then the PVA layer with the two-dimensional material attached was transferred to PET.
[0059] The two-dimensional material is strained by bending the flexible substrate, and the PL spectra under different strains are measured simultaneously. Compared with implementation cases 1 and 2, the peak position and intensity of the exciton emission of the two-dimensional material have only small changes by this method. This is because the two-dimensional material and the PVA substrate have weak van der Waals bonding forces, and when strain is applied by mechanical bending, large slip may occur.
[0060] Comparative Example 2
[0061] The preparation process of this comparative example is exactly the same as that of Example 1, except that the PVA film is replaced by a PMDS film, as follows:
[0062] First, the bulk 2D material source is repeatedly adhered and torn apart with tape to obtain a thinner sample. Then the tape with the thin sample is attached to PMDS, and then slowly torn off to dissociate a single-layer sample. Then, the PDMS with the single-layer target sample attached is transferred to a flexible substrate PET. The sample is deformed by bending the flexible substrate to generate strain, and the PL spectra under different strains are measured. Fig.12 As shown, the PL spectrum exhibits a small strain dependence and modulation efficiency due to the slip between the two-dimensional material and the PDMS substrate.
[0063] Comparative Example 3
[0064] The preparation process of this comparative example is exactly the same as that of Example 1, except that the PVA film is replaced by a PMMA film, as follows:
[0065] First, in blank SiO 2 The PMMA solution was spin-coated on a Si / Si substrate, and then the spin-coated substrate was placed on a heating table and heated for 3-5 minutes to remove residual moisture; the previously peeled two-dimensional material was transferred to the solidified PMMA surface layer by dry transfer, and then the PMMA layer attached with the two-dimensional material was transferred to the flexible substrate PET, and strain was applied to the two-dimensional material by bending the flexible substrate, while measuring the PL spectra under different strains. Due to the weak binding force between the two-dimensional material and PMMA, slippage occurred between the two, and the PL spectrum showed a small strain dependence.
[0066] Comparative Example 4
[0067] The preparation process of this comparative example is exactly the same as that of Example 1, except that the silicone gel is replaced with double-sided tape. Since the double-sided tape has weak adhesion, when the flexible substrate is bent, slippage occurs between the PVA layer and the PET layer, resulting in low strain transfer efficiency. Fig.13 As shown, the heterojunction PL spectrum shows little dependence on strain and a small strain modulation efficiency.
[0068] Comparative Example 5
[0069] The preparation process of this comparative example is exactly the same as that of Example 1, except that the annealing temperature is 80° C., the time is 2 h, and the obtained composite material is a heterojunction structure with weak interlayer coupling.
[0070] In order to better illustrate the characteristics and advantages of the composite material provided by the present invention, the present invention also conducted a series of characterizations and tests on the materials obtained from the above examples and comparative examples:
[0071] The composite material obtained in Example 1 was confirmed to be an R-type stacked heterostructure by measuring the second harmonic generation (SHG) imaging of the heterostructure and the polarization-resolved SHG of the monolayer region, with a twist angle of about 0.4° ( Figure 4b). Scanning tunneling microscopy (STM) images show that 1L WSe 2 / 1L WS 2 The heterostructure region has a typical clear moiré periodic pattern, and the moiré unit size is about 8 nanometers ( Figure 4 c). Moiré structure in transmission electron microscopy (TEM) images ( Figure 4 d) It further confirms that the studied heterostructure has strong interlayer coupling. The evolution of the PL spectra of intralayer and interlayer excitons when different tensile and compressive strains are applied to the three heterostructures in the composite material obtained in Example 1, Figure 5 a) For 1L WSe with a compressive strain of -0.41%, 2 / 1L WS 2 Heterostructure, interlayer exciton IE 1 and WSe 2 The A-exciton peaks blue-shift from 1.353 eV to 1.377 eV and from 1.620 eV to 1.628 eV, respectively. In contrast, when the tensile strain is 1.21%, the peaks red-shift from 1.353 eV to 1.318 eV and from 1.620 eV to 1.586 eV, respectively. It is worth noting that at a compressive strain of -0.41%, the interlayer exciton IE 2 The peak value slightly red-shifts from 1.441eV to 1.447eV; when the tensile strain is 1.21%, the interlayer exciton IE 2 The peak value is slightly blue-shifted from 1.441eV to 1.454eV. Figure 5 f and Figure 5 K shows that in 2L WSe 2 / 1L WS 2 and 1L WSe 2 / 2L WS 2 Similar energy migration trends of interlayer and intralayer excitons with strain are also observed in heterolayers. Figure 5 c. Figure 5 h and Figure 5 m shows the functional relationship between the PL peak energy of interlayer and intralayer excitons in the three heterostructures and the applied strain, as well as the corresponding linear fitting strain modulation efficiency S obtained from the experimental data. ΔEg Compared with the direct transition peak ( Figure 5 WSe in c 2 A exciton is -22.2meV / %, IE 1 =-30.1 meV / %), IE from the indirect KQ transition of momentum 2 The peak exhibits an opposite strain modulation slope and is much smaller (e.g. Figure 5 IE in c 2The strong orbital hybridization of Qdots is insensitive to mechanical strain.
[0072] In order to better understand the PL measurement results as a function of strain, the first principle calculation of the band structure of the heterostructure as a function of strain was performed on the composite material obtained in Example 1 of the present invention. The calculation results show that the KK conversion energy of the heterostructure decreases with increasing tensile strain, while the KQ conversion energy increases. This is mainly due to the larger energy drop of the K point in the conduction band compared to the valence band, while the movement of the Q point is negligible. In contrast, with increasing compressive strain, the WSe 2 / WS 2 The conduction band of the heterostructure K point increases significantly compared to the valence band, while the Q point of the valence band hardly moves, which leads to an increase in the KK conversion energy and a decrease in the KQ conversion energy. These calculated strain-dependent energy changes are in good agreement with the experimental results. In addition to the energy shift, the emission intensity of the excitons can also be modulated to a large extent. As the tensile strain increases, the interlayer excitons (IE 1 and IE 2 ) and intralayer excitons (WSe 2 The ratio of strained to unstrained PL intensity of A-excitons is significantly increased. It is worth noting that compared with 1L WSe 2 / 1L WS 2 Compared with heterogeneous layers, 2L WSe 2 / 1L WS 2 and 1L WSe 2 / 2L WS 2 The emission intensity of all excitons in the heterogeneous layer is enhanced much more under strain, because the encapsulation effect of the additional atomic layer further enhances the interlayer coupling during the strain process. Therefore, this example has demonstrated that the PVA encapsulation method can provide efficient strain modulation and can significantly adjust the emission energy of intralayer and interlayer excitons while improving the PL intensity.
[0073] In order to verify that the applied strain is effectively transferred to the material lattice, this embodiment also measures the Raman spectra of the sample with and without strain. Figure 6 As shown, under the corresponding tensile strain, the characteristic vibration peaks of all monolayers and heterostructures (such as A 1g mode) all show obvious monotonic red shift, and the single-layer WSe 2 of The value moved about 1.2cm -1 For a single-layer WS 2 、1L WSe 2 / 1L WS 2 、2L WSe2 / 1L WS 2 and 1L WSe 2 / 2L WS 2 Heterostructure, WS 2 A 1g The modes were offset by approximately 2.4 cm -1 、3.6cm -1 、4.8cm -1 and 3.8cm -1 .
[0074] The present invention also tests the PL spectra of the excitons in the two-dimensional permetallic sulfide used in the heterojunction structure in Example 1 under different strains. When the applied strain increases from 0% to 1.25%, 1L WS 2 The PL peak of 1L WSe red-shifted from 2.035 eV to 1.953 eV. 2 The PL peak of 1L WS red shifts from 1.651eV to 1.563eV. 2 and 1L WSe 2 The PL intensity of the strain-free state is enhanced by about 4.5 times and 2.5 times, respectively, because the strain bypasses the van Hove singular resonance and suppresses the non-radiative recombination of exciton annihilation. The corresponding band gap change (ΔE g ) are 82meV and 87.6meV respectively. According to the linear fitting of the experimental data, the strain modulation efficiency S is obtained. ΔEg -66.8meV / % and -64.4meV / % respectively ( Figure 7 c, d).
[0075] 2L WS 2 and 2L WSe 2 There are direct and indirect band gap transition peaks. 2 As the strain increases from 0% to 1.25%, the peak energy of A exciton increases from 1.907 to 1.845 eV, and the peak energy of I increases from 1.74 to 1.627 eV. The corresponding strain modulation efficiency S of A exciton and I peak ΔEg -54.2meV / % and -113.2meV / %, respectively. In 2L WSe 2 In the graph, the energies of the A exciton and the I peak show opposite strain dependence, such as Figure 8 As shown in the dashed line in b, as the tensile strain increases from 0% to 1.11%, the I peak red-shifts by 28 meV), while the A exciton blue-shifts by 53 meV. The calculated strain modulation efficiency S of the A exciton and the I peak ΔEg are 21.8meV / % and -41.1meV / %, respectively. From the above test results, we can see that 2L WSe 2The overall PL intensity is significantly enhanced, which indicates that the band gap structure of the material is transformed from an indirect band gap to a direct band gap under strain modulation.
[0076] The present invention also tests the composite material obtained in Example 1 for regulating the exciton multibody complex and valley polarization under low temperature conditions ( Fig. 9 ), the sample was transferred to a self-made curved copper stage to generate a fixed tensile strain, and the copper stage was further fixed in a low-temperature cold trap device for low-temperature testing. 2 Compared with the charged excitons, the composite material showed biexcitons (XX), localized excitons (X) and other charged excitons at 10K due to the reduction of valley scattering and phonon interaction. L ) and other exciton complexes. Under 0.5% tensile strain, compared with the case without strain, the peak energies of the A exciton, charged exciton, biexciton and local exciton of the composite material red-shifted by 22.9meV, 24.5meV, 14.3meV and 24.3meV, respectively.
[0077] The valley polarization of the excitons in the composite material provided by the present invention is significantly enhanced under strain modulation, where the valley polarization degree is defined as: PL =(Ι σ+ -Ι σ- ) / (Ι σ+ +Ι σ- ) under right circular (σ+) polarized light excitation, where Ι σ+ and σ- The collected σ+ and left circular (σ-) polarized PL intensities are shown in Figure 2, respectively. In the absence of strain, due to the simultaneous appearance of the K valley and -K valley under non-resonant excitation, the excitons exhibit very low valley polarization under the excitation of 488nm circularly polarized light. For 1L WSe 2 / 1L WS 2 and 2L WSe 2 / 1L WS 2 Heterostructure, due to the lack of phonon assistance, interlayer indirect exciton IE 2 The momentum of the interlayer excitons decreases with decreasing temperature and finally disappears completely. When the strain is 0.5%, the interlayer exciton IE 1 The peak energies of 1L WSe red-shift from 1.446 eV to 1.413 eV and from 1.412 eV to 1.391 eV, respectively, which increase the valley polarization by 13% and 10% compared with the unstrained case. 2 / 2L WS 2 Heterostructure, due to the similar energy of the conduction band Q point and K point, the momentum indirect KQ transition interlayer exciton IE 2 and momentum direct KK transition interlayer exciton IE 1Both appear at 10 K. Similar to the peak shift behavior at room temperature, when the strain increases to 0.5%, the interlayer exciton IE 1 The interlayer exciton IE is red-shifted from 1.334 eV to 1.344 eV. 2 The valley polarization increases to 8% and 20% from 1.447 eV to 1.434 eV, respectively.
[0078] From the perspective of the working principle, the strain-induced valley polarization enhancement of the composite material provided by the present invention can be attributed to the fact that the strain breaks the triple rotational symmetry of the material, resulting in unequal valley drifts in the momentum space K / -K valley, which in turn leads to different numbers of spin reorganizations under optical pumping. This characteristic is closely related to the stacking structure of the material and the interlayer coupling mode. Due to different light-selective valley conversion paths, the valley polarization of the interlayer excitons is opposite to the valley polarization of the intralayer excitons.
[0079] The above characterization and testing explain that the composite material obtained in Example 1 of the present invention has high responsiveness and sensitivity to external stress from the perspective of structure and working principle, and the use of non-slip flexible packaging can further enhance the above characteristics of the material. In order to further prove that this special packaging method and heterojunction structure also have the same strengthening effect on other two-dimensional transition metal sulfides, the present invention also performs PL spectrum tests and Raman spectroscopy tests on the composite material obtained in Example 2 under different strains, such as Fig.10 As shown in Figure 2, when the tensile strain increases from 0% to 1.15%, 1L MoS 2 The PL peak value of MoS in the heterojunction red shifts from 1.788eV to 1.622eV. When the compressive strain increases from 0% to -0.35%, the PL peak value blue shifts from 1.788eV to 1.828eV. The PL peak energy under different strains can be fitted to obtain the MoS 2 The strain modulation efficiency value S ΔEg -139.6meV / %. 1L MoS 2 The PL intensity of 1L WS decreases significantly with the increase of tensile strain, which is due to the transition of its energy band from direct band gap to indirect band gap. 2 / 1L MoS 2 The interlayer excitons in the heterojunction undergo a significant red shift as the strain increases, and their intensity decreases significantly. By extracting the PL peak energy under different strains, the MoS 2 The strain modulation efficiency is -112.8meV / %, and the interlayer exciton IE 1 , IE 2 The strain modulation efficiency values of 2L WS are -44.9meV / % and -89.1meV / %. 2 / 1L MoS 2As the strain increases in the heterojunction, the interlayer excitons show a smaller red shift range and a slightly reduced intensity. 2 Interlayer exciton IE 1 , IE 2 The strain modulation efficiency values are -52.2meV / %, -23.7meV / %, and -31.1meV / %, respectively.
[0080] Further measurement of 1L MoS in the composite material of Example 2 2 , 1L WS 2 / 1L MoS 2 With 2L WS 2 / 1L MoS 2 The strain-dependent Raman spectroscopy of heterojunction samples confirmed that the lattice deformation occurred, such as Fig.11 1L MoS 2 In-plane vibration mode The out-of-plane vibration mode A shows a sensitive dependence on strain. 1g It shows negligible movement in response to strain. MoS 2 Under tensile and compressive strains ranging from 0% to 1.05% and 0% to -0.35% The vibration peak shift amplitude values are -3.68 and 1.21 cm -1 , the average strain slope is about 3.5cm -1 / %.1L WS 2 / 1L MoS 2 With 2L WS 2 / 1L MoS 2 In-plane vibration modes of heterojunction Out-of-plane vibration mode A 1g All of them shifted significantly toward the low frequency direction. It is worth noting that the heterojunction comes from WS 2 of The mode splits into two E under tensile and compressive strains. 2g mode. Under tensile strain, 1L WS 2 / 1LMoS 2 With 2L WS 2 / 1L MoS 2 Heterojunction cleavage The peak blue shift The peaks are red-shifted, and under compressive strain, the two splitting peaks shift in opposite directions, and their overall performance shows a reverse crossover behavior.
[0081] The interlayer coupling in the heterostructure plays an important role in the formation of momentum direct KK interlayer excitons. Two peaks (marked as IE 1 and IE2 ), these two peaks are only observed in heterostructures with strong interlayer coupling. When bubbles and impurities are introduced between layers during stacking or the interlayer spacing is large, a weak interlayer coupling heterostructure is formed. The heterojunction structure of the composite material obtained in Comparative Example 5 is weak interlayer coupling. Compared with the interlayer excitons with energy coverage of 1.3eV to 1.5eV in the heterostructure with strong interlayer coupling, the interlayer exciton emission of the weak interlayer coupling heterostructure is mainly located in the spectral range of about 1.4eV to 1.5eV, which is consistent with the KQ transition interlayer exciton IE 2 This experimental result shows that the KK transition interlayer exciton IE 1 is suppressed in weakly coupled heterostructures.
[0082] The present invention also performed PL spectra of the composite material obtained in Comparative Example 5 under different strain conditions, with 1LWSe 2 / 1L WS 2 Heterogeneous layers and 1L WSe 2 / 2L WS 2 Heterogeneous layers are used as representatives. Fig.14 The dashed lines in the strain-dependent PL spectra in ab show that the interlayer exciton IE of the KQ transition of these two heterostructures 2 Under tensile strain, it blue-shifts and under compressive strain, it red-shifts, while WSe 2 The A excitons of the nanostructured nanostructures undergo a significant red shift under tensile strain and a blue shift under compressive strain. In addition to the change in emission energy, the PL intensity is significantly enhanced under strain. Fig.14 cd shows the extracted exciton energy as a function of strain. The corresponding strain modulation efficiency can be obtained by linear fitting the experimental data of the two heterostructures, where WSe 2 IE 2 The strain modulation efficiencies of interlayer excitons and A excitons are 17.7 meV / %, 28.7 meV / % and -38.2 meV / %, -50.6 meV / %, respectively. Figure 5 Compared with the data of the strong interlayer coupling sample shown in Figure 2, the strain modulation efficiency of the weak interlayer coupling heterostructure is lower. It can be seen that the preparation of heterostructures with strong interlayer coupling is the key to observe two types of interlayer excitons (IE 1 and IE 2 ) and one of the key factors to obtain high strain modulation efficiency.
[0083] The embodiments and comparative examples of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the enlightenment of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are protected by the present invention.
Claims
1. A composite material with tunable exciton emission intensity and valley polarization, characterized in that: It is composed of a two-dimensional heterojunction material and a flexible substrate; the two-dimensional heterojunction material includes 1 to 3 layers of stacked two-dimensional transition metal sulfide with a thickness of 0.7 to 3 nm, and there is no slip between the flexible substrate and the two-dimensional heterojunction material; The transition metal sulfide has a general chemical formula of MX2, wherein M is one of Ti, In, Ta, Mo, W, Re and Te, and X is S or Se; The preparation method of the composite material is as follows: all the single-layer two-dimensional transition metal sulfides are obtained by mechanical stripping, and transferred to a silicon-based substrate according to the twist angle, and annealed to obtain a heterojunction precursor; a flexible substrate is spin-coated on the surface of the heterojunction precursor, and then cured, packaged and separated from the silicon-based substrate in sequence to obtain the composite material; the annealing treatment conditions are: the vacuum degree is 0.8×10 -4 mbar ~4.2×10 -5 mbar, temperature is 120~180°C, and time is 4~8 h.
2. The composite material with tunable exciton emission intensity and valley polarization according to claim 1, characterized in that: The torsion angles between the layers of the stacked two-dimensional transition metal sulfide are the same, which is 0.1~4°.
3. The composite material with tunable exciton emission intensity and valley polarization according to claim 1, characterized in that: The two-dimensional heterojunction material also includes a two-dimensional semi-metal layer with a thickness of 0.3 to 1.5 nm; the two-dimensional semi-metal layer is one of graphene, black phosphorus, silicon, arsenic and boron.
4. The composite material with tunable exciton emission intensity and valley polarization according to claim 1, characterized in that: The flexible substrate is a single-layer or multi-layer material. When the flexible substrate is a multi-layer composite material, the layers starting from contact with the two-dimensional heterojunction material are a high-viscosity film, a flexible adhesive and a flexible thermoplastic resin.
5. The composite material with tunable exciton emission intensity and valley polarization according to claim 1, characterized in that: The spin coating conditions are: a rotation speed of 4000-6000 rpm and a time of 30-50 s.
6. The composite material with tunable exciton emission intensity and valley polarization according to claim 1, characterized in that: When the flexible substrate is a multilayer material, the high-viscosity film is PVA, the flexible adhesive is silica gel, and the flexible thermoplastic resin is PET and / or PETG. The high-viscosity film and the flexible thermoplastic resin need to be heated and baked when they are bonded. The baking temperature is 60-70°C and the baking time is 1-3 minutes.
7. The composite material with tunable exciton emission intensity and valley polarization according to claim 6, characterized in that: When the high viscosity film is PVA, the preparation process of the spin coating liquid is: stir the solid PVA particles and water at 100-130° C. and 800-900 rpm for 3-4 hours to obtain a PVA spin coating liquid with a PVA concentration of 3-20 wt%.
8. The composite material with tunable exciton emission intensity and valley polarization according to claim 7, characterized in that: The PVA spin coating liquid needs to be heated at 50-80°C for 1-3 minutes after spin coating to remove moisture. The thickness of the obtained PVA film is 20-40 mm; the thickness of the silica gel layer is 40-60 mm.