A kind of anti-scaling material based on lotus leaf bionics and its preparation method
Patent Information
- Application Number
- CN202410258334.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-07
AI Technical Summary
It is difficult to effectively solve the scaling and contamination problems of existing materials in water treatment systems, building materials, medical equipment and other fields, affecting equipment efficiency and lifespan, and increasing cleaning and maintenance costs.
Polydimethylsiloxane is used as the base material, and 3-methyltriethoxysilane is grafted to porous graphene to form 1H, 1H, 2H, 2H-perfluorooctyltriethoxy on its surface. A fluorinated protective layer of silane was used to imitate the hydrophobic structure of lotus leaves, and a bionic scaling-free material based on lotus leaves was prepared.
It achieves the self-cleaning effect of the material, significantly reduces the formation of scale, improves the hydrophobicity, mechanical strength and durability of the material, is suitable for use under high temperatures or harsh conditions, and extends the service life.
Smart Images

Figure CN117986877B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and particularly relates to a scaling-free material based on lotus leaf bionics and a preparation method thereof. Background Art
[0002] In the field of material science, such as water treatment systems, building materials and medical devices, scaling and contamination on the surface of materials not only affect the efficiency and life of the equipment, but also increase the cost of cleaning and maintenance. Bionic design provides a unique perspective and solution in this regard. By utilizing advanced nanofabrication technologies such as electron beam lithography, nanoimprinting and chemical etching, the micro-nanostructures of the lotus leaf surface can be replicated on polymer materials. These structures can effectively reduce the contact between water and other liquids and the surface of the material, thereby reducing the accumulation of pollutants.
[0003] In the field of materials science, the super-hydrophobic properties of lotus leaves have become a hot topic of research. This natural phenomenon has inspired the development of new anti-fouling materials that are not only fascinating in theory, but also have great potential in practical applications. The core of the lotus effect lies in two main factors: one is the special micro-nano structure of the lotus leaf surface, and the other is the chemical composition of its surface. These characteristics work together to form the super-hydrophobicity of the lotus leaf, even if water droplets hardly form a liquid film on its surface, but instead remain spherical and roll off easily, taking away dust and pollutants on the surface. Therefore, it is of great significance to develop a material that can effectively resist fouling and reduce scaling. Summary of the invention
[0004] Based on the above content, the present invention provides a scaling-free material based on lotus leaf bionics and a preparation method thereof. The present invention uses polydimethylsiloxane as the main material, grafts 3-methyltriethoxysilane, and then combines it with surface-activated porous graphene. In addition, by imitating the hydrophobic structure of lotus leaves, 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane is used to form a fluorinated protective layer on the surface of polydimethylsiloxane to prepare a scaling-free material based on lotus leaf bionics.
[0005] In order to solve the above technical problems, according to one aspect of the present invention, a scaling-free material based on lotus leaf bionics is provided, which is composed of polydimethylsiloxane, porous graphene and 1H,1H,2H,2H-perfluorooctyltriethoxysilane.
[0006] Another aspect of the present invention provides a method for preparing a scaling-free material based on lotus leaf bionics, comprising the following steps:
[0007] S1: Grafting reaction of polydimethylsiloxane;
[0008] S2: Surface activation of porous graphene;
[0009] S3: Combination of polydimethylsiloxane and open-pored graphene;
[0010] S4: mimics the hydrophobic structure of lotus leaves;
[0011] Preferably, the grafting reaction of polydimethylsiloxane in step S1 comprises the following steps:
[0012] A1: 3-methyltriethoxysilane was added to 10 times the volume of anhydrous ethanol, and the mixture was stirred at 300 rpm for 20 minutes to be uniformly dissolved to obtain a 3-methyltriethoxysilane solution. Polydimethylsiloxane was dissolved in 10 to 15 times the mass volume of anhydrous ethanol, and a 15 wt% HCl solution was added, and the mixture was stirred at 500 rpm for 10 minutes to obtain a polydimethylsiloxane solution. The 3-methyltriethoxysilane solution was slowly added dropwise to the polydimethylsiloxane solution within 10 minutes, heated in a constant temperature water bath at 50 to 60°C, stirred at 300 rpm for 30 minutes, reacted for 4 to 6 hours, cooled to room temperature, washed with anhydrous ethanol, and dried in a vacuum at 60°C to obtain a polydimethylsiloxane graft copolymer.
[0013] Preferably, in step A1, the ratio of the amount of polydimethylsiloxane to 3-methyltriethoxysilane is 1.5-2 g:1 mL; and the ratio of the amount of polydimethylsiloxane to HCl solution is 1 g:0.1-0.2 mL.
[0014] Preferably, the surface activation of the open-pored graphene in step S2 comprises the following steps:
[0015] B1: Grind graphite and screen through 300 mesh to obtain graphite powder; dissolve the graphite powder in concentrated sulfuric acid and control the temperature at 0°C in an ice bath; slowly add potassium permanganate within 5 minutes and control the temperature at 0-5°C in an ice bath; raise the temperature to 35°C and stir at 300rpm for 2-4h. After the reaction is completed, slowly add deionized water and finally add hydrogen peroxide solution and let stand for 15min; centrifuge at 5000rpm for 10min, wash the precipitate with deionized water, and dry at 80°C for 6h to obtain graphene oxide;
[0016] B2: Add the graphene oxide prepared in step B1 to deionized water, add sodium hydroxide to adjust the pH to 12, heat in a water bath to control the temperature to 90°C, treat at 150W for 10 minutes, and let it stand for 1 to 3 hours to obtain a reduced graphene oxide solution; dissolve silver nitrate in deionized water, add sodium borohydride, mix well, and obtain a mixed solution, add the mixed solution and polyvinyl pyrrolidone to the reduced graphene oxide solution, control the temperature to 120 to 150°C, perform ultrasonic treatment at 150W for 60 minutes, centrifuge to remove the supernatant, wash with deionized water, and dry at 80°C for 8 hours to obtain deposited graphene; thermally anneal the deposited graphene, rinse with nitric acid, then wash with deionized water, and vacuum dry at 50°C for 10 to 16 hours to obtain porous graphene;
[0017] B3: The porous graphene prepared in step B1 was uniformly dispersed in anhydrous ethanol, 15wt% HCl solution was added, and 3-methyltriethoxysilane solution was slowly added. The mixture was heated to 60-80°C under a nitrogen atmosphere, and stirred with a magnetic stirrer at 500rpm for 2-6h. After the reaction, the mixture was naturally cooled to room temperature, washed with anhydrous ethanol, centrifuged, and dried at 60°C for 12h to obtain activated porous graphene.
[0018] Preferably, in step B1, the ratio of the amount of graphite powder, concentrated sulfuric acid, potassium permanganate and hydrogen peroxide is 1g:20-23mL:2g:2mL, and the slowly adding of deionized water is to initially add deionized water with a volume of 2 times the concentrated sulfuric acid, and then continue to add deionized water with a volume of 4 times the concentrated sulfuric acid within 5 minutes.
[0019] Preferably, in step B2, the ratio of the graphene oxide to deionized water is 2-3 mg:1 mL; the ratio of the silver nitrate to deionized water is 1 g:40 mL; the ratio of the silver nitrate, sodium borohydride, polyvinyl pyrrolidone and reduced graphene oxide solution is 0.1 g:0.035-0.04 g:0.5 g:30 mL; the thermal annealing treatment is to gradually increase the temperature to 450-600 ° C at 10-15 ° C / min, continuously introduce argon at 1-10 mL / min, treat for 30-60 min, and naturally cool to room temperature.
[0020] Preferably, in step B3, the ratio of the amount of porous graphene, anhydrous ethanol, HCl solution and 3-methyltriethoxysilane is 1 g: 80-100 mL: 1-2 mL: 0.05-0.1 mL.
[0021] Preferably, the combination of polydimethylsiloxane and open-pored graphene in step S3 comprises the following steps:
[0022] C1: Add the activated porous graphene prepared in step B3 to anhydrous ethanol, stir with a magnetic stirrer at 500 rpm for 15 minutes, and then treat with 300W ultrasound for 30 to 60 minutes to obtain an activated porous graphene solution; disperse the polydimethylsiloxane graft copolymer prepared in step A1 in 15 times the mass volume of anhydrous ethanol to obtain a mixed solution; slowly add the activated porous graphene solution to the mixed solution within 10 minutes, stir with a magnetic stirrer at 500 rpm for 10 to 20 minutes, mix well, put into a vacuum degassing machine to remove bubbles, and vacuum dry at 20°C for 6 hours to obtain a polydimethylsiloxane composite.
[0023] Preferably, in step C1, the ratio of the activated porous graphene to anhydrous ethanol is 1 g: 60-80 mL; and the ratio of the activated porous graphene to the polydimethylsiloxane graft copolymer is 1: 1-1.5.
[0024] Preferably, the hydrophobic structure imitating lotus leaves in step S4 comprises the following steps:
[0025] D1: The polydimethylsiloxane complex prepared in step C1 is dissolved in 10 to 15 times the mass volume of anhydrous ethanol, subjected to ultrasonic treatment at 150W for 30 minutes, and mixed evenly to obtain a polydimethylsiloxane complex solution; 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane is dissolved in 10 to 20 times the mass volume of anhydrous ethanol to obtain a perfluorooctyltriethoxysilane solution; the polydimethylsiloxane complex solution is slowly added to the perfluorooctyltriethoxysilane solution for 10 minutes, stirred at a speed of 100 rpm, and Tween-80 is added at the same time; after stirring, the mixture is subjected to ultrasonic treatment at 200W for 20 to 30 minutes, and vacuum dried at 60 to 80°C for 8 hours to obtain a scale-free material.
[0026] Preferably, in step D1, the ratio of the polydimethylsiloxane complex to 1H,1H,2H,2H-perfluorooctyltriethoxysilane is 2-3:1; and the amount of Tween-80 is 0.1-0.5% of the total solution volume.
[0027] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0028] The core of the present invention is to use polydimethylsiloxane (PDMS) as a base material, combined with advanced surface modification and nanocomposite technology, to create a new material with excellent performance. First, the softness and elasticity of polydimethylsiloxane itself provide the material with basic physical deformation ability, which can withstand a certain degree of deformation without breaking. Then, by grafting 3-methyltriethoxysilane on the surface of polydimethylsiloxane and combining it with surface-activated porous graphene, the mechanical strength and stability of the material are further enhanced. As a reinforcing agent, porous graphene not only provides additional mechanical properties and heat resistance, but also increases the thermal stability of the material, so that the material can maintain structural and functional stability at higher temperatures and greater stresses. Finally, by forming a fluorinated protective layer of 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane on the surface of polydimethylsiloxane, the hydrophobicity of the material is greatly improved; this super hydrophobicity makes it difficult for water molecules to form stable contact on the surface of the material, thereby achieving a self-cleaning effect and effectively reducing the formation of scale.
[0029] The present invention utilizes the grafting of 3-methyltriethoxysilane and polydimethylsiloxane to help form a stable siloxane structure, enhance the chemical resistance and stability of polydimethylsiloxane, effectively improve the service life and anti-fouling performance of the material, and effectively improve the interface compatibility with porous graphene; HCl solution is used as a catalyst to promote the reaction in the grafting reaction, increase the crosslinking density, and effectively enhance the stability of polydimethylsiloxane. Graphene is a material composed of a single layer of carbon atoms, with a high surface area and special physical and chemical properties. Porous graphene can enhance the adsorption capacity and reaction activity of the material by introducing pores on the graphene layer, and helps to capture and decompose substances that cause scaling; 3-methyltriethoxysilane is used to perform surface activation treatment on porous graphene to enhance the surface activity of porous graphene, and effectively improve the combination of porous graphene and polydimethylsiloxane graft copolymer.
[0030] The present invention increases the microscopic roughness of the material surface by adding porous graphene, and combined with the hydrophobic properties of polydimethylsiloxane, it is more difficult for pollutants to accumulate on the material surface, effectively reducing scaling. The structural strength and heat resistance of porous graphene enhance the overall mechanical properties and durability of the material, making it more suitable for use under high temperature or other harsh conditions, which usually accelerate the formation of scale. Perfluorooctylsilane molecules contain long-chain perfluorocarbon groups, and this structure can greatly increase the hydrophobicity and oleophobicity of the material surface. When it is combined with polydimethylsiloxane and porous graphene, the hydrophobicity and oleophobicity of the entire composite material can be significantly improved, thereby making the material surface more difficult to be wetted by water and oily substances. Due to the chemical inertness of perfluorooctylsilane, the protective layer covering the surface of polydimethylsiloxane and porous graphene can improve the chemical stability of the entire material, making it more resistant to corrosion by acids, alkalis and other chemicals. The perfluorooctylsilane layer can effectively protect the underlying polydimethylsiloxane and porous graphene from environmental factors such as ultraviolet rays, effectively extending the service life of the material. In addition, perfluorooctylsilane forms a very thin protective layer, which is thin enough to ensure that it does not affect the physical properties of the material's internal structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a scaling test diagram of the samples of Examples 1 to 5 and Comparative Examples 1 to 3 prepared in the present invention in water containing calcium and magnesium ions.
[0032] Figure 2 The stable hydrophobicity test graphs of the samples prepared in Examples 1 to 5 and Comparative Examples 1 to 3 of the present invention are shown. DETAILED DESCRIPTION
[0033] In order to make the technical means, creative features, purpose and efficacy of the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments, but the following embodiments are only preferred embodiments of the present invention, not all. Based on the embodiments in the implementation mode, other embodiments obtained by those skilled in the art without creative work all belong to the protection scope of the present invention. The experimental methods in the following embodiments, unless otherwise specified, are conventional methods, and the materials, reagents, etc. used in the following embodiments, unless otherwise specified, can all be obtained from commercial channels.
[0034] Embodiment 1: A method for preparing a scaling-free material based on lotus leaf bionics, comprising the following steps:
[0035] S1: Grafting reaction of polydimethylsiloxane;
[0036] A1: Add 5 mL of 3-methyltriethoxysilane to 50 mL of anhydrous ethanol, stir at 300 rpm for 20 min to dissolve evenly, and obtain a 3-methyltriethoxysilane solution; dissolve 7.5 g of polydimethylsiloxane in 75 mL of anhydrous ethanol, and add 0.75 mL of 15 wt% HCl solution, stir at 500 rpm for 10 min to obtain a polydimethylsiloxane solution; slowly add the 3-methyltriethoxysilane solution dropwise to the polydimethylsiloxane solution within 10 min, heat at 50 ° C in a constant temperature water bath, stir at 300 rpm for 30 min, react for 4 h, cool to room temperature, wash with anhydrous ethanol, and vacuum dry at 60 ° C to obtain a polydimethylsiloxane graft copolymer.
[0037] S2: Surface activation of porous graphene;
[0038] B1: Grind graphite and sieve through 300 mesh to obtain graphite powder; dissolve 5g of graphite powder in 100mL of concentrated sulfuric acid and control the temperature at 0℃ in an ice bath; slowly add 10g of potassium permanganate within 5min and control the temperature at 5℃ in an ice bath; raise the temperature to 35℃ and stir at 300rpm for 2h. After the reaction, directly add 200mL of deionized water, then continue to add 400mL of deionized water within 5min, and finally add 10mL of hydrogen peroxide solution and let stand for 15min; centrifuge at 5000rpm for 10min, wash the precipitate with deionized water, and dry at 80℃ for 6h to obtain graphene oxide;
[0039] B2: 0.9 g of graphene oxide prepared in step B1 was added to 300 mL of deionized water, sodium hydroxide was added to adjust the pH to 12, the temperature was controlled at 90°C in a water bath, 150 W was used for 10 min, and the reaction was allowed to stand for 1 h to obtain a reduced graphene oxide solution; 1 g of silver nitrate was dissolved in 40 mL of deionized water, and 0.35 g of sodium borohydride was added. After mixing evenly, a mixed solution was obtained, and the mixed solution and 5 g of polyvinyl pyrrolidone were added to 300 mL of the reduced graphene oxide solution, the temperature was controlled at 120°C, and 150 W was used for ultrasonic treatment for 60 min. The supernatant was removed by centrifugation, the solution was washed with deionized water, and the solution was dried at 80°C for 8 h to obtain deposited graphene; the deposited graphene was subjected to thermal annealing treatment, the temperature was gradually increased to 450°C at 10°C / min, argon was continuously introduced at 1 mL / min, the solution was treated for 30 min, and the solution was naturally cooled to room temperature; the solution was rinsed with nitric acid, then washed with deionized water, and vacuum dried at 50°C for 10 h to obtain porous graphene;
[0040] B3: 0.8 g of porous graphene prepared in step B1 was uniformly dispersed in 64 mL of anhydrous ethanol, 0.8 mL of 15 wt% HCl solution was added, and 0.04 mL of 3-methyltriethoxysilane solution was slowly added. The temperature was heated to 60 ° C under a nitrogen atmosphere of 1 mL / min, and the reaction was stirred at 500 rpm with a magnetic stirrer for 2 h. After the reaction was completed, it was naturally cooled to room temperature, washed with anhydrous ethanol, centrifuged, and dried at 60 ° C for 12 h to obtain activated porous graphene.
[0041] S3: Combination of polydimethylsiloxane and open-pored graphene;
[0042] C1: 0.8 g of the activated porous graphene prepared in step B3 was added to 48 mL of anhydrous ethanol, stirred with a magnetic stirrer at 500 rpm for 15 min, and then ultrasonically treated at 300 W for 30 min to obtain an activated porous graphene solution; 0.53 g of the polydimethylsiloxane graft copolymer prepared in step A1 was dispersed in 8 mL of anhydrous ethanol to obtain a mixed solution; the activated porous graphene solution was slowly added to the mixed solution within 10 min, stirred with a magnetic stirrer at 500 rpm for 10 min, and after mixing evenly, the mixture was placed in a vacuum degassing machine to remove bubbles, and vacuum dried at 20° C. for 6 h to obtain a polydimethylsiloxane composite.
[0043] S4: mimics the hydrophobic structure of lotus leaves;
[0044] D1: Dissolve 0.8 g of the polydimethylsiloxane complex prepared in step C1 in 8 mL of anhydrous ethanol, perform ultrasonic treatment at 150 W for 30 min, mix well, and obtain a polydimethylsiloxane complex solution; dissolve 0.27 g of 1H,1H,2H,2H-perfluorooctyltriethoxysilane in 2.7 mL of anhydrous ethanol to obtain a perfluorooctyltriethoxysilane solution; slowly add the polydimethylsiloxane complex solution to the perfluorooctyltriethoxysilane solution for 10 min, stir at 100 rpm, and add 0.01 mL of Tween-80 at the same time; after stirring, perform ultrasonic treatment at 200 W for 20 min, and vacuum dry at 60°C for 8 h to obtain a scale-free material.
[0045] Embodiment 2: A method for preparing a scaling-free material based on lotus leaf bionics, comprising the following steps:
[0046] S1: Grafting reaction of polydimethylsiloxane;
[0047] A1: Add 10 mL of 3-methyltriethoxysilane to 100 mL of anhydrous ethanol, stir at 300 rpm for 20 min to dissolve evenly, and obtain a 3-methyltriethoxysilane solution; dissolve 15 g of polydimethylsiloxane in 180 mL of anhydrous ethanol, add 2 mL of 15 wt% HCl solution, and stir at 500 rpm for 10 min to obtain a polydimethylsiloxane solution; slowly add the 3-methyltriethoxysilane solution dropwise to the polydimethylsiloxane solution within 10 min, heat at 52 ° C in a constant temperature water bath, stir at 300 rpm for 30 min, react for 4 h, cool to room temperature, wash with anhydrous ethanol, and vacuum dry at 60 ° C to obtain a polydimethylsiloxane graft copolymer.
[0048] S2: Surface activation of porous graphene;
[0049] B1: Grind graphite and screen it through 300 mesh to obtain graphite powder; dissolve 5g of graphite powder in 105mL of concentrated sulfuric acid and control the temperature at 0℃ in an ice bath; slowly add 10g of potassium permanganate within 5min and control the temperature at 4℃ in an ice bath; raise the temperature to 35℃ and stir at 300rpm for 2.5h. After the reaction is completed, directly add 210mL of deionized water, then continue to add 420mL of deionized water within 5min, and finally add 10mL of hydrogen peroxide solution and let it stand for 15min; centrifuge at 5000rpm for 10min, wash the precipitate with deionized water, and dry at 80℃ for 6h to obtain graphene oxide;
[0050] B2: Add 2g of graphene oxide prepared in step B1 to 600mL of deionized water, add sodium hydroxide to adjust the pH to 12, heat in a water bath to control the temperature to 90°C, treat at 150W for 10min, and let it stand for 1.5h to obtain a reduced graphene oxide solution; dissolve 1g of silver nitrate in 40mL of deionized water, add 0.35g of sodium borohydride, mix well, and obtain a mixed solution, add the mixed solution and 5g of polyvinyl pyrrolidone to 300mL of the reduced graphene oxide solution, control the temperature to 130°C, ultrasonically treat at 150W for 60min, centrifuge to remove the supernatant, wash with deionized water, and dry at 80°C for 8h to obtain deposited graphene; thermally anneal the deposited graphene, gradually heat to 450°C at 11°C / min, continuously introduce argon at 2mL / min, treat for 40min, and naturally cool to room temperature; rinse with nitric acid, then wash with deionized water, and vacuum dry at 50°C for 12h to obtain porous graphene;
[0051] B3: Disperse 1 g of porous graphene prepared in step B1 evenly in 85 mL of anhydrous ethanol, add 1.2 mL of 15 wt% HCl solution, slowly add 0.06 mL of 3-methyltriethoxysilane solution, heat to 65 °C under 1 mL / min nitrogen atmosphere, stir with a magnetic stirrer at 500 rpm for 3 h, cool naturally to room temperature after the reaction, wash with anhydrous ethanol, centrifuge, and dry at 60 °C for 12 h to obtain activated porous graphene.
[0052] S3: Combination of polydimethylsiloxane and open-pored graphene;
[0053] C1: Add 1 g of the activated porous graphene prepared in step B3 to 65 mL of anhydrous ethanol, stir with a magnetic stirrer at 500 rpm for 15 min, and then treat with 300 W ultrasound for 35 min to obtain an activated porous graphene solution; disperse 0.7 g of the polydimethylsiloxane graft copolymer prepared in step A1 in 10.5 mL of anhydrous ethanol to obtain a mixed solution; slowly add the activated porous graphene solution to the mixed solution within 10 min, stir with a magnetic stirrer at 500 rpm for 12 min, mix well, put into a vacuum degasser to remove bubbles, and vacuum dry at 20°C for 6 h to obtain a polydimethylsiloxane complex.
[0054] S4: mimics the hydrophobic structure of lotus leaves;
[0055] D1: Dissolve 1 g of the polydimethylsiloxane complex prepared in step C1 in 12 mL of anhydrous ethanol, perform ultrasonic treatment at 150 W for 30 min, mix well, and obtain a polydimethylsiloxane complex solution; dissolve 0.35 g of 1H,1H,2H,2H-perfluorooctyltriethoxysilane in 4.2 mL of anhydrous ethanol to obtain a perfluorooctyltriethoxysilane solution; slowly add the polydimethylsiloxane complex solution to the perfluorooctyltriethoxysilane solution for 10 min, stir at 100 rpm, and add 0.03 mL of Tween-80 at the same time; after stirring, perform ultrasonic treatment at 200 W for 22 min, and vacuum dry at 65 ° C for 8 h to obtain a scale-free material.
[0056] Embodiment 3: A method for preparing a scaling-free material based on lotus leaf bionics, comprising the following steps:
[0057] S1: Grafting reaction of polydimethylsiloxane;
[0058] A1: Add 10 mL of 3-methyltriethoxysilane to 10 mL of anhydrous ethanol, stir at 300 rpm for 20 min to dissolve evenly, and obtain a 3-methyltriethoxysilane solution; dissolve 16 g of polydimethylsiloxane in 210 mL of anhydrous ethanol, add 2 mL of 15 wt% HCl solution, and stir at 500 rpm for 10 min to obtain a polydimethylsiloxane solution; slowly add the 3-methyltriethoxysilane solution dropwise to the polydimethylsiloxane solution within 10 min, heat at 55 ° C in a constant temperature water bath, stir at 300 rpm for 30 min, react for 5 h, cool to room temperature, wash with anhydrous ethanol, and vacuum dry at 60 ° C to obtain a polydimethylsiloxane graft copolymer.
[0059] S2: Surface activation of porous graphene;
[0060] B1: Grind graphite and sieve through 300 mesh to obtain graphite powder; dissolve 5g of graphite powder in 110mL of concentrated sulfuric acid and control the temperature at 0℃ in an ice bath; slowly add 10g of potassium permanganate within 5min and control the temperature at 3℃ in an ice bath; raise the temperature to 35℃ and stir at 300rpm for 3h. After the reaction, directly add 220mL of deionized water, then continue to add 440mL of deionized water within 5min, and finally add 10mL of hydrogen peroxide solution and let stand for 15min; centrifuge at 5000rpm for 10min, wash the precipitate with deionized water, and dry at 80℃ for 6h to obtain graphene oxide;
[0061] B2: Add 2g of graphene oxide prepared in step B1 to 700mL of deionized water, add sodium hydroxide to adjust the pH to 12, heat in a water bath to control the temperature to 90°C, treat at 150W for 10min, and let it stand for 2h to obtain a reduced graphene oxide solution; dissolve 1g of silver nitrate in 40mL of deionized water, add 0.35g of sodium borohydride, mix well, and obtain a mixed solution, add the mixed solution and 5g of polyvinyl pyrrolidone to 300mL of the reduced graphene oxide solution, control the temperature to 135°C, perform ultrasonic treatment at 150W for 60min, centrifuge to remove the supernatant, wash with deionized water, and dry at 80°C for 8h to obtain deposited graphene; perform thermal annealing on the deposited graphene, gradually heat to 530°C at 12°C / min, continuously introduce argon at 5mL / min, treat for 45min, and naturally cool to room temperature; rinse with nitric acid, then wash with deionized water, and vacuum dry at 50°C for 14h to obtain porous graphene;
[0062] B3: Disperse 1 g of porous graphene prepared in step B1 evenly in 90 mL of anhydrous ethanol, add 1.5 mL of 15 wt% HCl solution, slowly add 0.08 mL of 3-methyltriethoxysilane solution, heat to 70 °C under nitrogen atmosphere, stir with a magnetic stirrer at 500 rpm for 4 h, cool naturally to room temperature after the reaction, wash with anhydrous ethanol, centrifuge, and dry at 60 °C for 12 h to obtain activated porous graphene.
[0063] S3: Combination of polydimethylsiloxane and open-pored graphene;
[0064] C1: Add 1 g of the activated porous graphene prepared in step B3 to 70 mL of anhydrous ethanol, stir with a magnetic stirrer at 500 rpm for 15 min, and then treat with 300 W ultrasound for 45 min to obtain an activated porous graphene solution; disperse 0.8 g of the polydimethylsiloxane graft copolymer prepared in step A1 in 12 mL of anhydrous ethanol to obtain a mixed solution; slowly add the activated porous graphene solution to the mixed solution within 10 min, stir with a magnetic stirrer at 500 rpm for 15 min, mix well, put into a vacuum degasser to remove bubbles, and vacuum dry at 20° C. for 6 h to obtain a polydimethylsiloxane composite.
[0065] S4: mimics the hydrophobic structure of lotus leaves;
[0066] D1: Dissolve 1 g of the polydimethylsiloxane complex prepared in step C1 in 13 mL of anhydrous ethanol, perform ultrasonic treatment at 150 W for 30 min, mix well, and obtain a polydimethylsiloxane complex solution; dissolve 0.45 g of 1H,1H,2H,2H-perfluorooctyltriethoxysilane in 6.75 mL of anhydrous ethanol to obtain a perfluorooctyltriethoxysilane solution; slowly add the polydimethylsiloxane complex solution to the perfluorooctyltriethoxysilane solution for 10 min and stir at 100 rpm, and simultaneously add 0.06 mL of Tween-80; after stirring, perform ultrasonic treatment at 200 W for 25 min, and vacuum dry at 70°C for 8 h to obtain a scale-free material.
[0067] Embodiment 4: A method for preparing a scaling-free material based on lotus leaf bionics, comprising the following steps:
[0068] S1: Grafting reaction of polydimethylsiloxane;
[0069] A1: 10 mL of 3-methyltriethoxysilane was added to 100 mL of anhydrous ethanol, and the mixture was stirred at 300 rpm for 20 min to be uniformly dissolved to obtain a 3-methyltriethoxysilane solution. 18 g of polydimethylsiloxane was dissolved in 270 mL of anhydrous ethanol, and 3 mL of a 15 wt% HCl solution was added, and the mixture was stirred at 500 rpm for 10 min to obtain a polydimethylsiloxane solution. The 3-methyltriethoxysilane solution was slowly added dropwise to the polydimethylsiloxane solution within 10 min, heated in a constant temperature water bath at 58 ° C, stirred at 300 rpm for 30 min, reacted for 5.5 h, cooled to room temperature, washed with anhydrous ethanol, and vacuum dried at 60 ° C to obtain a polydimethylsiloxane graft copolymer.
[0070] S2: Surface activation of porous graphene;
[0071] B1: Grind graphite and screen it through 300 mesh to obtain graphite powder; dissolve 5g of graphite powder in 115mL of concentrated sulfuric acid and control the temperature at 0℃ in an ice bath; slowly add 10g of potassium permanganate within 5min and control the temperature at 0℃ in an ice bath; raise the temperature to 35℃ and stir at 300rpm for 3.5h. After the reaction is completed, directly add 230mL of deionized water, then continue to add 460mL of deionized water within 5min, and finally add 10mL of hydrogen peroxide solution, let it stand for 15min; centrifuge at 5000rpm for 10min, wash the precipitate with deionized water, and dry at 80℃ for 6h to obtain graphene oxide;
[0072] B2: Add 2g of graphene oxide prepared in step B1 to 800mL of deionized water, add sodium hydroxide to adjust the pH to 12, heat in a water bath to control the temperature to 90°C, treat at 150W for 10min, and let it stand for 2.5h to obtain a reduced graphene oxide solution; dissolve 1g of silver nitrate in 40mL of deionized water, add 0.35g of sodium borohydride, mix well, and obtain a mixed solution, add the mixed solution and 5g of polyvinyl pyrrolidone to 300mL of the reduced graphene oxide solution, control the temperature to 145°C, ultrasonically treat at 150W for 60min, centrifuge to remove the supernatant, wash with deionized water, and dry at 80°C for 8h to obtain deposited graphene; thermally anneal the deposited graphene, gradually heat to 580°C at 14°C / min, continuously introduce argon at 8mL / min, treat for 55min, and naturally cool to room temperature; rinse with nitric acid, then wash with deionized water, and vacuum dry at 50°C for 15h to obtain porous graphene;
[0073] B3: Disperse 1 g of porous graphene prepared in step B1 evenly in 95 mL of anhydrous ethanol, add 1.8 mL of 15 wt% HCl solution, slowly add 0.09 mL of 3-methyltriethoxysilane solution, heat to 75 °C under nitrogen atmosphere, stir with a magnetic stirrer at 500 rpm for 5 h, cool naturally to room temperature after the reaction, wash with anhydrous ethanol, centrifuge, and dry at 60 °C for 12 h to obtain activated porous graphene.
[0074] S3: Combination of polydimethylsiloxane and open-pored graphene;
[0075] C1: Add 1 g of the activated porous graphene prepared in step B3 to 75 mL of anhydrous ethanol, stir with a magnetic stirrer at 500 rpm for 15 min, and then treat with 300 W ultrasound for 55 min to obtain an activated porous graphene solution; disperse 0.9 g of the polydimethylsiloxane graft copolymer prepared in step A1 in 13.5 mL of anhydrous ethanol to obtain a mixed solution; slowly add the activated porous graphene solution to the mixed solution within 10 min, stir with a magnetic stirrer at 500 rpm for 18 min, mix well, put into a vacuum degasser to remove bubbles, and vacuum dry at 20°C for 6 h to obtain a polydimethylsiloxane composite.
[0076] S4: mimics the hydrophobic structure of lotus leaves;
[0077] D1: Dissolve 1 g of the polydimethylsiloxane complex prepared in step C1 in 14 mL of anhydrous ethanol, perform ultrasonic treatment at 150 W for 30 min, mix well, and obtain a polydimethylsiloxane complex solution; dissolve 0.5 g of 1H,1H,2H,2H-perfluorooctyltriethoxysilane in 9 mL of anhydrous ethanol to obtain a perfluorooctyltriethoxysilane solution; slowly add the polydimethylsiloxane complex solution to the perfluorooctyltriethoxysilane solution for 10 min, stir at 100 rpm, and add 0.1 mL of Tween-80 at the same time; after stirring, perform ultrasonic treatment at 200 W for 28 min, and vacuum dry at 75 ° C for 8 h to obtain a scale-free material.
[0078] Embodiment 5: A method for preparing a scaling-free material based on lotus leaf bionics, comprising the following steps:
[0079] S1: Grafting reaction of polydimethylsiloxane;
[0080] A1: 10 mL of 3-methyltriethoxysilane was added to 100 mL of anhydrous ethanol, and the mixture was stirred at 300 rpm for 20 min to be uniformly dissolved to obtain a 3-methyltriethoxysilane solution. 20 g of polydimethylsiloxane was dissolved in 300 mL of anhydrous ethanol, and 4 mL of a 15 wt% HCl solution was added, and the mixture was stirred at 500 rpm for 10 min to obtain a polydimethylsiloxane solution. The 3-methyltriethoxysilane solution was slowly added dropwise to the polydimethylsiloxane solution within 10 min, heated in a constant temperature water bath at 60°C, stirred at 300 rpm for 30 min, reacted for 6 h, cooled to room temperature, washed with anhydrous ethanol, and dried in a vacuum at 60°C to obtain a polydimethylsiloxane graft copolymer.
[0081] S2: Surface activation of porous graphene;
[0082] B1: Grind graphite and sieve it through 300 mesh to obtain graphite powder; dissolve 5g of graphite powder in 115mL of concentrated sulfuric acid and control the temperature at 0℃ in an ice bath; slowly add 10g of potassium permanganate within 5min and control the temperature at 0℃ in an ice bath; raise the temperature to 35℃ and stir at 300rpm for 4h. After the reaction, directly add 230mL of deionized water, then continue to add 460mL of deionized water within 5min, and finally add 10mL of hydrogen peroxide solution and let it stand for 15min; centrifuge at 5000rpm for 10min, wash the precipitate with deionized water, and dry at 80℃ for 6h to obtain graphene oxide;
[0083] B2: Add 2g of graphene oxide prepared in step B1 to 1000mL of deionized water, add sodium hydroxide to adjust the pH to 12, heat in a water bath to control the temperature to 90°C, treat at 150W for 10min, and let it stand for 3h to react to obtain a reduced graphene oxide solution; dissolve 1g of silver nitrate in 40mL of deionized water, add 0.35g of sodium borohydride, mix well to obtain a mixed solution, add the mixed solution and 5g of polyvinyl pyrrolidone to 300mL of the reduced graphene oxide solution, control the temperature to 150°C, ultrasonically treat at 150W for 60min, centrifuge to remove the supernatant, wash with deionized water, and dry at 80°C for 8h to obtain deposited graphene; thermally anneal the deposited graphene, gradually heat to 600°C at 15°C / min, continuously introduce argon at 10mL / min, treat for 60min, and naturally cool to room temperature; rinse with nitric acid, then wash with deionized water, and vacuum dry at 50°C for 16h to obtain porous graphene;
[0084] B3: Disperse 1 g of porous graphene prepared in step B1 uniformly in 100 mL of anhydrous ethanol, add 2 mL of 15 wt% HCl solution, slowly add 0.1 mL of 3-methyltriethoxysilane solution, heat to 80 °C under a 1 mL / min nitrogen atmosphere, stir with a magnetic stirrer at 500 rpm for 6 h, cool naturally to room temperature after the reaction, wash with anhydrous ethanol, centrifuge, and dry at 60 °C for 12 h to obtain activated porous graphene.
[0085] S3: Combination of polydimethylsiloxane and open-pored graphene;
[0086] C1: Add 1 g of the activated porous graphene prepared in step B3 to 80 mL of anhydrous ethanol, stir with a magnetic stirrer at 500 rpm for 15 min, and then treat with 300 W ultrasound for 60 min to obtain an activated porous graphene solution; disperse 1 g of the polydimethylsiloxane graft copolymer prepared in step A1 in 15 mL of anhydrous ethanol to obtain a mixed solution; slowly add the activated porous graphene solution to the mixed solution within 10 min, stir with a magnetic stirrer at 500 rpm for 20 min, mix well, put into a vacuum degassing machine to remove bubbles, and vacuum dry at 20°C for 6 h to obtain a polydimethylsiloxane composite.
[0087] S4: mimics the hydrophobic structure of lotus leaves;
[0088] D1: Dissolve 1 g of the polydimethylsiloxane complex prepared in step C1 in 15 mL of anhydrous ethanol, perform ultrasonic treatment at 150 W for 30 min, mix well, and obtain a polydimethylsiloxane complex solution; dissolve 0.5 g of 1H,1H,2H,2H-perfluorooctyltriethoxysilane in 10 mL of anhydrous ethanol to obtain a perfluorooctyltriethoxysilane solution; slowly add the polydimethylsiloxane complex solution to the perfluorooctyltriethoxysilane solution for 10 min, stir at 100 rpm, and add 0.125 mL of Tween-80 at the same time; after stirring, perform ultrasonic treatment at 200 W for 30 min, and vacuum dry at 80°C for 8 h to obtain a scale-free material.
[0089] Comparative Example 1: is basically the same as Example 2, except that Comparative Example 1 does not incorporate porous graphene.
[0090] Comparative Example 2 is basically the same as Example 3, except that the thin layer formed by 1H,1H,2H,2H-perfluorooctyltriethoxysilane is not used in Comparative Example 2.
[0091] Comparative Example 3: A scale-free material prepared by grafting polydimethylsiloxane with 3-methyltriethoxysilane.
[0092] Performance Test:
[0093] Hydrophobicity test: The scale-free materials prepared in the above Examples 1 to 5 and Comparative Examples 1 to 3 were subjected to contact angle tests. The larger the contact angle, the better the hydrophobic effect. A contact angle greater than 140° was recorded as A, a contact angle between 130 and 140° was recorded as B, and a contact angle less than 130° was recorded as C. All samples were tested at room temperature and 50% humidity. A 5 μl water droplet was used for each test. To ensure data reliability, 5 contact angle measurements were performed for each sample, and the average value was taken as the final result. The test results are shown in Table 1.
[0094] Hydrophobic stability test: The test steps are basically the same as above. The test conditions are divided into three types. The first is tested at a high temperature of 85°C and a humidity of 50%; the second is tested at a humidity of 85% and room temperature; the third is tested at room temperature, a humidity of 50%, and an ultraviolet irradiation UV intensity of 0.5W / m²; the test time is 72h. The test results are shown in Table 1.
[0095] Table 1. Hydrophobicity and stability test results.
[0096]
[0097] It can be seen from the results in Table 1 that the scale-free material prepared by the present invention has good hydrophobicity, and can show excellent stable hydrophobicity under high temperature, high humidity and ultraviolet irradiation; the protective layer formed by 1H,1H,2H,2H-perfluorooctyltriethoxysilane can effectively improve the stability of the scale-free material under high temperature, high humidity and ultraviolet irradiation conditions. In addition, the synergistic effect of 1H,1H,2H,2H-perfluorooctyltriethoxysilane and porous graphene effectively improves the hydrophobicity of the scale-free material.
[0098] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
Claims
1. A method for preparing a scaling-free material based on lotus leaf bionics, characterized in that: The anti-fouling material based on lotus leaf biomimetic is composed of polydimethylsiloxane, porous graphene, 1H,1H,2H,2H-perfluorooctyltriethoxysilane and 3-methyltriethoxysilane; The preparation method of the anti-fouling material based on lotus leaf bionics comprises the following steps: S1: Grafting reaction of polydimethylsiloxane; S2: Surface activation of porous graphene; S3: Combination of polydimethylsiloxane and porous graphene; S4: mimics the hydrophobic structure of lotus leaves; The grafting reaction of polydimethylsiloxane in step S1 comprises the following steps: A1: 3-methyltriethoxysilane was added to 10 times the volume of anhydrous ethanol, and stirred at 300 rpm for 20 minutes to dissolve evenly to obtain a 3-methyltriethoxysilane solution; polydimethylsiloxane was dissolved in 10 to 15 times the mass volume of anhydrous ethanol, and a 15wt% HCl solution was added, and stirred at 500 rpm for 10 minutes to obtain a polydimethylsiloxane solution; the 3-methyltriethoxysilane solution was slowly added dropwise to the polydimethylsiloxane solution within 10 minutes, heated in a constant temperature water bath at 50 to 60°C, stirred at 300 rpm for 30 minutes, reacted for 4 to 6 hours, cooled to room temperature, washed with anhydrous ethanol, and vacuum dried at 60°C to obtain a polydimethylsiloxane graft copolymer; The surface activation of the porous graphene in step S2 comprises the following steps: B1: Grind graphite and screen through 300 mesh to obtain graphite powder; dissolve the graphite powder in concentrated sulfuric acid and control the temperature at 0°C in an ice bath; slowly add potassium permanganate within 5 minutes and control the temperature at 0-5°C in an ice bath; raise the temperature to 35°C and stir at 300rpm for 2-4h. After the reaction is completed, slowly add deionized water and finally add hydrogen peroxide solution and let stand for 15min; centrifuge at 5000rpm for 10min, wash the precipitate with deionized water, and dry at 80°C for 6h to obtain graphene oxide; B2: Add the graphene oxide prepared in step B1 to deionized water, add sodium hydroxide to adjust the pH to 12, heat in a water bath to control the temperature to 90°C, treat at 150W for 10 minutes, and let it stand for 1 to 3 hours to obtain a reduced graphene oxide solution; dissolve silver nitrate in deionized water, add sodium borohydride, mix well, and obtain a mixed solution, add the mixed solution and polyvinyl pyrrolidone to the reduced graphene oxide solution, control the temperature to 120 to 150°C, perform ultrasonic treatment at 150W for 60 minutes, centrifuge to remove the supernatant, wash with deionized water, and dry at 80°C for 8 hours to obtain deposited graphene; thermally anneal the deposited graphene, rinse with nitric acid, then wash with deionized water, and vacuum dry at 50°C for 10 to 16 hours to obtain porous graphene; B3: The porous graphene prepared in step B1 was uniformly dispersed in anhydrous ethanol, 15wt% HCl solution was added, 3-methyltriethoxysilane solution was slowly added, the temperature was heated to 60-80°C under a nitrogen atmosphere, and a magnetic stirrer was stirred at 500rpm for 2-6h. After the reaction was completed, it was naturally cooled to room temperature, washed with anhydrous ethanol, centrifuged, and dried at 60°C for 12h to obtain activated porous graphene; The hydrophobic structure imitating lotus leaf in step S4 comprises the following steps: D1: The polydimethylsiloxane complex prepared in step C1 is dissolved in 10 to 15 times the mass volume of anhydrous ethanol, subjected to ultrasonic treatment at 150W for 30 minutes, and mixed evenly to obtain a polydimethylsiloxane complex solution; 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane is dissolved in 10 to 20 times the mass volume of anhydrous ethanol to obtain a perfluorooctyltriethoxysilane solution; the polydimethylsiloxane complex solution is slowly added to the perfluorooctyltriethoxysilane solution for 10 minutes, stirred at a speed of 100 rpm, and Tween-80 is added at the same time; after stirring, the mixture is subjected to ultrasonic treatment at 200W for 20 to 30 minutes, and vacuum dried at 60 to 80°C for 8 hours to obtain a scale-free material.
2. The method for preparing a scaling-free material based on lotus leaf bionics according to claim 1, characterized in that: In step A1, the ratio of the amount of polydimethylsiloxane to 3-methyltriethoxysilane is 1.5-2 g:1 mL; the ratio of the amount of polydimethylsiloxane to HCl solution is 1 g:0.1-0.2 mL.
3. The method for preparing a scaling-free material based on lotus leaf bionics according to claim 2, characterized in that: The ratio of the amount of graphite powder, concentrated sulfuric acid, potassium permanganate and hydrogen peroxide used in step B1 is 1g:20-23mL:2g:2mL, and the deionized water is slowly added by initially adding deionized water with a volume of 2 times the concentrated sulfuric acid, and then continuously adding deionized water with a volume of 4 times the concentrated sulfuric acid within 5 minutes.
4. The method for preparing a scaling-free material based on lotus leaf bionics according to claim 3, characterized in that: In step B2, the ratio of graphene oxide to deionized water is 2-3 mg: 1 mL; the ratio of silver nitrate to deionized water is 1 g: 40 mL; the ratio of silver nitrate, sodium borohydride, polyvinyl pyrrolidone and reduced graphene oxide solution is 0.1 g: 0.035-0.04 g: 0.5 g: 30 mL; the thermal annealing treatment is to gradually increase the temperature to 450-600 ° C at 10-15 ° C / min, continuously introduce argon at 1-10 mL / min, treat for 30-60 min, and naturally cool to room temperature.
5. The method for preparing a scaling-free material based on lotus leaf bionics according to claim 4, characterized in that: The ratio of the amount of porous graphene, anhydrous ethanol, HCl solution and 3-methyltriethoxysilane used in step B3 is 1g:80-100mL:1-2mL:0.05-0.1mL.
6. The method for preparing a scaling-free material based on lotus leaf bionics according to claim 5, characterized in that: The combination of polydimethylsiloxane and porous graphene in step S3 comprises the following steps: C1: Add the activated porous graphene prepared in step B3 to anhydrous ethanol, stir with a magnetic stirrer at 500 rpm for 15 minutes, and then treat with 300W ultrasound for 30 to 60 minutes to obtain an activated porous graphene solution; disperse the polydimethylsiloxane graft copolymer prepared in step A1 in 15 times the mass volume of anhydrous ethanol to obtain a mixed solution; slowly add the activated porous graphene solution to the mixed solution within 10 minutes, stir with a magnetic stirrer at 500 rpm for 10 to 20 minutes, mix well, put into a vacuum degassing machine to remove bubbles, and vacuum dry at 20°C for 6 hours to obtain a polydimethylsiloxane composite.
7. The method for preparing a scaling-free material based on lotus leaf bionics according to claim 6, characterized in that: In step C1, the ratio of the amount of the activated porous graphene to anhydrous ethanol is 1 g: 60-80 mL; the ratio of the amount of the activated porous graphene to the polydimethylsiloxane graft copolymer is 1: 1-1.
5.
8. The method for preparing a scaling-free material based on lotus leaf bionics according to claim 7, characterized in that: In step D1, the ratio of the polydimethylsiloxane complex to 1H,1H,2H,2H-perfluorooctyltriethoxysilane is 2-3:1; and the amount of Tween-80 is 0.1-0.5% of the total solution volume.
Citation Information
Patent Citations
Superhydrophobic composite coating with self-repair function and preparation method thereof
CN105038439A
Method for composite preparation of high-conductivity and high electromagnetic shielding flexible composite materials through adoption of graphene sponge and polydimethylsiloxane