A high-performance rare earth-based radiation cooling coating and preparation method thereof

By using rare earth-based materials and specific processes in radiant refrigeration coatings, the problem in the existing technology that radiant refrigeration coatings are difficult to achieve both high reflectivity and high emissivity is solved, achieving efficient heat dissipation and avoiding additional covers. Used as surface layer, suitable for building exterior walls and roofs.

CN118006156BActive Publication Date: 2024-10-25ZHONGXIN YI TU TECH DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410042326.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-11
Publication Date
2024-10-25
Estimated Expiration
2044-01-11

AI Technical Summary

Technical Problem

It is difficult for existing radiant cooling coatings to achieve high reflectivity and high emissivity at the same time, and an additional overcoat layer is required to improve aging resistance. However, the overcoat layer will reduce the radiant cooling function of the coating, leading to a vicious cycle.

Method used

It adopts high-performance rare earth-based radiation refrigeration coating, including reflection enhancement layer and radiation refrigeration layer. The reflection enhancement layer is composed of water-based resin, metal powder filler and additives. The radiation refrigeration layer is composed of germanium oxide, niobium oxide, lanthanum oxide and selenium oxide. Specific proportions and processes are used to increase the reflectivity and emissivity of the coating without the need for an additional overcoat.

Benefits of technology

It achieves high reflectivity and high emissivity, with a heat dissipation power of more than 100W/m2 at room temperature and an outdoor cooling of more than 5 degrees without the need for additional covering layers. It is suitable for building exterior walls and roofs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118006156B_ABST
    Figure CN118006156B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-performance rare earth-based radiation cooling coating and a preparation method thereof. The high-performance rare earth-based radiation cooling coating comprises a reflection enhancement layer and a radiation cooling layer; the reflection enhancement layer comprises: water-based resin, metal powder filler, additives and water; the radiation cooling layer comprises: germanium oxide, niobium oxide, lanthanum oxide and selenium oxide. The high-performance rare earth-based radiation cooling coating window of the present invention has high emissivity and high reflectivity, and does not require an additional cover layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating materials, in particular to a high-performance rare earth-based radiation refrigeration coating and a preparation method thereof. Background Art

[0002] Among many energy-saving building materials, radiation cooling paint is an emerging paint product in recent years. This coating product has both high sunlight reflection effect and high "atmospheric window" emission effect. High sunlight reflection performance can reduce the incident sunlight energy, while high "atmospheric window" emission performance can emit heat into outer space in the form of 8-13 micron thermal radiation, achieving heat dissipation and cooling effect. Applying radiation cooling paint to the wall can effectively reduce the incident external energy in the building, thereby achieving energy saving and consumption reduction.

[0003] The core material of radiant cooling coating is the functional filler in the coating. In the prior art, two types of fillers are usually used to achieve the radiant cooling function. The first type of material is the sunlight reflective filler. Among this type of filler, titanium dioxide is the most commonly used sunlight reflective filler with the best comprehensive performance, but it absorbs ultraviolet rays and causes the overall reflectivity to be low. The second type of material is the emissive filler. Common emissive fillers are silica microspheres and glass microspheres. This type of material has good emissive performance in the 9.2-micron far-infrared band. However, the emissive material will reduce the solid content of the reflective filler in the coating, thereby further reducing the reflectivity of the coating.

[0004] In the prior art, a single radiation cooling coating often cannot achieve both the functionality and aging resistance of radiation cooling. This is because in the prior art, reflective functional fillers and emissive functional fillers need to be added to the coating at the same time, which results in a high proportion of total fillers and a small proportion of resin. The resin mainly acts as a bonding filler and cannot protect the paint surface. Therefore, in actual use, existing radiation cooling coatings often require an additional layer of topcoat to protect the coating. The use of a topcoat is a double-edged sword. On the one hand, the topcoat can improve the aging resistance and service life of the coating, while on the other hand, the topcoat will reduce the functionality of the lower radiation cooling layer to a certain extent. In order to make up for the loss of coating functionality, the solid content of the filler can only be further increased, thus falling into a vicious circle.

[0005] Therefore, the present invention proposes a high-performance rare earth-based radiation cooling coating with high emissivity, high reflectivity and no need for an additional topcoat. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a high-performance rare earth-based radiant cooling coating and a preparation method thereof, so as to at least achieve the effect of high window emissivity and high reflectivity without the need for an additional cover layer.

[0007] The objective of the present invention is achieved through the following technical solutions:

[0008] A high-performance rare earth-based radiation cooling coating, comprising a reflection enhancement layer and a radiation cooling layer;

[0009] The reflection enhancement layer comprises: water-based resin, metal powder filler, additives and water;

[0010] The radiation cooling layer comprises germanium oxide, niobium oxide, lanthanum oxide and selenium oxide.

[0011] Furthermore, the water-based resin includes water-based polyacrylic resin or polyurethane resin.

[0012] Furthermore, the auxiliary agent includes a leveling agent and a defoaming agent.

[0013] Furthermore, the metal powder filler includes at least one of aluminum powder, zinc powder, iron powder and magnesium powder.

[0014] Furthermore, the reflection enhancement layer comprises, by weight: 40-45 parts of water-based resin, 20-25 parts of metal powder filler, 5-10 parts of additives and 20-35 parts of water;

[0015] Furthermore, the radiation cooling layer comprises, by weight: 20-35 parts of germanium oxide, 25-36 parts of niobium oxide, 13-20 parts of lanthanum oxide and 16-35 parts of selenium oxide.

[0016] Furthermore, the weight ratio of the reflection enhancement layer to the radiation enhancement layer is 1:2.5.

[0017] The preparation method of the radiation cooling coating comprises the following steps:

[0018] S1: preparing a reflection enhancement layer coating: taking 20-25 parts of aluminum powder, 8-10 parts of an additive and 20-35 parts of water, and mixing them evenly, and then adding 40-45 parts of a water-based resin, and mixing evenly to obtain the reflection enhancement layer coating;

[0019] S2: preparing a radiation cooling layer coating: mixing 20-35 parts of germanium oxide, 25-36 parts of niobium oxide, 13-20 parts of lanthanum oxide and 16-35 parts of selenium oxide by weight, crushing the mixture, sintering the mixture at a high temperature, quenching the mixture in water and drying the mixture to obtain a coarse powder A;

[0020] The coarse powder A is added to a solvent for grinding to obtain slurry A1 with a D50 of 15-25 μm, slurry A2 with a D50 of 5-10 μm, and slurry A3 with a D50 of 0.3-0.7 μm respectively; the coarse powder A is prepared into an aqueous solution, ground to a particle size of 1-5 μm, then atomized and dried, and subjected to a second sintering at a high temperature, and the obtained powder is dispersed in a solvent to obtain slurry A4; the slurries A1, A2, A3 and A4 are mixed in a weight ratio of 1:1:0.5:0.15 to obtain the radiation cooling slurry;

[0021] By weight, 30 parts of the radiation cooling slurry, 40 parts of fluorocarbon resin or silicone resin, 5 parts of curing agent, 5-10 parts of general auxiliary agent and 20-30 parts of butyl acetate are mixed evenly to obtain the radiation cooling layer coating.

[0022] The curing agent is selected to be compatible with the fluorocarbon resin or the silicone resin.

[0023] Further, the solvent includes water or butyl acetate;

[0024] And / or, the solid content of the A1 slurry, A2 slurry, A3 slurry and A4 slurry is 30-40%.

[0025] Furthermore, the general auxiliary agent includes at least one of a leveling agent, a defoaming agent and a thickener.

[0026] Further, the reflection enhancement layer is a lower layer, which is coated on the surface of the object and contacts the object;

[0027] The radiation cooling layer is an upper layer, coated on the surface of the reflection enhancement layer, and does not contact with the object.

[0028] The beneficial effects of the present invention are:

[0029] The radiant cooling coating of the radiant cooling coating of the present invention has a reflectivity of 90%, an emissivity of 0.95, and a heat dissipation power of 100W / m at room temperature. 2 Above, the outdoor temperature drops by more than 5 degrees;

[0030] The radiation cooling paint of the present invention is suitable for building exterior walls and building roofs.

[0031] The bottom coating will also affect the coating's reflection effect on sunlight. When the bottom layer has good reflection performance, it can improve the surface layer's reflection performance of sunlight to a certain extent; otherwise, it will reduce the coating's reflection performance of sunlight. In actual applications, the building exterior walls and roof surfaces that usually need to be painted have lower reflection performance, such as red brick walls and black roofs that have been waterproofed. In the coating described in this patent, the reflection enhancement layer is used as the primer, which can minimize the impact of the building exterior wall and roof's own performance on the final performance of the coating. In addition, the reflection enhancement layer described in this patent can improve the overall reflection effect of the coating to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The UV-Vis-Infrared spectrophotometer in Example 1 was used for testing;

[0033] Figure 2 The reflectivity test result of the radiant cooling coating in Example 1;

[0034] Figure 3 This is a comparison chart of the temperature changes within one day between the wall surface coated with the radiant cooling coating in Example 1 and the wall surface not coated with the radiant cooling coating. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following.

[0036] Example 1

[0037] Take 20 parts of aluminum powder, 8 parts of BYK191 dispersant, 20 parts of water, and 2 parts of BYK7420 orientation rearrangement agent, and stir them thoroughly in water using a stirring plate to obtain a uniform aluminum powder slurry. Add 40 parts of waterborne polyurethane resin emulsion to the aluminum powder slurry in batches and stir thoroughly for 2 hours to obtain a uniform reflection enhancement layer coating. The coating layer thickness is 20μm. The reflectivity of the primer can be tested by a UV-visible-infrared spectrophotometer. The test results are as follows: Figure 1 As shown, the solar reflectivity is 80%.

[0038] Before preparing the radiation cooling coating, it is necessary to first calcine and prepare filler powder with radiation cooling effect. Take 20 parts of germanium oxide, 26 parts of niobium oxide, 16 parts of lanthanum oxide, and 30 parts of selenium oxide.

[0039] After the raw materials are fully mixed, a certain amount of water is added and wet-milled in a planetary ball mill. The ball mill speed is 400 rpm, the grinding time is 12 hours, and the ratio of large, medium and small balls is 3:4:3. The volume ratio of air in the cavity: liquid: ball is controlled at 1:1:1. After grinding, the grinding beads are filtered with a 40-mesh screen to obtain a coarsely ground slurry. The coarsely ground slurry is fully dried in a 90-degree oven to obtain a precursor sample that is agglomerated. The block precursor sample is put into a powder crusher again to obtain a uniformly mixed precursor powder. The precursor powder is loaded into a corundum crucible and heated in a smelting furnace. The temperature is increased from room temperature to 1400 degrees at a heating rate of 5 degrees per minute, and the temperature is maintained for 4 hours. The liquid is directly poured into water for cold quenching, and the powder in the water is filtered to obtain a coarse powder.

[0040] A total of 10 kg of a 40% coarse material powder solution was prepared, wherein the dispersant content was 12-15%, the dispersant was BYK111 type dispersant, and the solvent was butyl acetate. The solution was put into a sand mill at 1500-1600 rpm for sand grinding, the grinding ball particle size was 0.5 mm, and the slurry particle size was measured once every 15 minutes with a laser particle size analyzer, and slurry A1 with a D50 of 19.5 μm, slurry A2 with a D50 of 4.2 μm, and slurry A3 with a D50 of 0.63 μm were obtained respectively.

[0041] Use water as solvent, prepare a 40% coarse powder solution, add 13% BYK111 dispersant, grind the slurry in a sand mill, monitor the particle size until it is 1-10μm, and the actual D50 particle size after grinding is 3.2μm. After the slurry is atomized and dried, it is injected into a suspension sintering furnace, and the sintering degree is set to 1250 degrees. After sufficient sintering, spherical powder is obtained. The obtained spherical powder is reconfigured into a 30% solution, the solvent is butyl acetate, and 5% BYK111 dispersant is added again. Use a disc stirrer to fully stir to obtain A4 slurry. The four slurries are mixed in a mass ratio of A1:A2:A3:A4=1:1:0.5:0.15 to finally obtain a finished slurry.

[0042] Take 30 parts of the above-mentioned radiation cooling slurry, 40 parts of polyurethane resin, 5 parts of corresponding curing agent, 10 parts of general leveling and defoaming agent, and 20 parts of butyl acetate, and mix them evenly to obtain the finished coating. Apply it on the surface of the reflection enhancement layer with a thickness of 20μm. The average reflectivity of the radiation cooling coating is 94%, the emissivity is 0.95, and the heat dissipation power is 122W / m2 at room temperature. Compared with the unpainted wall, the temperature is reduced by more than 4 degrees.

[0043] In addition, in order to highlight the experimental effect of the reflection enhancement layer, this patent also applies a radiation cooling coating on the surface of common red bricks. Specifically, the common outdoor red bricks are used as the coating surface, and the reflection enhancement layer is first applied with a thickness of 20μm. After the resin layer is completely dry, the radiation cooling coating is applied again on the surface with a thickness of 10-20μm. After the resin layer is completely dry, the average reflectivity of the coating is 89.5% and the emissivity is 0.95.

[0044] Example 2

[0045] Take 25 parts of aluminum powder, 8 parts of BYK191 dispersant, 35 parts of water, and 2 parts of BYK7420 orientation rearrangement agent, and stir them in water with a stirring plate to obtain a uniform aluminum powder slurry. Add 45 parts of waterborne polyurethane resin emulsion to the aluminum powder slurry in batches and stir them for 2 hours to obtain a uniform reflection enhancement layer coating. The coating layer thickness is 20μm, and the primer reflectivity can be tested by UV-visible-infrared spectrophotometer.

[0046] Before preparing the radiation cooling coating, it is necessary to first calcine and prepare filler powder with radiation cooling effect. Take 35 parts of germanium oxide, 35 parts of niobium oxide, 20 parts of lanthanum oxide, and 16 parts of selenium oxide.

[0047] After the raw materials are fully mixed, a certain amount of water is added and wet-milled in a planetary ball mill. The ball mill speed is 400 rpm, the grinding time is 12 hours, and the ratio of large, medium and small balls is 3:4:3. The volume ratio of air in the cavity: liquid: ball is controlled at 1:1:1. After grinding, the grinding beads are filtered with a 40-mesh screen to obtain a coarsely ground slurry. The coarsely ground slurry is fully dried in a 90-degree oven to obtain a precursor sample that is agglomerated. The block precursor sample is put into a powder crusher again to obtain a uniformly mixed precursor powder. The precursor powder is loaded into a corundum crucible and heated in a smelting furnace. The temperature is increased from room temperature to 1400 degrees at a heating rate of 5 degrees per minute, and the temperature is maintained for 4 hours. The liquid is directly poured into water for cold quenching, and the powder in the water is filtered to obtain a coarse powder.

[0048] A total of 10 kg of a 40% coarse material powder solution was prepared, wherein the dispersant content was 12-15%, the dispersant was BYK111 type dispersant, and the solvent was butyl acetate. The solution was put into a sand mill at 1500-1600 rpm for sand grinding, the grinding ball particle size was 0.5 mm, and the slurry particle size was measured once every 15 minutes with a laser particle size analyzer, and slurry A1 with a D50 of 19.5 μm, slurry A2 with a D50 of 4.2 μm, and slurry A3 with a D50 of 0.63 μm were obtained respectively.

[0049] Use water as solvent, prepare a 40% coarse powder solution, add 13% BYK111 dispersant, grind the slurry in a sand mill, monitor the particle size until it is 1-10μm, and the actual D50 particle size after grinding is 3.2μm. After the slurry is atomized and dried, it is injected into a suspension sintering furnace, and the sintering degree is set to 1250 degrees. After sufficient sintering, spherical powder is obtained. The obtained spherical powder is reconfigured into a 30% solution, the solvent is butyl acetate, and 5% BYK111 dispersant is added again. Use a disc stirrer to fully stir to obtain A4 slurry. The four slurries are mixed in a mass ratio of A1:A2:A3:A4=1:0.8:0.:6:0.1 to finally obtain a finished slurry.

[0050] Take 30 parts of the above-mentioned radiation cooling slurry, 40 parts of polyurethane resin, 5 parts of corresponding curing agent, 10 parts of leveling and defoaming agent, and 30 parts of butyl acetate, and mix them evenly to obtain the finished coating. Apply it on the surface of the reflection enhancement layer with a thickness of 20μm. The reflectivity of the radiation cooling coating is 94.3%, the emissivity is 0.95, and the heat dissipation power is 122W / m2 at room temperature. Compared with the unpainted wall, the temperature is reduced by more than 4 degrees.

[0051] In addition, in order to highlight the experimental effect of the reflection enhancement layer, this patent also applies a radiation cooling coating on the surface of common red bricks. Specifically, the common outdoor red bricks are used as the coating surface, and the reflection enhancement layer is first applied with a thickness of 20μm. After the resin layer is completely dry, the radiation cooling coating is applied again on the surface with a thickness of 10-20μm. After the resin layer is completely dry, the average reflectivity of the coating is 90.2% and the emissivity is 0.95.

[0052] Comparative Example 1

[0053] The specific method for preparing the commonly used solar reflective filler - titanium dioxide slurry is as follows:

[0054] Take 30 parts of rutile titanium dioxide filler, add 60 parts of water and 8 parts of BYK111 dispersant. After mixing evenly, wet grind in a planetary ball mill, the ball mill speed is 400 rpm, the grinding time is 12-16 hours, the ratio of large, medium and small balls is 3:4:3, and the volume ratio of air: liquid: ball in the cavity is controlled at 1:1:1. After grinding, filter the grinding beads with a 40-mesh screen to obtain a coarsely ground mixed slurry, and then put the obtained mixed slurry into a sand mill for grinding. Use 5mm grinding balls, control the sand mill speed to 1000-1500 rpm, monitor the particle size every half an hour, until the D50 particle size is 0.5-1 micron, stop grinding, and obtain titanium dioxide slurry. Put 30 parts of titanium dioxide slurry, 30 parts of acrylic resin, 10 parts of glass beads, 5 parts of general additives (including 2 parts of BYK111 dispersant, 2 parts of general leveling agent, and 1 part of defoaming agent), and 20 parts of water in the stirrer, control the stirrer speed to 200 rpm, and stir for 6 hours to obtain the final finished coating.

[0055] During the painting process, aluminum sheets and common red bricks are used as base materials, and paint is applied on their surfaces with a thickness of 20-30μm.

[0056] Comparative Example 2

[0057] The preparation method of the radiation cooling coating is the same as that of comparative example 1, and the difference from comparative example 1 is that a transparent overcoat layer is applied again on the surface of the radiation cooling coating. The preparation method of the overcoat layer is as follows: 30 parts of polyurethane resin, 5 parts of resin matching curing agent, and 40 parts of butyl acetate are mixed thoroughly to form the overcoat layer.

[0058] The painting process is the same as that of comparative example 1, and the substrate is also selected from aluminum sheets and common red brick surfaces. The thickness of the functional layer is 20-30 μm, and after the functional layer is completely dried, the topcoat is applied with a thickness of 10 μm.

[0059] Comparative Example 3

[0060] A rare earth-based radiation cooling coating is prepared, and the method is the same as that in the embodiment, except that it does not include a reflection enhancement layer, but only includes a radiation cooling layer, as follows

[0061] Take 25 parts of germanium oxide, 28 parts of niobium oxide, 16 parts of lanthanum oxide, and 30 parts of selenium oxide. Here, the natural unseparated mixture of lanthanum oxide and cerium oxide is the upstream raw material for producing lanthanum oxide and cerium oxide, which has a lower cost than lanthanum oxide and cerium oxide.

[0062] After the raw materials are fully mixed, a certain amount of water is added and wet-milled in a planetary ball mill. The ball mill speed is 400 rpm, the grinding time is 12 hours, and the ratio of large, medium and small balls is 3:4:3. The volume ratio of air in the cavity: liquid: ball is controlled at 1:1:1. After grinding, the grinding beads are filtered with a 40-mesh screen to obtain a coarsely ground slurry. The coarsely ground slurry is fully dried in a 90-degree oven to obtain a precursor sample that is agglomerated. The block precursor sample is put into a powder crusher again to obtain a uniformly mixed precursor powder. The precursor powder is loaded into a corundum crucible and heated in a smelting furnace. The temperature is increased from room temperature to 1400 degrees at a heating rate of 5 degrees per minute, and the temperature is maintained for 4 hours. The liquid is directly poured into water for cold quenching, and the powder in the water is filtered to obtain a coarse powder.

[0063] A total of 10 kg of a 40% coarse material powder solution was prepared, wherein the dispersant content was 12-15%, the dispersant was BYK111 type dispersant, and the solvent was butyl acetate. The solution was put into a sand mill at 1500-1600 rpm for sand grinding, the grinding ball particle size was 0.5 mm, and the slurry particle size was measured once every 15 minutes with a laser particle size analyzer, and slurry A1 with a D50 of 19.5 μm, slurry A2 with a D50 of 4.2 μm, and slurry A3 with a D50 of 0.63 μm were obtained respectively.

[0064] Use water as solvent, prepare a 40% coarse powder solution, add 13% BYK111 dispersant, grind the slurry in a sand mill, monitor the particle size until it is 1-10μm, and the actual D50 particle size after grinding is 3.2μm. After the slurry is atomized and dried, it is injected into a suspension sintering furnace, and the sintering degree is set to 1250 degrees. After sufficient sintering, spherical powder is obtained. The obtained spherical powder is reconfigured into a 30% solution, the solvent is butyl acetate, and 5% BYK111 dispersant is added again. Use a disc stirrer to fully stir to obtain A4 slurry. The four slurries are mixed in a mass ratio of A1:A2:A3:A4=1:1:0.5:0.15 to finally obtain a finished slurry.

[0065] Take 30 parts of the above radiation cooling slurry, 40 parts of fluorocarbon or silicone resin, 5 parts of corresponding curing agent, 10 parts of leveling and defoaming agent, and 20 parts of butyl acetate, and mix them evenly to obtain the finished coating. Apply it on the surface of aluminum sheet and red brick with a thickness of 20μm. The reflectivity of the radiation cooling coating is 82%, and the emissivity is 0.88. Due to the poor performance, the radiation cooling function cannot be realized under the sun.

[0066] Experimental example

[0067] After the coatings of Example 1, Comparative Examples 1 and 2 were applied on the surfaces of aluminum sheets and red bricks, the reflectivity of the coatings and the window emissivity were statistically measured, wherein the reflectivity was detected by an ultraviolet-visible-infrared spectrophotometer, and the window emissivity was detected by an IR-1 hemispherical emissivity tester (the average value was recorded).

[0068] In addition, the anti-aging properties of the coatings of Examples 1 and 2 and Comparative Examples 1 and 2 were tested, and the specific method was as follows:

[0069] The test was conducted using a high temperature and high humidity xenon lamp aging tester. The humidity was controlled at 85%. The xenon lamp was used to directly irradiate the sample surface. The sample status was observed every 20-30 hours. The sample status included yellowing, delamination, powdering, etc., and the coating surface status was recorded.

[0070] The experimental data are shown in the following table

[0071]

[0072] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A high-performance rare earth-based radiation cooling coating, characterized in that: including a reflection enhancement layer and a radiation cooling layer; The reflection enhancement layer comprises: water-based resin, metal powder filler, additives and water; The radiation cooling layer comprises: germanium oxide, niobium oxide, lanthanum oxide and selenium oxide; The metal powder filler includes at least one of aluminum powder, zinc powder, iron powder and magnesium powder; The preparation method of the radiation cooling coating comprises the following steps: S1: preparing a reflection enhancement layer coating: taking 20-25 parts of aluminum powder, 8-10 parts of an additive and 20-35 parts of water, and mixing them evenly, and then adding 40-45 parts of a water-based resin, and mixing evenly to obtain the reflection enhancement layer coating; S2: preparing a radiation cooling layer coating: mixing 20-35 parts of germanium oxide, 25-36 parts of niobium oxide, 13-20 parts of lanthanum oxide and 16-35 parts of selenium oxide by weight, crushing the mixture, sintering the mixture at a high temperature, quenching the mixture in water and drying the mixture to obtain a coarse powder A; The coarse powder A is added to a solvent for grinding to obtain slurry A1 with a D50 of 15-25 μm, slurry A2 with a D50 of 5-10 μm, and slurry A3 with a D50 of 0.3-0.7 μm respectively; the coarse powder A is prepared into an aqueous solution, ground to a particle size of 1-5 μm, then atomized and dried, and subjected to a second sintering at a high temperature, and the obtained powder is dispersed in a solvent to obtain slurry A4; the slurries A1, A2, A3 and A4 are mixed in a weight ratio of 1:1:0.5:0.15 to obtain the radiation cooling slurry; By weight, 30 parts of the radiation cooling slurry, 40 parts of fluorocarbon resin or silicone resin, 5 parts of curing agent, 5-10 parts of general auxiliary agent and 20-30 parts of butyl acetate are mixed evenly to obtain the radiation cooling layer coating.

2. The refrigeration coating according to claim 1, characterized in that: The water-based resin includes water-based polyacrylic resin or polyurethane resin.

3. The refrigeration coating according to claim 1, characterized in that: The auxiliary agent includes at least one of a leveling agent, a defoaming agent and an orientation rearrangement agent.

4. The refrigeration coating according to claim 1, characterized in that: The reflection enhancement layer comprises, by weight, 40-45 parts of water-based resin, 20-25 parts of metal powder filler, 5-10 parts of auxiliary agent and 20-35 parts of water.

5. The refrigeration coating according to claim 1, characterized in that: The weight ratio of the reflection enhancement layer to the radiation enhancement layer is 1:2.

5.

6. The refrigeration coating according to claim 1, characterized in that: The universal auxiliary agent includes at least one of a leveling agent, a defoaming agent and a thickener.

7. The method for using the radiant cooling coating according to any one of claims 1 to 6, characterized in that: The reflection enhancement layer is a lower layer, which is coated on the surface of the object and contacts the object; The radiation cooling layer is an upper layer, coated on the surface of the reflection enhancement layer, and does not contact with the object.