A high-performance polyamide reverse osmosis membrane mediated by ordered stacking of three-dimensional nanohelices and a preparation method thereof

Mediated by the orderly stacking layers of three-dimensional nanospiral materials, sub-nanometer channels are formed, combining the ravine effect and the resistance series effect to solve the problem of the existing polyamide reverse osmosis membrane's poor removal effect of neutral small molecule pollutants. Significantly improved water permeability and retention capacity.

CN118001945BActive Publication Date: 2024-10-01TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410153293.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-04
Publication Date
2024-10-01
Estimated Expiration
2044-02-04

AI Technical Summary

Technical Problem

The existing polyamide reverse osmosis membrane has poor removal effect on neutral small molecule pollutants, and its water permeability and salt/neutral small molecule selectivity are limited, which affects its performance in water treatment.

Method used

Three-dimensional nano-spiral materials are used to form an intermediate layer through orderly stacking to form a sub-nanometer channel, which combines the gully effect and the resistance series effect to enhance the water permeability and neutral small molecule pollutant interception ability of the reverse osmosis membrane.

Benefits of technology

It significantly improves the water permeability and neutral small molecule pollutant interception capacity of the reverse osmosis membrane, optimizes the water molecule transmission path, and enhances the interception effect of salt and neutral small molecule pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118001945B_ABST
    Figure CN118001945B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-performance polyamide reverse osmosis membrane mediated by a three-dimensional nano-helix ordered stacking layer and a preparation method thereof, and belongs to the field of membrane separation technology. First, a three-dimensional nano-helix is ​​prepared and a dispersion of the three-dimensional nano-helix is ​​prepared, which is dispersed on the surface of a base membrane, and then the base membrane with the three-dimensional nano-helix ordered stacking layer on the surface is infiltrated with an m-phenylenediamine / water solution, and then the surface of the base membrane is covered with n-hexane containing trimesoyl chloride, and an interfacial polymerization reaction based on the three-dimensional nano-helix ordered stacking layer occurs, and a three-dimensional nano-helix ordered stacking layer is introduced between the base membrane and the polyamide layer. In the preparation method, the three-dimensional nano-helix material is easy to prepare, and the prepared high-performance polyamide reverse osmosis membrane mediated by the three-dimensional nano-helix ordered stacking layer maintains excellent interception of salt and nitrosamine pollutants without losing the membrane water permeability. The method of the present invention does not need to change the overall membrane preparation process during the amplification process, and is easy to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of membrane separation, and in particular relates to a high-performance polyamide reverse osmosis membrane mediated by a three-dimensional nano-helical ordered stacking layer and a preparation method thereof. Background Art

[0002] Reverse osmosis membrane is an important technology for achieving water pollution control and water resource regeneration, and is widely used in the fields of deep sewage treatment, seawater desalination, etc. At present, commercial polyamide reverse osmosis membranes have poor removal effects on neutral small molecule pollutants, and their performance is restricted by the upper limit of water permeability-salt / neutral small molecule pollutant selectivity. It is urgent to prepare high-performance reverse osmosis membranes through innovative preparation methods, and simultaneously enhance the removal efficiency of neutral small molecule pollutants and water permeability of reverse osmosis membranes, thereby improving the water treatment efficiency of reverse osmosis membranes.

[0003] The reverse osmosis membrane is mainly composed of three layers: a polyamide layer, a polysulfone porous base membrane, and a non-woven fabric, among which the polyamide layer plays the main separation role. Recently, some studies have shown that the influence of the porous base membrane characteristics on the overall separation performance of the reverse osmosis membrane cannot be ignored. The porous base membrane has non-porous and porous areas. Water molecules are difficult to penetrate in the non-porous areas of the base membrane. When water molecules pass through the polyamide layer, they must diffuse to the porous areas of the base membrane for transportation, which extends the water molecule transportation path (i.e., the funnel effect). By introducing a relatively loose intermediate layer between the base membrane and the polyamide layer, it is beneficial to optimize the water molecule transmission channel between the polyamide layer and the porous base membrane, and improve the water permeability of the reverse osmosis membrane (i.e., the gully effect). At the same time, if the intermediate layer has a certain interception efficiency for the target pollutant, the interception effect of the reverse osmosis membrane on the pollutant can be enhanced through the resistance series effect. Summary of the invention

[0004] The purpose of the present invention is to provide a high-performance polyamide reverse osmosis membrane mediated by a three-dimensional nano-helix ordered stacking layer and a preparation method thereof. The present invention adopts a three-dimensional nano-helix material, forms an intermediate layer by orderly stacking, and then prepares a new type of reverse osmosis membrane. The three-dimensional nano-helix ordered stacking will form a sub-nanometer channel, which has a certain interception effect on salt and neutral small molecule pollutants. Through the gully effect and the resistance series effect, the water permeability and neutral small molecule pollutant interception capacity of the reverse osmosis membrane can be significantly enhanced.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention first provides a method for preparing a reverse osmosis membrane mediated by a three-dimensional nano-helical ordered stacking layer, the method comprising: first preparing a three-dimensional nano-helical body and preparing a dispersion of the three-dimensional nano-helical body, then pre-loading the three-dimensional nano-helical body onto a base film surface to form a base film loaded with a three-dimensional nano-helical ordered stacking layer, then infiltrating the base film loaded with a three-dimensional nano-helical ordered stacking layer with an m-phenylenediamine / water solution, then covering the base film surface with n-hexane containing trimesoyl chloride, causing an interfacial polymerization reaction, forming a polyamide layer on the three-dimensional nano-helical ordered stacking layer, and drying to prepare a reverse osmosis membrane mediated by a three-dimensional nano-helical ordered stacking layer;

[0007] The three-dimensional nano helix is ​​prepared by the following method: mixing a mixed aqueous solution of ammonium heptamolybdate and thiourea with pinene alcohol and oleylamine, reacting the mixture at a certain temperature, cooling, solid-liquid separation, and washing to obtain the three-dimensional nano helix.

[0008] In one embodiment of the present invention, in the mixed aqueous solution of ammonium heptamolybdate and thiourea, the mass concentration of ammonium heptamolybdate is 100-200 mg / mL, and the mass concentration of thiourea is 150-250 mg / mL.

[0009] In one embodiment of the present invention, the volume ratio of the mixed aqueous solution of ammonium heptamolybdate and thiourea, pineneol and oleylamine is 1-3:3-5:4-6.

[0010] In one embodiment of the present invention, during the preparation of the three-dimensional nanohelix, the reaction temperature is 150-250° C. and the reaction time is 5-8 hours. Furthermore, the reaction is carried out in a sealed autoclave.

[0011] In one embodiment of the present invention, the preparation method specifically comprises:

[0012] (1) Preparing a three-dimensional nano-helix: mixing a mixed aqueous solution of ammonium heptamolybdate and thiourea with pineneol and oleylamine, reacting the mixture at a certain temperature, cooling, solid-liquid separation, and washing to obtain a three-dimensional nano-helix;

[0013] (2) Preparation of a three-dimensional nanohelix dispersion: mixing the three-dimensional nanohelix with a dispersion solvent in a certain ratio, and obtaining a three-dimensional nanohelix dispersion after ultrasonic treatment;

[0014] (3) Preloading of three-dimensional nanohelices: The three-dimensional nanohelices are loaded on the surface of the basement membrane by vacuum filtration to form an ordered stacking layer of three-dimensional nanohelices on the surface of the basement membrane;

[0015] (4) Wetting of the base film: the base film loaded with the ordered stacked layers of three-dimensional nanohelices is treated in a 10-40 g / L m-phenylenediamine solution for 1-5 min, and then the excess solution on the surface of the film is removed;

[0016] (5) Interfacial polymerization: treating the base film obtained in step (4) with a 1-3 g / L hexane solution of trimesoyl chloride for 30-90 s, removing excess solution from the membrane surface, washing, and drying to obtain the three-dimensional nano-helical ordered stacking layer-mediated reverse osmosis membrane.

[0017] In one embodiment of the present invention, in step (2), the dispersion solvent includes one or both of water and ethanol.

[0018] In one embodiment of the present invention, in step (2), the weight ratio of the three-dimensional nanohelix to the dispersion solvent is 1:2000-5000.

[0019] In one embodiment of the present invention, in step (2), the ultrasonic time is 5-30 min.

[0020] In one embodiment of the present invention, in step (3), the base membrane is a polysulfone ultrafiltration membrane or a polyethersulfone ultrafiltration membrane.

[0021] In one embodiment of the present invention, in step (4), the concentration of m-phenylenediamine in the m-phenylenediamine solution is 10-40 g / L.

[0022] In one embodiment of the present invention, in step (4), the washing is preferably performed multiple times using n-hexane solution and deionized water; further, the drying includes natural drying, vacuum drying, etc., preferably in a vacuum drying oven at 40°C for 2 to 8 minutes.

[0023] In one embodiment of the present invention, in step (5), the concentration of the n-hexane solution of trimesoyl chloride is 1 to 3 g / L.

[0024] The present invention also provides a reverse osmosis membrane mediated by a three-dimensional nano-helical ordered stacking layer prepared by the above preparation method. The present invention introduces a three-dimensional nano-helical ordered stacking layer between the base membrane and the polyamide layer to simultaneously improve the neutral small molecule pollutant interception performance and water permeability of the reverse osmosis membrane.

[0025] The invention also provides application of the reverse osmosis membrane in water treatment.

[0026] The present invention has the following beneficial effects:

[0027] (1) The present invention introduces three-dimensional nanohelices between the base film and the polyamide layer. The orderly stacking of the three-dimensional nanohelices can effectively optimize the transmission path of water molecules between the polyamide and the base film, slow down the funnel effect, and reduce the water mass transfer resistance.

[0028] (2) In the reverse osmosis membrane of the present invention, the three-dimensional nano-helices are stacked in an orderly manner to form nano-scale screening channels between each other, which have a certain salt and neutral small molecule pollutant interception effect. Based on the resistance series effect, they work together with the polyamide layer to play an interception role, thereby enhancing the water permeability of the reverse osmosis membrane and the salt and neutral small molecule pollutant interception effect.

[0029] (3) The preparation method of the present invention only requires pre-loading the three-dimensional nano-helical ordered stacking layer on the surface of the base film before the traditional interfacial polymerization process, without changing the overall film-making process, and is easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 1 is a scanning electron microscope image of the surface of four polyamide layer reverse osmosis membranes prepared in Comparative Example 1 and Examples 1-3.

[0031] Figure 2 It is a comparison chart of water permeability of four polyamide reverse osmosis membranes prepared in Comparative Example 1 and Examples 1-3, and a comparison chart of sodium chloride retention of Comparative Example 2 and these four polyamide reverse osmosis membranes.

[0032] Figure 3 It is a comparison chart of pollutant retention of two polyamide reverse osmosis membranes prepared in Comparative Example 1 and Example 2, as well as the retention effect of Comparative Example 2 on neutral small molecule pollutants. DETAILED DESCRIPTION

[0033] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Comparative Example 1

[0035] The base membrane (polysulfone ultrafiltration membrane) was treated in a 20 g / L m-phenylenediamine / water solution for 2 min, excess droplets on the surface of the base membrane were removed with a roller, and the surface of the base membrane was treated with a n-hexane solution containing 1 g / L trimesoyl chloride for 60 s. The solution was poured off, the membrane was washed with n-hexane and deionized water for several times, and the membrane was treated in a vacuum drying oven at 40°C for 3 min.

[0036] Comparative Example 2

[0037] (1) Preparation of three-dimensional nanohelices: 300 mg of ammonium heptamolybdate and 380 mg of thiourea were dissolved in 2 mL of deionized water, respectively, and then mixed with 4 mL of pinene alcohol and 5 mL of oleylamine. The mixture was sealed in an autoclave and heated at 200° C. for 6 h. After cooling, the product was collected by centrifugation and washed with ethanol several times.

[0038] (2) Preparation of three-dimensional nanohelix dispersion: three-dimensional nanohelix and water were mixed at a weight ratio of 1:2500, and then ultrasonicated for 30 minutes to obtain a 0.4 g / L three-dimensional nanohelix dispersion.

[0039] (3) Loading of three-dimensional nanohelices: 300 μL of 0.4 g / L three-dimensional nanohelices were loaded on the surface of the basement membrane (same as comparative example 1) by vacuum filtration to form a three-dimensional nanohelical ordered stacking layer.

[0040] Example 1

[0041] (1) Preparation of three-dimensional nanohelices: 300 mg of ammonium heptamolybdate and 380 mg of thiourea were dissolved in 2 mL of deionized water, respectively, and then mixed with 4 mL of pinene alcohol and 5 mL of oleylamine. The mixture was sealed in an autoclave and heated at 200° C. for 6 h. After cooling, the product was collected by centrifugation and washed with ethanol several times.

[0042] (2) Preparation of three-dimensional nanohelix dispersion: The three-dimensional nanohelix and water were mixed at a weight ratio of 1:2500, and then ultrasonicated for 30 minutes to obtain a 0.4 g / L three-dimensional nanohelix orderly stacked dispersion.

[0043] (3) Pre-loading of three-dimensional nanohelices: 200 μL of 0.4 g / L three-dimensional nanohelices were loaded on the surface of the basement membrane (same as comparative example 1) by vacuum filtration to form a three-dimensional nanohelical ordered stacking layer.

[0044] (4) Wetting of the base membrane: The base membrane loaded with the ordered stacked layers of three-dimensional nanohelices was treated in a 20 g / L m-phenylenediamine solution for 2 min, and then the excess solution on the membrane surface was removed.

[0045] (5) Interfacial polymerization: The base film treated in step (4) was treated with a 1 g / L hexane solution of trimesoyl chloride for 60 s, and the excess solution on the membrane surface was poured off. The membrane was then washed several times with a hexane solution and deionized water, and the membrane was placed in a vacuum drying oven at 40°C for 3 min.

[0046] Example 2

[0047] (1) Preparation of three-dimensional nanohelices: 300 mg of ammonium heptamolybdate and 380 mg of thiourea were dissolved in 2 mL of deionized water, respectively, and then mixed with 4 mL of pinene alcohol and 5 mL of oleylamine. The mixture was sealed in an autoclave and heated at 200° C. for 6 h. After cooling, the product was collected by centrifugation and washed with ethanol several times.

[0048] (2) Preparation of three-dimensional nanohelix dispersion: The three-dimensional nanohelix orderly stacking and water were mixed in a weight ratio of 1:2500, and then ultrasonicated for 30 minutes to obtain a 0.4 g / L three-dimensional nanohelix orderly stacking dispersion.

[0049] (2) Pre-loading of three-dimensional nanohelices: 300 μL of 0.4 g / L three-dimensional nanohelices were loaded on the surface of the basement membrane (same as comparative example 1) by vacuum filtration to form a three-dimensional nanohelical ordered stacking layer.

[0050] (3) Basement membrane wetting: The basement membrane loaded with orderly stacked three-dimensional nanohelices was treated in a 20 g / L m-phenylenediamine solution for 2 min, and then the excess solution on the membrane surface was removed.

[0051] (4) Interfacial polymerization: The base film treated in step (3) was treated with a 1 g / L hexane solution of trimesoyl chloride for 60 s, and the excess solution on the membrane surface was poured off. The membrane was then washed several times with an n-hexane solution and deionized water, and the membrane was placed in a vacuum drying oven at 40°C for 3 min.

[0052] Example 3

[0053] (1) Preparation of three-dimensional nanohelices: 300 mg of ammonium heptamolybdate and 380 mg of thiourea were dissolved in 2 ml of deionized water, respectively, and then mixed with 4 mL of pinene alcohol and 5 mL of oleylamine. The mixture was sealed in an autoclave and heated at 200° C. for 6 h. After cooling, the product was collected by centrifugation and washed with ethanol several times.

[0054] (2) Preparation of three-dimensional nanohelix dispersion: The three-dimensional nanohelix orderly stacking and water were mixed in a weight ratio of 1:2500, and then ultrasonicated for 30 minutes to obtain a 0.4 g / L three-dimensional nanohelix orderly stacking dispersion.

[0055] (2) Pre-loading of three-dimensional nanohelices: 400 μL of 0.4 g / L three-dimensional nanohelices were loaded on the surface of the basement membrane (same as comparative example 1) by vacuum filtration to form a three-dimensional nanohelical ordered stacking layer.

[0056] (3) Wetting of the base membrane: The base membrane loaded with the ordered stacked layers of three-dimensional nanohelices was treated in a 20 g / L m-phenylenediamine solution for 2 min, and then the excess solution on the membrane surface was removed.

[0057] (4) Interfacial polymerization: The base film treated in step (3) was treated with a 1 g / L hexane solution of trimesoyl chloride for 60 s, and the excess solution on the membrane surface was poured off. The membrane was then washed several times with an n-hexane solution and deionized water, and the membrane was placed in a vacuum drying oven at 40°C for 3 min.

[0058] Test Example 1

[0059] Surface morphology: Figure 1 The scanning electron microscope observations shown show that the surfaces of the polyamide layers of Comparative Example 1 and Examples 1, 2, and 3 all present a typical "peak-valley" structure, proving that a polyamide layer with separation performance is prepared. Compared with Comparative Example 1, the surface of the polyamide membrane of the Examples has no obvious change.

[0060] Test Example 2

[0061] Water permeability and NaCl retention rate: Use pure water to pre-press each membrane sample at an operating pressure of 16 bar for 1.5 hours, and test under cross-flow filtration conditions with an operating pressure of 16 bar, a water temperature of 25°C, and a cross-flow rate of 22.4 cm / s. At the same time, take the volume of water out of each sample membrane to measure and calculate the water permeability; Use pure water to pre-press each membrane sample at an operating pressure of 16 bar for 1.5 hours, prepare a 2000 mg / L NaCl aqueous solution, and test under cross-flow filtration conditions with an operating pressure of 16 bar, a water temperature of 25°C, and a cross-flow rate of 22.4 cm / s. Determine the NaCl concentration of the inlet and outlet water based on conductivity, and calculate the NaCl retention rate. The test results are as follows: Figure 2 shown.

[0062] Depend on Figure 2 It can be seen that the water permeability of Comparative Example 1 is 1.8 L·m -2 ·h -1 bar -1 Compared with the comparative example, the water permeability of Examples 1-3 is significantly improved, which may be due to the gully effect of the ordered stacking layer of three-dimensional nano-helices, which optimizes the transport path of water molecules between the base film and the polyamide layer and reduces the transport resistance of water molecules. Among them, the water permeability of Example 2 is the highest, reaching 3.63L·m -2 ·h -1 bar -1 , which is 201% of Comparative Example 1. At the same time, Figure 2 It also shows that the NaCl retention rate of Comparative Example 2 reaches 7.9%, indicating that the ordered stacking of the three-dimensional nano-helices may form nano-scale sieving channels to partially retain salt; the NaCl retention rates of Examples 1-3 are all improved compared with those of Comparative Example 1 (Comparative Example 1 is 97.3%, Example 1 is 98.5%, Example 2 is 98.7%, and Example 3 is 98.9%). Based on the series resistance effect, the polyamide layer and the polyamide layer work together to enhance the salt retention effect of the reverse osmosis membrane.

[0063] Test Example 3

[0064] Retention of neutral small molecule pollutants: The membrane sample was pre-pressed with pure water for 1.5 h at an operating pressure of 16 bar, and 200 μg / L solutions of N-nitrosodimethylamine, N-nitrosomethylethylamine, N-nitrosopyrrolidine, and N-nitrosodiethylamine were prepared respectively. The test was carried out under cross-flow filtration conditions with an operating pressure of 16 bar, a water temperature of 25°C, and a cross-flow rate of 22.4 cm / s. The concentrations of neutral small molecule pollutants in the feed liquid and the permeate were determined based on high performance liquid chromatography-tandem quadrupole mass spectrometry, and the retention rate was calculated. The test results are shown in the figure. Figure 3 shown.

[0065] Depend on Figure 3 It can be seen that the pollutant retention rates of Comparative Example 1 for N-nitrosodimethylamine, N-nitrosomethylethylamine, N-nitrosopyrrolidine and N-nitrosodiethylamine are 46.8%, 79.0%, 86.7% and 93.2%, respectively, and the retention rates of Comparative Example 2 for these nitrosamine pollutants are 4.50%, 5.36%, 5.07% and 6.33%, respectively, indicating that the ordered stacking of three-dimensional nanohelices may form nanoscale sieving channels to intercept neutral small molecule pollutants; compared with Comparative Example 1, the retention rates of Example 2 for these nitrosamine pollutants are 69.9%, 87.6%, 89.9% and 95.0%, respectively, indicating that the polyamide reverse osmosis membrane mediated by the ordered stacking layer of three-dimensional nanohelices can effectively intercept nitrosamine pollutants by relying on the series resistance effect while maintaining excellent water permeability.

[0066] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing a reverse osmosis membrane mediated by three-dimensional nano-helical ordered stacking layers, characterized in that: The method comprises: firstly preparing a three-dimensional nano-helix, and preparing a dispersion of the three-dimensional nano-helix, and then pre-loading the dispersion onto the surface of a base film to form a base film loaded with a three-dimensional nano-helix ordered stacking layer, and then infiltrating the base film loaded with the three-dimensional nano-helix ordered stacking layer with a m-phenylenediamine / water solution, and then covering the surface of the base film with n-hexane containing trimesoyl chloride to generate an interfacial polymerization reaction to form a polyamide layer on the three-dimensional nano-helix ordered stacking layer, and drying to prepare a reverse osmosis membrane mediated by the three-dimensional nano-helix ordered stacking layer; The three-dimensional nano helix is ​​prepared by the following method: mixing a mixed aqueous solution of ammonium heptamolybdate and thiourea with pinene alcohol and oleylamine, reacting the mixture at a certain temperature, cooling, solid-liquid separation, and washing to obtain the three-dimensional nano helix.

2. The method for preparing a reverse osmosis membrane mediated by a three-dimensional nano-helical ordered stacking layer according to claim 1, characterized in that: In the mixed aqueous solution of ammonium heptamolybdate and thiourea, the mass concentration of ammonium heptamolybdate is 100-200 mg / mL, and the mass concentration of thiourea is 150-250 mg / mL.

3. The method for preparing a reverse osmosis membrane mediated by a three-dimensional nano-helical ordered stacking layer according to claim 1, characterized in that: The volume ratio of the mixed aqueous solution of ammonium heptamolybdate and thiourea, pineneol and oleylamine is 1-3:3-5:4-6.

4. The method for preparing a reverse osmosis membrane mediated by a three-dimensional nano-helical ordered stacking layer according to any one of claims 1 to 3, characterized in that: In the process of preparing the three-dimensional nano-helix, the reaction temperature is 150-250° C. and the reaction time is 5-8 hours.

5. The method for preparing a reverse osmosis membrane mediated by a three-dimensional nano-helical ordered stacking layer according to claim 4, characterized in that: The preparation method specifically comprises: (1) Preparing a three-dimensional nano-helix: mixing a mixed aqueous solution of ammonium heptamolybdate and thiourea with pineneol and oleylamine, reacting the mixture at a certain temperature, cooling, solid-liquid separation, and washing to obtain a three-dimensional nano-helix; (2) Preparation of a three-dimensional nanohelix dispersion: mixing the three-dimensional nanohelix with a dispersion solvent in a certain ratio, and obtaining a three-dimensional nanohelix dispersion after ultrasonic treatment; (3) Preloading of three-dimensional nanohelices: The three-dimensional nanohelices are loaded on the surface of the basement membrane by vacuum filtration to form an ordered stacking layer of three-dimensional nanohelices on the surface of the basement membrane; (4) Wetting of the base film: the base film loaded with the ordered stacked layers of three-dimensional nanohelices is treated in a m-phenylenediamine solution for 1 to 5 minutes, and then the excess solution on the surface of the film is removed; (5) Interfacial polymerization: treating the base film obtained in step (4) with a n-hexane solution of trimesoyl chloride for 30 to 90 seconds, removing excess solution from the membrane surface, washing, and drying to obtain the reverse osmosis membrane mediated by the three-dimensional nano-helical ordered stacking layer.

6. According to the method for preparing a reverse osmosis membrane mediated by three-dimensional nano-helical ordered stacking layers according to claim 5, in step (2), the dispersion solvent comprises one or both of water and ethanol.

7. The method for preparing a reverse osmosis membrane mediated by a three-dimensional nano-helix ordered stacking layer according to claim 5, wherein in step (2), the weight ratio of the three-dimensional nano-helix to the dispersion solvent is 1:2000-5000.

8. The method for preparing a reverse osmosis membrane mediated by three-dimensional nano-helical ordered stacking layers according to any one of claims 5 to 7, wherein in step (3), the base membrane is any one of a polysulfone ultrafiltration membrane and a polyethersulfone ultrafiltration membrane. 9 . A reverse osmosis membrane mediated by three-dimensional nano-helical ordered stacking layers prepared according to the preparation method according to any one of claims 1 to 8 .

10. Use of the reverse osmosis membrane according to claim 9 in water treatment.