A method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate
By combining femtosecond laser nanodomain inversion with wet etching, the problem of efficient and high-quality fabrication of complex micro- and nanostructures on the surface of lithium niobate was solved, and the fabrication of high-precision complex structures was achieved to meet optical requirements.
Patent Information
- Application Number
- CN202410052608.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-15
AI Technical Summary
Existing technologies make it difficult to achieve high-precision, high-efficiency, and high-quality fabrication of complex micro/nano structures on the surface of lithium niobate, especially the fabrication of complex three-dimensional structures such as pointed cone structures.
By using femtosecond lasers to perform nanodomain inversion treatment inside lithium niobate materials, combined with wet etching processes, selective etching is achieved by leveraging the difference in etching resistance between the laser-polarized nanodomain inversion region and the untreated region. With the high-precision exposure control of the laser focus, high-precision complex structures can be fabricated.
The efficient and high-quality preparation of high-precision complex structures on the surface of lithium niobate materials has been achieved, with low surface roughness and high precision of nanoscale structures, meeting optical requirements.
Smart Images

Figure CN118002909B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of laser micro-nano processing technology, specifically involving the fabrication of high-precision complex micro-nano structures on the surface of lithium niobate materials using etching-assisted femtosecond laser polarized lithium niobate domain inversion technology. Background Technology
[0002] Lithium niobate crystals possess a wide transmission window, high nonlinearity, and an electro-optic coefficient, thus exhibiting excellent electro-optic, acousto-optic, thermo-optic, and piezoelectric nonlinear properties. They have wide applications in nonlinear optics fields such as electro-optic modulation, optical switching, photonic integration, and frequency conversion, earning them the title of "silicon of photonics." To date, researchers have proposed various lithium niobate processing techniques, including electron beam lithography (EBL), photolithography-assisted dry etching, wet etching, and chemical mechanical polishing. However, these methods all require pre-patterned masks, resulting in complex processes and difficulties in fabricating complex three-dimensional structures.
[0003] Femtosecond lasers possess high peak power and high processing freedom, enabling the fabrication of complex structures on the surfaces of hard and brittle materials. Femtosecond laser-based direct writing technology is a high-precision, maskless direct writing method. Therefore, femtosecond laser direct writing technology is one of the effective methods for achieving high-precision, complex lithium niobate micro / nanostructure fabrication. In recent years, femtosecond laser direct writing technology has been used to fabricate photonic crystals and nano-ferroelectric domains within lithium niobate crystals. However, the surface roughness of lithium niobate structures fabricated using femtosecond laser direct writing technology is relatively high, making it difficult to meet optical requirements. Furthermore, existing laser processing methods have limited precision, making it difficult to achieve nanoscale lithium niobate structure fabrication. High-quality and efficient fabrication of complex three-dimensional structures, such as pointed cone structures, is particularly challenging. Therefore, achieving high-precision, efficient, and high-quality processing of complex micro / nanostructures on the surface of lithium niobate is a major challenge in the field of lithium niobate micro / nano manufacturing. Summary of the Invention
[0004] To address the challenges of precision machining of complex structures on the surfaces of hard and brittle materials such as lithium niobate in existing technologies, this invention provides a method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate. This method utilizes a femtosecond laser to perform nanodomain inversion within the lithium niobate material. Specifically, the femtosecond laser is focused on the -z plane of lithium niobate, generating strong multiphoton absorption, thus creating a localized temperature field within the material. This temperature gradient field, combined with the thermoelectric and pyroelectric effects of lithium niobate, forms a thermoelectric field opposite to the spontaneous polarization field. By strictly controlling the laser power to make the thermoelectric field greater than the spontaneous polarization field, the nanodomains will invert. At this point, the etching resistance of the laser-treated and untreated areas changes, allowing for selective etching in conjunction with subsequent wet etching processes. Notably, the laser-polarized nanodomains inverted areas are retained during the subsequent wet etching process, while the untreated portions are removed. Due to this characteristic, combined with high-precision single-pulse exposure control of the laser focus, efficient and high-quality fabrication of high-precision complex structures on the surface of lithium niobate materials can be achieved.
[0005] This invention is achieved through the following technical solution:
[0006] A method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate, specifically including the following steps:
[0007] Step 1: Sample preparation;
[0008] First, the sample to be processed was ultrasonically cleaned in acetone, ethanol and deionized water respectively, and then dried with a syringe. Then, the crystal plane of the lithium niobate sample was identified, and the -z plane was found as the surface to be processed. The sample preparation was completed.
[0009] Step 2: Femtosecond laser polarization of nanodomains inversion on the sample to be processed;
[0010] First, the sample to be processed is fixed on a three-dimensional electronically controlled platform with its -z-plane facing upwards. The femtosecond laser emitted from the femtosecond laser amplifier enters the micro-nano fabrication system and is focused onto the upper surface of the sample. Then, the position of the laser spot and the focal point are confirmed by the sample surface exposure and scribing scanning method. The laser processing power is adjusted until it exceeds the reversal threshold, causing the nanodomains in the vicinity of the sample surface to reverse, so that the polarization direction of the nanodomains points in the opposite direction of the temperature gradient, thereby making the laser-irradiated area of the -z-plane sample positively charged. Then, the pre-designed processing file is read into the processing program, and the direct writing processing from the inside to the surface is performed by scanning point by point and layer by layer.
[0011] Step 3: Sample etching;
[0012] The specific steps are as follows: First, the sample obtained in step two is cleaned in sequence with acetone, ethanol, and deionized water to remove residual debris on the surface after processing. The sample is then placed in an open polytetrafluoroethylene beaker containing a mixed solution of hydrofluoric acid and nitric acid for high-temperature etching. Due to the laser polarization nanodomain inversion in step two, the laser-irradiated area of the -z plane sample becomes positively charged, making it difficult to combine with hydrogen ions in the etching solution and react, thus inhibiting etching. Ultimately, the inverted area is retained, while the unprocessed area is removed. Then, the etched sample is first ultrasonically treated with acetone solution, then with ethanol solution, and finally with deionized water, and finally dried with a rubber bulb. The surface structure of the sample after high-temperature etching is exposed, realizing the preparation of a high-quality nanocone array structure on the material surface.
[0013] Furthermore, in step one, the sample to be processed is a transparent lithium niobate crystal sheet with a thickness of 0.3-0.5 mm.
[0014] Further, in step two, the micro / nano fabrication system includes a first concave lens L1, a second convex lens L2, a third convex lens L3, a first semi-reflective lens M1, a second semi-reflective lens M2, an image sensor CCD, an objective lens O, and a three-dimensional electronic control platform; the femtosecond laser emitted from the laser is expanded sequentially by the first concave lens L1 and the second convex lens L2; then the beam reaches the objective lens O via the first semi-reflective lens M1; in addition, the mercury lamp light source illuminates the sample on the platform sequentially by the second semi-reflective lens M2, the first semi-reflective lens M1, and the focusing ring objective lens O, and the reflected light is finally reflected by the second semi-reflective lens M2 and then reaches the image sensor CCD for imaging via the third convex lens L3.
[0015] Furthermore, in step two, the three-dimensional electronic control platform is a three-axis electronic control platform with X-axis, Y-axis and Z-axis, wherein the X-axis and Y-axis have a movement range of 0-5cm and an accuracy of 1-100nm, and the Z-axis has a movement range of 0-5mm and a movement accuracy of 1-100nm.
[0016] Furthermore, in step two, the femtosecond laser is an infrared femtosecond laser with a wavelength of 1030nm; the laser repetition frequency is 90-200kHz, and the pulse width is 150-280fs; the objective lens used is a 5×-40× lens with a numerical aperture of 0.1-0.6; the single pulse energy of laser ablation is 0.8-2.5nJ; the laser scanning speed is 1-50mm / s; the point spacing of the processing data is 200-1000nm, the line spacing is 200-1000nm, and the layer spacing is 100-500nm.
[0017] Furthermore, in step three, the mass fraction of the hydrofluoric acid solution is 10%-40%, the mass fraction of the nitric acid solution is 10%-69%, the volume ratio of the nitric acid and hydrofluoric acid mixed solution is 1:2, the temperature range of the high-temperature etching is 300-500K, and the high-temperature etching time range is 10-20min.
[0018] Furthermore, in step three, the height of the nanocone array structure ranges from 0.4 to 2 μm, the cone angle ranges from 10 to 60°, and the roughness ranges from 0.34 to 1 nm.
[0019] Compared with the prior art, the advantages of the present invention are as follows:
[0020] (1) The present invention provides a method for processing high-precision complex micro-nano structures on the surface of lithium niobate. Compared with the femtosecond laser direct writing technology, the surface roughness of the structure after laser direct writing is difficult to meet the optical requirements. However, the present invention uses wet etching to assist laser polarization nanodomain inversion to achieve the preparation of high surface quality structures.
[0021] (2) The writing of nanodomains proposed in this invention, combined with subsequent etching to expose the structure, can achieve high-precision preparation of nanoscale structures on the surface of lithium niobate materials. Attached Figure Description
[0022] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the accompanying drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn to scale.
[0023] Figure 1 This is a schematic diagram of the femtosecond laser processing optical path for a method of processing high-precision complex micro / nano structures on the surface of lithium niobate according to the present invention.
[0024] Among them, the first concave lens L1, the second convex lens L2, the third convex lens L3, the first semi-reflective lens M1, the second semi-reflective lens M2, the image sensor CCD, and the objective lens O;
[0025] Figure 2 This is an overall flowchart of a method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate according to the present invention;
[0026] Figure 3 This is a schematic diagram of a method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate according to the present invention.
[0027] In the figure, a is the image of lithium niobate without laser irradiation, b is the image of lithium niobate nanodomains with reversed polarization direction after laser irradiation, and c is the image of nanocone surface structure formed in the nanodomain region after etching.
[0028] Figure 4 This is a flowchart of a method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate according to the present invention;
[0029] Figure 5 Scanning electron microscope images of high-precision nanocone structures with different periods prepared by a method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate according to the present invention.
[0030] Wherein, a is a periodic 200nm nanocone array pattern, b is a periodic 500nm nanocone array pattern, and c is a periodic 700nm nanocone array pattern;
[0031] Figure 6 A scanning electron microscope image of a patterned lithium niobate structure with the letter "LN" prepared according to a method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate according to the present invention.
[0032] Where a is the overall view of the patterned structure, and b is a magnified view of a part of the patterned structure;
[0033] Figure 7 Comparison of scanning electron microscope images of lithium niobate surfaces marked "LN bulk" prepared by a high-precision complex micro / nano structure fabrication method of the present invention and a traditional laser modification method;
[0034] In this image, a is a scanning electron microscope (SEM) image of the structure prepared by etching-assisted femtosecond laser polarization lithium niobate domain inversion technology, and b is a scanning electron microscope (SEM) image of the structure prepared by etching-assisted femtosecond laser modification technology.
[0035] Figure 8 Transmittance test curve of a lithium niobate surface nanocone antireflection structure prepared by a high-precision complex micro / nano structure fabrication method of the present invention;
[0036] Figure 9 A graph showing the equivalent dielectric constant of a lithium niobate surface nanocone structure prepared by a high-precision complex micro / nano structure fabrication method of the present invention as a function of height and position.
[0037] Figure 10 The atomic force diagram of the lithium niobate structure surface prepared by the method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate according to the present invention. Detailed Implementation
[0038] To clearly and completely describe the technical solution and its specific working process of the present invention, the specific embodiments of the present invention are as follows, in conjunction with the accompanying drawings:
[0039] Example 1
[0040] High-precision nanocone "LN" patterned structures were prepared on the surface of lithium niobate using etching-assisted femtosecond laser polarization lithium niobate domain inversion technology.
[0041] Depend on Figure 1 As shown, the 1030nm femtosecond laser emitted by the laser is expanded sequentially by the first concave lens L1 and the second convex lens L2; then the beam reaches the objective lens O through the first semi-reflective lens M1; in addition, the mercury lamp light source illuminates the sample on the platform sequentially through the second semi-reflective lens M2, the first semi-reflective lens M1 and the focusing ring objective lens O, and the reflected light is finally reflected by the second semi-reflective lens M2 and then reaches the image sensor CCD through the third convex lens L3 to form an image.
[0042] Specifically, such as Figure 2 The diagram shown is an overall flow chart of a method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate according to this embodiment. The specific steps of the fabrication method are as follows:
[0043] Step 1: Sample preparation;
[0044] First, a z-cut lithium niobate sample with a length of 1 cm, a width of 1 cm, and a thickness of 500 μm was ultrasonically cleaned in acetone, ethanol, and deionized water for 10 min, and then dried with a syringe. Subsequently, the crystal planes of the lithium niobate sample were identified, and the -z plane was found as the surface to be processed. The sample preparation was then completed.
[0045] Step 2: Femtosecond laser polarization of nanodomains inversion on the sample to be processed;
[0046] First, the sample was fixed on the 3D electronic control platform with its z-plane facing upwards. The laser power emitted from the laser was adjusted so that the single-pulse energy of the laser after passing through the objective lens was 0.8 nJ. The image sensor and the illumination mercury lamp light source were turned on. The 3D electronic control platform was adjusted, first adjusting the Z-axis, and the sample was slowly raised to locate the upper surface of the sample to be processed in the imaging system. The processing control program was opened, the shutter was opened, and the X-axis was adjusted. At the same time, the program controlled the Z-axis up and down by 1 μm until ablation marks appeared on the sample. At this point, the laser focus was on the upper surface of the sample. Then, the shutter was closed, the X-axis was adjusted to move away from the ablation position, and the patterned processing data of the letters "LN" was imported. The scanning mode was from the inside of the material to the surface, and the single-pulse laser polarization nanodomain inversion process of the lithium niobate nanocone structure was started. The femtosecond laser wavelength was 1030 nm, the repetition frequency was 200 kHz, the pulse width was 280 fs, the laser scanning speed was 0.1 mm / s, the objective lens was a 40× lens, and the numerical aperture was 0.6.
[0047] Step 3: Sample etching;
[0048] The specific steps are as follows: First, the sample obtained in step two is cleaned sequentially with acetone, ethanol, and deionized water to remove residual debris from the surface after processing. The sample is then placed in an open PTFE beaker containing a 1:2 mixture of 69% nitric acid solution and 40% hydrofluoric acid solution, and etched at 450K for 15 minutes. After etching, the sample is first subjected to acetone solution, then ethanol solution, and finally deionized water, each solution being ultrasonically treated for 10 minutes. Finally, it is dried with a syringe. The surface structure of the sample after high-temperature etching is exposed, achieving the fabrication of a high-precision nanocone structure on the lithium niobate surface.
[0049] Example 2
[0050] Nanocone antireflective structures were prepared on the surface of lithium niobate using etching-assisted femtosecond laser polarization lithium niobate domain inversion technology.
[0051] Processing systems such as Figure 1 As shown, the same as in Example 1.
[0052] This embodiment provides a method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate. The specific steps are as follows:
[0053] (1) Preparation of samples to be processed;
[0054] Same as Example 1
[0055] (2) Sample to be processed by femtosecond laser polarized nanodomain inversion;
[0056] First, the sample was fixed on the 3D electronic control platform with its z-plane facing upwards. The laser power emitted from the laser was adjusted so that the single-pulse energy after passing through the objective lens was 1 nJ. The image sensor and the illumination mercury lamp light source were turned on. The 3D electronic control platform was adjusted, first adjusting the Z-axis, and the sample was slowly raised to locate the upper surface of the sample to be processed in the imaging system. The processing control program was opened, the shutter was opened, and the X-axis was adjusted. At the same time, the program controlled the Z-axis up and down by 1 μm until ablation marks appeared on the sample. At this point, the laser focus was on the upper surface of the sample. Then, the shutter was closed, the X-axis was adjusted to move away from the ablation position, and the processing data of the nanocone antireflection structure with a period of 1 μm was imported. The scanning mode was from the inside of the material to the surface, and the laser polarization nanodomain inversion process of lithium niobate was started. The femtosecond laser wavelength was 1030 nm, the repetition frequency was 200 kHz, the pulse width was 280 fs, the laser scanning speed was 0.4 mm / s, the objective lens was a 40× lens, and the numerical aperture was 0.6.
[0057] (3) Sample etching;
[0058] First, the sample obtained in step two was cleaned sequentially with acetone, ethanol, and deionized water to remove residual debris from the surface after processing. The sample was then placed in an open PTFE beaker containing a 1:2 mixture of 69% nitric acid solution and 40% hydrofluoric acid solution, and etched at 400K for 10 minutes. After etching, the sample was ultrasonically treated first with acetone, then with ethanol, and finally with deionized water, each for 10 minutes. Finally, it was dried with a syringe. The surface structure of the etched sample was exposed, thus achieving the fabrication of a nanocone antireflective structure on the lithium niobate surface.
[0059] Depend on Figure 3 It is known that the etching-assisted femtosecond laser polarization lithium niobate domain reversal technology can be used to prepare nanocone structures on the surface of lithium niobate. Specifically, after femtosecond laser irradiation of lithium niobate nanodomains, the polarization direction of the nanodomains will be reversed. Subsequently, through further selective etching, nanocone surface structures are formed in the nanodomain regions.
[0060] Depend on Figure 4 It is known that after laser polarization nanodomain inversion, as the etching process proceeds, a surface nanocone structure gradually forms. The nanocone prepared using the method of this invention has a maximum height of 2 μm and a minimum cone angle of 10°.
[0061] Depend on Figure 5 It is known that high-precision lithium niobate nanocone structures with periods of 200 nm, 500 nm and 700 nm can be prepared by using etching-assisted femtosecond laser polarization lithium niobate domain inversion technology.
[0062] Depend on Figure 6 It is known that the method of the present invention can be used to prepare large-area patterned structures of lithium niobate with the letter "LN".
[0063] Depend on Figure 7 As can be seen from b, traditional laser modification methods, based on the principle of removing material after modification etching, can only achieve recessed lithium niobate structures with the inscription "LN bulk". Figure 7 As shown in a, the method of the present invention can be used to prepare inverse structures such as protruding lithium niobate with the letter "LN bulk" based on the principle of retaining materials after polarization reversal etching.
[0064] Depend on Figure 8 It can be seen that the method of the present invention can be used to prepare large-area lithium niobate nanocone antireflective structures with good antireflective effect, increasing the transmittance from 79% to 85%.
[0065] Depend on Figure 9It is known that the antireflective effect of lithium niobate is determined by the surface refractive index gradient. Different structural morphologies correspond to different equivalent refractive index gradients. Common antireflective structural morphologies include cone-shaped, pyramidal, and moth-eye-shaped structures, among which the cone-shaped structure has a better antireflective effect due to its high refractive index gradient. The method of this invention can achieve high-quality preparation of nanoconical structures on the surface of lithium niobate to achieve a large refractive index gradient, thereby achieving a better antireflective effect.
[0066] Depend on Figure 10 It is known that the surface roughness of lithium niobate, traditionally written by laser, is typically on the order of hundreds of nanometers, which is insufficient to meet the optical requirements of devices. The method of this invention enables the high-quality fabrication of lithium niobate surface structures with a surface roughness as low as 0.34 nm, a surface quality sufficient to meet the optical requirements of devices.
[0067] The preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
[0068] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0069] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate, characterized in that, Specifically, the steps include the following: Step 1: Sample preparation; First, the sample to be processed was ultrasonically cleaned in acetone, ethanol and deionized water respectively, and then dried with a syringe. Then, the crystal plane of the lithium niobate sample was identified, and the -z plane was found as the surface to be processed. The sample preparation was completed. Step 2: Femtosecond laser polarization of nanodomains inversion on the sample to be processed; First, the sample to be processed is fixed on the three-dimensional electronic control platform with the -z plane facing upward. After the femtosecond laser emitted from the femtosecond laser amplifier enters the micro-nano processing system, it is focused onto the upper surface of the sample to be processed. Subsequently, the position of the laser spot and the position of the focal point are confirmed by the sample surface exposure and scribing scanning method. The laser processing power is adjusted until it exceeds the reversal threshold, so that the nanodomains in the vicinity of the sample surface are reversed and the polarization direction of the nanodomains points to the opposite of the temperature gradient, so that the laser irradiated area of the -z surface sample is positively charged. Then, the pre-designed processing file is read into the processing program, and the direct writing processing from the inside to the surface is performed by the point-by-point and layer-by-layer scanning method. Step 3: Sample etching; The specific steps are as follows: First, the sample obtained in step two is cleaned in sequence with acetone, ethanol, and deionized water to remove residual debris on the surface after processing. The sample is then placed in an open polytetrafluoroethylene beaker containing a mixture of hydrofluoric acid and nitric acid solutions for high-temperature etching. Due to the laser polarization nanodomain inversion in step two, the laser-irradiated area of the -z plane sample becomes positively charged, making it less likely to combine with hydrogen ions in the etching solution and react, thus inhibiting etching. Ultimately, the inverted area is retained, while the unprocessed area is removed. Then, the etched sample is ultrasonically treated with acetone solution, followed by ethanol solution, and finally deionized water. Finally, it is dried with a rubber bulb. The surface structure of the sample after high-temperature etching is exposed, realizing the preparation of a high-quality nanocone array structure on the material surface. In step two, the femtosecond laser is an infrared femtosecond laser with a wavelength of 1030nm; the laser repetition frequency is 90-200kHz, and the pulse width is 150-280fs; the objective lens used is a 5×-40× lens with a numerical aperture of 0.1-0.6; the single pulse energy of laser ablation is 0.8-2.5nJ; the laser scanning speed is 1-50mm / s; the point spacing of the processing data is 200-1000nm, the line spacing is 200-1000nm, and the layer spacing is 100-500nm. In step three, the height of the nanocone array structure ranges from 0.4 to 2 μm, the cone angle ranges from 10 to 60°, and the roughness ranges from 0.34 to 1 nm.
2. The method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate as described in claim 1, characterized in that, In step one, the sample to be processed is a transparent lithium niobate crystal sheet with a thickness of 0.3-0.5 mm.
3. The method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate as described in claim 1, characterized in that, In step two, the micro / nano fabrication system includes a first concave lens L1, a second convex lens L2, a third convex lens L3, a first semi-reflective lens M1, a second semi-reflective lens M2, an image sensor CCD, an objective lens O, and a three-dimensional electronic control platform. The femtosecond laser emitted from the laser is expanded sequentially by the first concave lens L1 and the second convex lens L2. Then, the beam reaches the objective lens O through the first semi-reflective lens M1. In addition, the mercury lamp light source illuminates the sample on the platform sequentially by the second semi-reflective lens M2, the first semi-reflective lens M1, and the focusing ring objective lens O. The reflected light is finally reflected by the second semi-reflective lens M2 and then reaches the image sensor CCD for imaging through the third convex lens L3.
4. The method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate as described in claim 1, characterized in that, In step two, the three-dimensional electronic control platform is a three-axis electronic control platform with X-axis, Y-axis and Z-axis. The movement range of the X-axis and Y-axis is 0-5cm and the accuracy is 1-100nm. The movement range of the Z-axis is 0-5mm and the movement accuracy is 1-100nm.
5. The method for fabricating high-precision complex micro / nano structures on the surface of lithium niobate as described in claim 1, characterized in that, In step three, the mass fraction of the hydrofluoric acid solution is 10%-40%, the mass fraction of the nitric acid solution is 10%-69%, the volume ratio of the nitric acid solution to the hydrofluoric acid solution in the mixed solution is 1:2, the temperature range of the high-temperature etching is 300-500K, and the high-temperature etching time range is 10-20min.
Citation Information
Patent Citations
Process for forming a microstructure in a substrate of a ferroelectric single crystal
US6117346A