A 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment and its preparation method and application

Through electric arc furnace smelting and vacuum refining furnace refining processes, carbon and oxygen co-injection and composite deoxidizer technology are used to improve the inclusion level of 05Cr17Ni4Cu4Nb stainless steel, solving the problem of insufficient inclusion levels in the existing technology and meeting the requirements of ultra-thin film meet the high performance requirements of ship power equipment.

CN118007012BActive Publication Date: 2024-10-15ZHEJIANG DALONG ALLOY STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410349254.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-10-15
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

The inclusion level of existing 05Cr17Ni4Cu4Nb stainless steel cannot meet the high requirements of ultra-thin film ship power equipment, especially in terms of low-temperature impact performance, which fails to meet the 10J standard.

Method used

The electric arc furnace smelting and vacuum refining furnace refining processes are used to promote inclusions by adding carbon and oxygen to co-inject foam slag during the melting period and using composite deoxidants including Al, 7Al2O3·12CaO, CaCO3, Fe, CaF2 and Mn during the reduction period. The floating removal of substances and gases improves the purification effect of stainless steel.

Benefits of technology

The inclusion grade of 05Cr17Ni4Cu4Nb stainless steel has been significantly improved, enabling it to meet the application requirements in the field of ultra-thin plates. The inclusion grade reaches A≤0.5, B≤1.0, C≤0.5, D≤1.0, Ds≤1.5, which meets the low temperature impact performance. Require.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005028905340000141
    Figure GDA0005028905340000141
Patent Text Reader

Abstract

The present invention provides a 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment and a preparation method and application thereof, belonging to the field of metallurgical technology. The present invention adopts an oxidation method for smelting, adds a slag-making agent during the smelting and melting period, and simultaneously sprays carbon and oxygen to form foam slag, fully utilizing the intense reaction and boiling of C-O during the oxidation period, promoting the floating of inclusions and gases and removing them with the slag flow, thereby achieving the effect of purifying molten steel; adding a composite deoxidizer during the reduction period, compared with other deoxidizers in the prior art, can further improve the grade of stainless steel inclusions; by adding Mn and CaF2, a synergistic effect can be formed with the 7Al2O3·12CaO pre-melted slag, thereby further improving the deoxidation effect, and then improving the inclusion grade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment, and a preparation method and application thereof. Background Art

[0002] 05Cr17Ni4Cu4Nb stainless steel is the main material for key parts in the fields of electromechanics and electronics. Due to its high strength and strong corrosion resistance, it is widely used in the fields of shipbuilding, energy and power equipment design and manufacturing. However, when used for special equipment for underwater power of ships (ultra-thin film processing parts ≤2mm), the inclusion level of 05Cr17Ni4Cu4Nb stainless steel is required to meet the requirements of A≤0.5, B≤1.0, C≤1.0, and D≤1.0. Under the H1150M heat treatment condition, the low-temperature impact requirement of -80℃ is greater than 10J. However, the inclusion level of the currently prepared 05Cr17Ni4Cu4Nb stainless steel is A≤2, B≤2, and C≤2.5, which is difficult to meet the use requirements. Therefore, how to improve the inclusion level of 05Cr17Ni4Cu4Nb stainless steel has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0003] The purpose of the present invention is to provide a 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment and its preparation method and application. The preparation method provided by the present invention can greatly improve the inclusion level of 05Cr17Ni4Cu4Nb stainless steel for ultra-thin diaphragm plate material, so that it can meet the application of ultra-thin plate field.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment, comprising the following steps:

[0006] (1) smelting scrap steel in an electric arc furnace to obtain molten steel;

[0007] (2) refining the molten steel obtained in step (1) in a vacuum refining furnace to obtain refined molten steel;

[0008] (3) pouring and heat treating the refined molten steel obtained in step (2) in sequence to obtain 05Cr17Ni4Cu4Nb stainless steel ingots for ultra-thin diaphragm ship power equipment;

[0009] The electric arc furnace smelting in step (1) comprises a melting period, an oxidation period and a reduction period which are carried out in sequence;

[0010] During the melting period, a slag-making agent is added and carbon and oxygen are co-sprayed to form foamed slag;

[0011] The oxidation period is carried out under oxygen blowing conditions;

[0012] During the reduction period, alloy raw materials and composite deoxidizer are added;

[0013] The composite deoxidizer comprises the following components in mass percentage: 40-50% Al, 1-3% 7Al2O3·12CaO, 5-8% CaCO3, 10-20% Fe, 20-30% CaF2 and 1-3% Mn.

[0014] Preferably, the carbon injection amount during the co-injection of carbon and oxygen is 3-8 kg / t; and the time for the co-injection of carbon and oxygen to form the foamed slag is 8-10 minutes.

[0015] Preferably, the pressure of the oxygen blowing is 1-2 MPa.

[0016] Preferably, during the reduction period, thin slag material, deoxidizer, alloy raw material, reducing agent and composite deoxidizer are added in sequence.

[0017] Preferably, the thin slag material includes lime and fluorite; the deoxidizer includes silicon manganese and ferromanganese; the alloy raw material includes ferrochrome and nickel plate; and the reducing agent includes at least one of ferrosilicon powder, calcium carbide, carbon powder and AD powder.

[0018] Preferably, the composite deoxidizer comprises the following components in mass percentage: Al 42-48%, 7Al2O3·12CaO 1.5-2.5%, CaCO3 6-7%, Fe 12-18%, CaF2 22-28% and Mn 1.5-2.5%.

[0019] Preferably, the vacuum refining furnace refining in step (2) includes a VOD stage, a VCD stage, a VOH stage and a VD stage performed in sequence.

[0020] Preferably, in step (3), the pouring temperature is 1550° C., the pouring flow rate is 1 to 2 t / min, and the pouring is performed under argon protection.

[0021] The present invention also provides a 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment prepared by the preparation method described in the above technical solution.

[0022] The present invention also provides the use of the 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment described in the above technical solution in the diaphragm of ship power equipment.

[0023] The invention provides a method for preparing a 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment, comprising the following steps: subjecting scrap steel to electric arc furnace smelting to obtain molten steel; subjecting the molten steel to vacuum refining furnace refining to obtain refined molten steel; subjecting the refined molten steel to sequential pouring and heat treatment to obtain a 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment; the electric arc furnace smelting comprises a melting period, an oxidation period and a reduction period performed sequentially; during the melting period, a slag-forming agent is added and carbon and oxygen are co-sprayed to form foamed slag; the oxidation period is performed under oxygen blowing conditions; during the reduction period, alloy raw materials and a composite deoxidizer are added; the composite deoxidizer comprises the following components in mass percentage: 40-50% Al, 1-3% 7Al2O3·12CaO, 5-8% CaCO3, 10-20% Fe, 20-30% CaF2 and 1-3% Mn. The present invention adopts oxidation method for smelting, adds slag-making agent in the smelting melting period, and simultaneously sprays carbon and oxygen to form foam slag, fully utilizes the intense reaction and boiling of CO in the oxidation period, promotes the floating of inclusions and gas and removes them with the slag flow, so as to achieve the effect of purifying molten steel; adds composite deoxidizer in the reduction period, and can further improve the grade of stainless steel inclusions compared with other deoxidizers in the prior art; wherein, metal aluminum is used as deoxidizer, 7Al2O3·12CaO can quickly adsorb the deoxidation product Al2O3 inclusions, and at the same time form large inclusions to float up removal; calcium carbonate is decomposed into CaO at high temperature, reacts with the deoxidation product Al2O3 inclusion to form low melting point CaO-Al2O3 inclusion, modifies the inclusion and forms large inclusions to float up and remove quickly, and its rapid decomposition is conducive to slag formation; Fe increases the density of the composite deoxidizer to prevent it from floating up quickly in the molten steel and reducing its deoxidation effect; by adding Mn and CaF2, it can form a synergistic effect with 7Al2O3·12CaO pre-melted slag, thereby further improving the deoxidation effect and further improving the inclusion grade. Experimental results show that the inclusion grade of the 05Cr17Ni4Cu4Nb stainless steel ingot prepared by the present invention is A≤0.5, B≤1.0, C≤0.5, D≤1.0, Ds≤1.5. DETAILED DESCRIPTION

[0024] The present invention provides a method for preparing 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment, comprising the following steps:

[0025] (1) smelting scrap steel in an electric arc furnace to obtain molten steel;

[0026] (2) refining the molten steel obtained in step (1) in a vacuum refining furnace to obtain refined molten steel;

[0027] (3) pouring and heat treating the refined molten steel obtained in step (2) in sequence to obtain 05Cr17Ni4Cu4Nb stainless steel ingots for ultra-thin diaphragm ship power equipment;

[0028] The electric arc furnace smelting in step (1) comprises a melting period, an oxidation period and a reduction period which are carried out in sequence;

[0029] During the melting period, a slag-making agent is added and carbon and oxygen are co-sprayed to form foamed slag;

[0030] The oxidation period is carried out under oxygen blowing conditions;

[0031] During the reduction period, alloy raw materials and composite deoxidizer are added;

[0032] The composite deoxidizer comprises the following components in mass percentage: 40-50% Al, 1-3% 7Al2O3·12CaO, 5-8% CaCO3, 10-20% Fe, 20-30% CaF2 and 1-3% Mn.

[0033] Unless otherwise specified, the present invention has no particular limitation on the sources of the raw materials used, and the raw materials may be prepared using commercially available products or well-known preparation methods known to those skilled in the art.

[0034] The invention smelts scrap steel in an electric arc furnace to obtain molten steel.

[0035] In the present invention, the mass percentage of S in the scrap steel is preferably ≤0.020%; the mass percentage of P in the scrap steel is preferably ≤0.020%. The present invention can further improve the inclusion grade by using pure scrap steel with S≤0.020% and P≤0.020%.

[0036] In the present invention, the electric arc furnace smelting includes a melting period, an oxidation period and a reduction period which are performed in sequence.

[0037] In the present invention, a slag-forming agent is added during the melting period and carbon and oxygen are co-sprayed to form foamed slag.

[0038] In the present invention, the slag-forming agent is preferably FeO; the mass of the slag-forming agent is preferably 2-4% of the mass of the molten steel; the slag-forming agent is preferably added when the temperature of the molten steel is 1560° C. In the present invention, the FeO is beneficial to dephosphorization, promoting the floating of inclusions and gases and their removal with the slag.

[0039] In the present invention, the carbon spraying amount during the carbon and oxygen co-spraying is preferably 3-8 kg / t, more preferably 5 kg / t; the time for the carbon and oxygen co-spraying to form foamed slag is preferably 8-10 min; the carbon and oxygen co-spraying is preferably started when the molten steel temperature is 1560°C; the oxygen flow rate during the carbon and oxygen co-spraying is preferably 7-8 cum / min; the carbon and oxygen co-spraying is preferably carried out by blowing oxygen with an oxygen blowing tube. The present invention has no special limitation on the carbon spraying flow rate during the carbon and oxygen co-spraying, and it can be sprayed within the above time. The present invention implements carbon and oxygen co-spraying at the end of the melting period, which can produce a strong carbon-oxygen reaction, causing the molten steel to boil, and the impurities in the molten steel to fully float, further achieving the effect of purifying the molten steel.

[0040] In the present invention, it is preferred that the oxidation stage is entered when the temperature of the molten steel is 1600-1650°C.

[0041] In the present invention, the oxidation period is carried out under oxygen blowing conditions; the oxygen blowing pressure is preferably 1-2 MPa, more preferably 1.5 MPa; the boiling time of the molten steel in the oxidation period is preferably 5-7 minutes. The present invention adopts an oxygen-enriched dephosphorization process in the initial oxidation stage, and performs oxidative decarburization when the molten steel is boiling to remove gas and inclusions in the molten steel.

[0042] In the present invention, Mn is preferably added after the molten steel has been boiling for 5 to 7 minutes; the mass of the Mn is preferably 0.2% of the mass of the molten steel. The addition of manganese in the present invention can enable pre-deoxidation.

[0043] In the present invention, the decarburization amount in the oxidation period is preferably ≥40%; when the C content in the molten steel is 0.80-1.0wt%, P≤0.015wt%, and the molten steel temperature is 1670-1720°C, it is preferably entered into the reduction period.

[0044] In the present invention, after the oxidation period, the molten steel is preferably deslagging. The present invention has no particular limitation on the deslagging operation, and the operation well known to those skilled in the art can be adopted.

[0045] In the present invention, alloy raw materials and composite deoxidizer are added during the reduction period, and preferably thin slag, deoxidizer, alloy raw materials, reducing agent and composite deoxidizer are added in sequence.

[0046] In the present invention, the thin slag material preferably includes lime and fluorite. The present invention has no special limitation on the amount of the thin slag material, and the C content can be adjusted to 1.0wt%. The present invention has no special limitation on the timing of adding the thin slag material, and the thin slag material can be added during the reduction period.

[0047] In the present invention, the deoxidizer preferably includes silicon manganese and ferromanganese; the content of silicon manganese is preferably 3-8 kg / t, more preferably 5 kg / t; the content of ferromanganese is preferably 3-8 kg / t, more preferably 5 kg / t. The present invention has no special limitation on the timing of adding the deoxidizer, and it can be judged according to common sense.

[0048] In the present invention, the alloy raw materials preferably include ferrochrome and nickel plate. The present invention has no special limitation on the amount of ferrochrome, and ferrochrome can be added at [Cr] = 15wt%; the present invention has no special limitation on the amount of nickel plate, and nickel plate can be added at [Ni] = 3wt%.

[0049] In the present invention, the reducing agent preferably includes at least one of ferrosilicon powder, calcium carbide, carbon powder and AD powder; the content of the ferrosilicon powder is preferably 3-8 kg / t, more preferably 5 kg / t; the content of the calcium carbide is preferably 2-3 kg / t; the content of the carbon powder is preferably 0.5-2 kg / t, more preferably 1 kg / t; the content of the AD powder is preferably 5-8 kg / t. In the present invention, ferrosilicon powder, calcium carbide, carbon powder and AD powder are used to make white slag for deoxidation.

[0050] In the present invention, the retention time of the white slag after adding the reducing agent to make the white slag is preferably 15 to 25 minutes, more preferably 20 minutes. In the present invention, the reducing agent is preferably added after the thin slag is made. In the present invention, the white slag is kept for the above time after making the white slag to fully perform reduction and deoxidation.

[0051] In the present invention, the composite deoxidizer comprises the following components in mass percentage: Al 40-50%, 7Al2O3·12CaO 1-3%, CaCO3 5-8%, Fe 10-20%, CaF2 20-30% and Mn 1-3%, preferably Al 42-48%, 7Al2O3·12CaO 1.5-2.5%, CaCO3 6-7%, Fe 12-18%, CaF2 22-28% and Mn 1.5-2.5%, more preferably Al 45-46%, 7Al2O3·12CaO 2%, CaCO3 6.5%, Fe 13-15%, CaF2 25-26% and Mn 2%. The present invention adds a composite deoxidizer during the reduction period, which can further improve the grade of stainless steel inclusions compared with other deoxidizers in the prior art; wherein, metal aluminum is used as a deoxidizer, 7Al2O3·12CaO can quickly adsorb deoxidation product Al2O3 inclusions, and at the same time form large inclusions that float up for removal; calcium carbonate is decomposed into CaO at high temperature, reacts with deoxidation product Al2O3 inclusions to form low-melting-point CaO-Al2O3 inclusions, modifies inclusions and forms large inclusions that float up for removal quickly, and at the same time, its rapid decomposition is conducive to slag formation; Fe increases the density of the composite deoxidizer to prevent it from floating up quickly in molten steel and reducing its deoxidation effect; by adding Mn and CaF2, a synergistic effect can be formed with the 7Al2O3·12CaO pre-molten slag, thereby further improving the deoxidation effect and further improving the inclusion grade.

[0052] In the present invention, the content of the composite deoxidizer is preferably 5-10 kg / t, more preferably 8 kg / t. The present invention can further improve the deoxidation effect by controlling the content of the composite deoxidizer, thereby further improving the inclusion grade.

[0053] The present invention has no special limitation on the preparation method of the composite deoxidizer, as long as the raw materials are mixed uniformly.

[0054] In the present invention, the composite deoxidizer is preferably added 10 minutes before the molten steel is transferred into the ladle.

[0055] In the present invention, when the composition of the molten steel meets the required requirements and the temperature of the molten steel is 1700°C, the molten steel is preferably transferred into a ladle, and then the slag in the ladle is skimmed to obtain the molten steel.

[0056] The present invention has no special limitation on the operation of transferring the molten steel into the ladle, and the operation well known to those skilled in the art can be adopted.

[0057] In the present invention, the slagging in the ladle is preferably performed until the residue amount is ≤1.5kg / t.

[0058] In the present invention, when the temperature of the molten steel is 1650° C., the molten steel is preferably refined in a vacuum refining furnace.

[0059] After obtaining the molten steel, the present invention refines the molten steel in a vacuum refining furnace to obtain refined molten steel. Compared with the traditional VOD stainless steel smelting, the vacuum refining furnace (VODC) refining of the present invention reduces the LF (ladle furnace smelting) treatment process before VOD, can improve the quality of molten steel, remove gas and inclusions in the molten steel, add necessary alloys, adjust the temperature and homogenize the composition; can also improve the productivity of the primary melting furnace, and move the operation in the low-load operation state in the primary melting furnace to the outside of the furnace; can improve the operational flexibility, shorten the smelting cycle, reduce the smelting cost, and the VODC stainless steel refining is carried out in a vacuum environment throughout the process, which prolongs the vacuum treatment time of the molten steel and can significantly reduce the content of harmful gas elements and inclusions in the steel.

[0060] In the present invention, the vacuum refining furnace refining preferably includes a VOD stage, a VCD stage, a VOH stage and a VD stage performed in sequence.

[0061] In the present invention, the temperatures of the VOD stage, the VCD stage, the VOH stage and the VD stage are preferably independently 1650-1680°C.

[0062] In the present invention, the vacuum degree of the VOD stage is preferably 80-120 mbar; the VOD stage is preferably top-blown oxygen and bottom-blown argon; the oxygen blowing amount of the VOD stage is preferably 450-650 mbar. 3 / h, more preferably 500 to 550 m 3 / h; the argon blowing amount in the VOD stage is preferably 3 to 6m 3 / h, more preferably 4 to 5m 3 / h. The present invention has no special limitation on the duration of the VOD stage, as long as the carbon content in the molten steel is below 0.03wt%. The VOD stage of the present invention is a vacuum oxygen blowing decarburization process.

[0063] In the present invention, the vacuum degree of the VCD stage is preferably 1-5 mbar; the vacuum pumping time of the VCD stage is preferably 8-10 min; the VCD stage is preferably bottom-blown argon; the argon flow rate of the VCD stage is preferably 3-6 m 3 / h.

[0064] In the present invention, the slag is preferably added in sequence in the VCD stage; the slag is preferably lime and fluorite; the content of the lime is preferably 15-23 kg / t, more preferably 20 kg / t; the content of the fluorite is preferably 1-5 kg / t, more preferably 3 kg / t. The present invention has no special limitation on the time of the VCD stage, and conventional judgment can be made based on factors such as the measured temperature (1650-1700°C), the amount of alloy added, and the steel pouring temperature (1500-1600°C). The VCD stage of the present invention is a vacuum carbon deoxidation process.

[0065] In the present invention, the vacuum degree of the VOH stage is preferably 350-450 mbar, more preferably 380-420 mbar; the VOH stage is preferably top-blown oxygen and bottom-blown argon; the oxygen flow rate of the VOH stage is preferably 450-550 mbar. 3 / h, more preferably 480-520m 3 / h; the argon flow rate in the VOH stage is preferably 3 to 6m 3 / h, more preferably 4 to 5m 3 / h; the VOH stage preferably adopts aluminum addition to increase the temperature; when the aluminum is added to 1% of the mass of the molten steel, the temperature of the molten steel is preferably increased by 250%. The present invention has no special limitation on the time of the VOH stage, and it can be judged according to common sense. The VOH stage of the present invention is a vacuum oxygen blowing heating and temperature raising process.

[0066] In the present invention, the vacuum degree of the VD stage is preferably ≤2.0 mbar; the VD stage is preferably bottom-blown argon; the argon flow rate of the VD stage is preferably 4.5-6 m 3 / h, more preferably 5 to 5.5 m 3 The present invention has no special limitation on the duration of the VD stage, as long as the ingredients meet the specified requirements.

[0067] After the refining in the vacuum refining furnace is completed, the present invention preferably performs component fine-tuning, steel tapping and calming in sequence on the molten steel obtained by the vacuum refining furnace to obtain refined molten steel.

[0068] In the present invention, the composition fine-tuning is preferably performed by adding a pre-baked alloy. The present invention has no limitation on the type of the alloy, and the alloy can be selected according to the required composition.

[0069] In the present invention, the steel tapping is preferably carried out in bottom blowing of argon. The present invention has no special limitation on the operation of the steel tapping, and the operation well known to those skilled in the art can be adopted. In the present invention, argon is blown in the ladle to fully float the inclusions in the molten steel.

[0070] In the present invention, the sedation time is preferably 5 to 7 minutes.

[0071] After obtaining the refined molten steel, the present invention sequentially casts and heat-treats the refined molten steel to obtain 05Cr17Ni4Cu4Nb stainless steel ingots for ultra-thin diaphragm ship power equipment.

[0072] In the present invention, the pouring system is preferably inspected before pouring. The present invention has no special limitation on the operation of the pouring system inspection, as long as it is ensured to be dry and free of moisture, and the pouring channel and the steel mold are clean and free of pollution.

[0073] In the present invention, the pouring temperature is preferably 1550°C; the pouring flow rate is preferably 1-2 t / min; the pouring is preferably carried out under argon protection; the argon flow rate is preferably 5-10 L / min. The present invention adopts argon protection pouring to prevent secondary oxidation.

[0074] After the pouring is completed, the present invention preferably demoulds the product obtained by pouring.

[0075] In the present invention, the demoulding time is preferably (0.112R 2 / 60)h, where R is the maximum radius of the steel ingot, in cm.

[0076] In the present invention, the heat treatment is preferably annealing treatment; the temperature of the heat treatment is preferably 650-700°C; the holding time of the heat treatment is preferably 0.8-1 min / mm; the cooling method of the heat treatment is preferably furnace cooling and air cooling in sequence; the terminal temperature of the furnace cooling is preferably ≤500°C. The present invention has no special restrictions on the operation of the furnace cooling and air cooling, and the operation well known to those skilled in the art can be adopted.

[0077] The present invention adopts oxidation method for smelting, adds slag-making agent in the smelting melting period, and simultaneously sprays carbon and oxygen to form foam slag, fully utilizes the intense reaction and boiling of CO in the oxidation period, promotes the floating of inclusions and gas and removes them with the slag flow, so as to achieve the effect of purifying molten steel; adds composite deoxidizer in the reduction period, and can further improve the grade of stainless steel inclusions compared with other deoxidizers in the prior art; wherein, metal aluminum is used as deoxidizer, 7Al2O3·12CaO can quickly adsorb the deoxidation product Al2O3 inclusions, and at the same time form large inclusions to float up removal; calcium carbonate is decomposed into CaO at high temperature, which reacts with the deoxidation product Al2O3 inclusion to form low-melting-point CaO-Al2O3 inclusions, which modify the inclusions and form large inclusions that float up and are removed quickly. At the same time, its rapid decomposition is conducive to slag formation; Fe increases the density of the composite deoxidizer to prevent it from floating up quickly in the molten steel and reducing its deoxidation effect; by adding Mn and CaF2, a synergistic effect can be formed with the 7Al2O3·12CaO pre-molten slag, thereby further improving the deoxidation effect and thus improving the inclusion grade.

[0078] The present invention also provides a 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment prepared by the preparation method described in the above technical solution.

[0079] In the present invention, the composition of the 05Cr17Ni4Cu4Nb stainless steel ingot preferably includes, by mass percentage, C0.047-0.060%, Si≤0.50%, Mn 0.50-0.80%, Cr 15.50-16.50%, Ni 3.25-4.50%, Nb 0.23-0.38%, Cu 3.20-4.50%, S≤0.010%, P≤0.025% and the balance Fe.

[0080] The 05Cr17Ni4Cu4Nb stainless steel ingot provided by the invention has a high inclusion grade, so that it can meet the application in the field of ultra-thin plates.

[0081] The present invention also provides the use of the 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment described in the above technical solution in the diaphragm of ship power equipment.

[0082] The present invention has no special limitation on the application of the 05Cr17Ni4Cu4Nb stainless steel ingot in the diaphragm of ship power equipment, and the application operation familiar to those skilled in the art can be adopted.

[0083] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0084] Example 1

[0085] The method for preparing 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment comprises the following steps:

[0086] (1) S≤0.020wt% and P≤0.020wt% scrap steel is subjected to electric arc furnace smelting to obtain molten steel; the electric arc furnace smelting consists of a melting period, an oxidation period and a reduction period which are carried out in sequence;

[0087] In the melting period, when the temperature of the molten steel is 1560℃, 2% FeO by weight of the molten steel is added, and carbon and oxygen are co-sprayed to form foamed slag for 8 minutes; the carbon spraying amount is 5kg / t; oxygen is blown at the furnace mouth with an oxygen blowing pipe; the oxygen spraying amount is 7cum / min; when the temperature of the molten steel is 1600℃, it enters the oxidation period;

[0088] The oxidation period is carried out under oxygen blowing conditions; the oxygen blowing pressure is 1.5MPa; the decarburization amount in the oxidation period is ≥40%; the molten steel is boiled for 5 minutes in the oxidation period, and then 0.2% of Mn by mass of the molten steel is added; when the C content in the molten steel is 0.80-1.0wt%, P≤0.015wt%, and the molten steel temperature is 1670℃, the slag is removed and the reduction period begins;

[0089] During the reduction period, 200kg of lime and 70kg of fluorite are added in sequence to adjust C≈1.0%, 5kg / t of silicon manganese, 5kg / t of ferromanganese, 15wt% of ferrochrome, and 3wt% of nickel plate are added. After the thin slag is made, 5kg / t of ferrosilicon powder and 1kg / t of carbon powder are added to make white slag. Samples are taken for analysis after 10 minutes, and samples are taken again for component analysis every 5 minutes. The white slag is kept for 20 minutes, and 8kg / t of composite deoxidizer is added 10 minutes before being transferred to the ladle. When the molten steel composition reaches the specified range and the temperature is 1700°C, it is transferred to the ladle, and the slag in the ladle is skimmed until the residue amount is ≤1.5kg / t. At 1650°C, it is transferred to the VODC vacuum refining furnace for vacuum refining furnace refining;

[0090] The composite deoxidizer is composed of the following components in mass percentage: Al 41%, 7Al2O3·12CaO 3%, CaCO38%, Fe 15%, CaF230% and Mn 3%;

[0091] (2) refining the molten steel obtained in step (1) in a vacuum refining furnace, then analyzing the composition, adding pre-baked alloy to fine-tune the composition according to the result, and then placing the steel under bottom blowing argon gas, and then calming for 5 minutes to obtain refined molten steel;

[0092] The vacuum refining furnace refining consists of a VOD stage, a VCD stage, a VOH stage and a VD stage which are carried out in sequence;

[0093] The process parameters of the VOD stage are: temperature 1650°C, vacuum 80 mbar; top blowing oxygen, bottom blowing argon; oxygen blowing volume 450 m 3 / h; argon blowing volume is 3m 3 / h, when the C content in molten steel is lower than 0.03wt%, it enters the VCD stage;

[0094] The process parameters of the VCD stage are: temperature 1655℃, vacuum degree 1mbar; vacuum time 8min; bottom blowing argon; argon flow rate 3m 3 / h; break the air, take samples and measure the temperature, then add 20kg / t of lime and 3kg / t of fluorite, and judge that it has entered the VOH stage according to the measured temperature, the amount of alloy added and the pouring temperature;

[0095] The process parameters of the VOH stage are: temperature 1670℃, vacuum 350mbar; top blowing oxygen, bottom blowing argon; oxygen flow rate 450m 3 / h; Argon flow rate 3m 3 / h; adding aluminum to increase the temperature; when aluminum is added to the molten steel by 1% of its mass, the temperature of the molten steel increases by 250%;

[0096] The process parameters of the VD stage are: temperature 1670℃, vacuum 1.0mbar; bottom blowing argon; argon flow rate 4.5m 3 / h, and the process ends when the ingredients meet the specified requirements;

[0097] (3) The refined molten steel obtained in step (2) is sequentially poured, demolded and annealed to obtain 05Cr17Ni4Cu4Nb stainless steel ingots for ultra-thin diaphragm ship power equipment; wherein, before pouring, the pouring system is checked to ensure that it is dry and free of moisture, and the runner and steel mold are clean and free of pollution; the pouring temperature is 1550°C; the pouring flow rate is 1t / min; argon protection pouring, the argon blowing volume is 5L / min; the demolding time is 24h; the annealing temperature is 650°C, the insulation time is 0.8min / mm, the furnace is cooled to ≤500°C and then air-cooled out of the furnace.

[0098] In terms of mass percentage, the composition of the 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment is C 0.047%, Si 0.40%, Mn 0.50%, Cr 15.50%, Ni 3.25%, Nb 0.23%, Cu 3.20%, S 0.010%, P 0.025% and the balance Fe.

[0099] Example 2

[0100] The method for preparing 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment comprises the following steps:

[0101] (1) S≤0.020wt% and P≤0.020wt% scrap steel is subjected to electric arc furnace smelting to obtain molten steel; the electric arc furnace smelting consists of a melting period, an oxidation period and a reduction period which are carried out in sequence;

[0102] In the melting period, when the temperature of the molten steel is 1560℃, 3% FeO by weight of the molten steel is added, and carbon and oxygen are co-sprayed to form foamed slag for 9 minutes; the carbon spraying amount is 5kg / t; oxygen is blown at the furnace mouth with an oxygen blowing pipe; the oxygen spraying amount is 8cum / min; when the temperature of the molten steel is 1650℃, it enters the oxidation period;

[0103] The oxidation period is carried out under oxygen blowing conditions; the oxygen blowing pressure is 1.5MPa; the decarburization amount in the oxidation period is ≥40%; the molten steel is boiled for 6 minutes in the oxidation period, and then 0.2% of Mn by mass of the molten steel is added; when the C content in the molten steel is 0.80-1.0wt%, P≤0.015wt%, and the molten steel temperature is 1700℃, the slag is removed and the reduction period begins;

[0104] During the reduction period, 150kg of lime and 100kg of fluorite are added in sequence to adjust C≈1.0%, 5kg / t of silicon manganese, 5kg / t of ferromanganese, 15wt% of ferrochrome, and 3wt% of nickel plate are added according to [Cr]=10wt%. After the thin slag is made, 2-3kg / t of calcium carbide and 5-8kg / t of AD powder are added to make white slag. Samples are taken for analysis every 15 minutes, and samples are taken again for component analysis every 5 minutes. The white slag is kept for 20 minutes, and 8kg / t of composite deoxidizer is added 10 minutes before being transferred to the ladle. When the molten steel composition reaches the specified range and the temperature is 1700°C, it is transferred to the ladle, and the slag in the ladle is skimmed until the residue amount is ≤1.5kg / t. At 1650°C, it is transferred to the VODC vacuum refining furnace for vacuum refining furnace refining;

[0105] The composite deoxidizer is composed of the following components in mass percentage: Al 50%, 7Al2O3·12CaO 1%, CaCO35%, Fe 20%, CaF223% and Mn 1%;

[0106] (2) refining the molten steel obtained in step (1) in a vacuum refining furnace, then analyzing the composition, adding pre-baked alloy to fine-tune the composition according to the result, and then placing the steel under bottom blowing argon gas, and then calming for 6 minutes to obtain refined molten steel;

[0107] The vacuum refining furnace refining consists of a VOD stage, a VCD stage, a VOH stage and a VD stage which are carried out in sequence;

[0108] The process parameters of the VOD stage are: temperature 1650°C, vacuum 100 mbar; top blowing oxygen, bottom blowing argon; oxygen blowing volume 550 m 3 / h; argon blowing volume is 5m 3 / h, when the C content in molten steel is lower than 0.03wt%, it enters the VCD stage;

[0109] The process parameters of the VCD stage are: temperature 1655℃, vacuum degree 3mbar; vacuum time 9min; bottom blowing argon; argon flow rate 5m 3 / h; break the air, take samples and measure the temperature, then add 20kg / t of lime and 3kg / t of fluorite, and judge whether it has entered the VOH stage according to the measured temperature, the amount of alloy added, the temperature of steel casting and other factors;

[0110] The process parameters of the VOH stage are: temperature 1675℃, vacuum 400mbar; top blowing oxygen, bottom blowing argon; oxygen flow rate 500m 3 / h; Argon flow rate 5m 3 / h; adding aluminum to increase the temperature; when aluminum is added to the molten steel by 1% of its mass, the temperature of the molten steel increases by 250%;

[0111] The process parameters of the VD stage are: temperature 1675℃, vacuum 2.0mbar; bottom blowing argon; argon flow rate 5.5m 3 / h, and the process ends when the ingredients meet the specified requirements;

[0112] (3) The refined molten steel obtained in step (2) is sequentially poured, demolded and annealed to obtain 05Cr17Ni4Cu4Nb stainless steel ingots for ultra-thin diaphragm ship power equipment; wherein, before pouring, the pouring system is checked to ensure that it is dry and free of moisture, and the runner and steel mold are clean and free of pollution; the pouring temperature is 1550°C; the pouring flow rate is 2t / min; argon protection pouring, the argon blowing volume is 8L / min; the demolding time is 18h; the annealing temperature is 700°C, the insulation time is 0.9min / mm, the furnace is cooled to ≤500°C and then air-cooled out of the furnace.

[0113] In terms of mass percentage, the composition of the 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment is C 0.050%, Si 0.50%, Mn 0.60%, Cr 15.00%, Ni 3.00%, Nb 0.30%, Cu 4.00%, S 0.010%, P 0.025% and the balance Fe.

[0114] Example 3

[0115] The method for preparing 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment comprises the following steps:

[0116] (1) S≤0.020wt% and P≤0.020wt% scrap steel is subjected to electric arc furnace smelting to obtain molten steel; the electric arc furnace smelting consists of a melting period, an oxidation period and a reduction period which are carried out in sequence;

[0117] In the melting period, when the temperature of the molten steel is 1560℃, 4% FeO by weight of the molten steel is added, and carbon and oxygen are co-sprayed to form foamed slag for 10 minutes; the carbon spraying amount is 5kg / t; oxygen is blown at the furnace mouth with an oxygen blowing pipe; the oxygen spraying amount is 8cum / min; when the temperature of the molten steel is 1650℃, it enters the oxidation period;

[0118] The oxidation period is carried out under oxygen blowing conditions; the oxygen blowing pressure is 1.5MPa; the decarburization amount in the oxidation period is ≥40%; the molten steel is boiled for 7 minutes in the oxidation period, and then 0.2% of Mn by mass of the molten steel is added; when the C content in the molten steel is 0.80-1.0wt%, P≤0.015wt%, and the molten steel temperature is 1720℃, the slag is removed and the reduction period begins;

[0119] During the reduction period, 100kg of lime and 50kg of fluorite are added in sequence to adjust C≈1.0%, 5kg / t of silicon manganese, 5kg / t of ferromanganese, 15wt% of ferrochrome, and 3wt% of nickel plate are added according to [Cr]=15wt%. After the thin slag is made, 5kg / t of ferrosilicon powder and 1kg / t of carbon powder are added to make white slag. Samples are taken for analysis after 15 minutes, and samples are taken again for component analysis every 5 minutes. The white slag is kept for 20 minutes, and 8kg / t of composite deoxidizer is added 10 minutes before being transferred to the ladle. When the composition of the molten steel reaches the specified range and the temperature is 1700°C, it is transferred to the ladle, and the slag in the ladle is skimmed until the residue amount is ≤1.5kg / t. At 1650°C, it is transferred to the VODC vacuum refining furnace for vacuum refining furnace refining;

[0120] The composite deoxidizer is composed of the following components in mass percentage: Al 45%, 7Al2O3·12CaO 3%, CaCO3 6%, Fe 16%, CaF2 28% and Mn 2%;

[0121] (2) refining the molten steel obtained in step (1) in a vacuum refining furnace, then analyzing the composition, adding pre-baked alloy to fine-tune the composition according to the result, and then placing the steel under bottom blowing argon gas, and then calming for 7 minutes to obtain refined molten steel;

[0122] The vacuum refining furnace refining consists of a VOD stage, a VCD stage, a VOH stage and a VD stage which are carried out in sequence;

[0123] The process parameters of the VOD stage are: temperature 1650°C, vacuum 120 mbar; top blowing oxygen, bottom blowing argon; oxygen blowing volume 650 m 3 / h; argon blowing volume is 6m 3 / h, when the C content in molten steel is lower than 0.03wt%, it enters the VCD stage;

[0124] The process parameters of the VCD stage are: temperature 1655℃, vacuum degree 5mbar; vacuum time 10min; bottom blowing argon; argon flow rate 6m 3 / h; break the air, take samples and measure the temperature, then add 20kg / t of lime and 3kg / t of fluorite, and judge whether it has entered the VOH stage according to the measured temperature, the amount of alloy added, the temperature of steel casting and other factors;

[0125] The process parameters of the VOH stage are: temperature 1675℃, vacuum 450mbar; top blowing oxygen, bottom blowing argon; oxygen flow rate 550m 3 / h; Argon flow rate 6m 3 / h; adding aluminum to increase the temperature; when aluminum is added to the molten steel by 1% of its mass, the temperature of the molten steel increases by 250%;

[0126] The process parameters of the VD stage are: temperature 1675℃, vacuum 2.0mbar; bottom blowing argon; argon flow rate 6m 3 / h, and the process ends when the ingredients meet the specified requirements;

[0127] (3) The refined molten steel obtained in step (2) is sequentially poured, demolded and annealed to obtain 05Cr17Ni4Cu4Nb stainless steel ingots for ultra-thin diaphragm ship power equipment; wherein, before pouring, the pouring system is checked to ensure that it is dry and free of moisture, and the runner and steel mold are clean and free of pollution; the pouring temperature is 1550°C; the pouring flow rate is 2t / min; argon protection pouring, the argon blowing volume is 10L / min; the demolding time is 18h; the annealing temperature is 700°C, the insulation time is 1min / mm, the furnace is cooled to ≤500°C and then air-cooled out of the furnace.

[0128] In terms of mass percentage, the composition of the 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment is C 0.060%, Si 0.20%, Mn 0.80%, Cr 16.50%, Ni 4.50%, Nb 0.38%, Cu 4.50%, S 0.010%, P 0.025% and the balance Fe.

[0129] Comparative Example 1

[0130] The composition of the composite deoxidizer was modified on the basis of Example 1 as follows: CaF2 and Mn were omitted, and the content of 7Al2O3·12CaO was modified to the sum of the contents of 7Al2O3·12CaO, CaF2 and Mn, while other conditions remained unchanged.

[0131] Comparative Example 2

[0132] The composition of the composite deoxidizer was modified on the basis of Example 1 as follows: Mn was omitted, the content of CaF2 was modified to the sum of the contents of CaF2 and Mn, and other conditions remained unchanged.

[0133] Comparative Example 3

[0134] The composition of the composite deoxidizer was modified on the basis of Example 1 as follows: CaF2 was omitted, and the content of Mn was modified to the sum of the contents of CaF2 and Mn, while other conditions remained unchanged.

[0135] Comparative Example 4

[0136] The composition of the composite deoxidizer was modified on the basis of Example 1 as follows: 7Al2O3·12CaO was omitted, the content of CaF2 was modified to the sum of the contents of CaF2 and 7Al2O3·12CaO, and other conditions remained unchanged.

[0137] The performance tests were performed on the 05Cr17Ni4Cu4Nb stainless steel ingots prepared in Examples 1 to 3 and Comparative Examples 1 to 4. The mechanical property data are shown in Table 1 (CMA test), and the non-metallic inclusion test results are shown in Table 2.

[0138] Table 1 Mechanical properties data of 05Cr17Ni4Cu4Nb stainless steel ingots prepared in Examples 1 to 3

[0139]

[0140] Table 2 Non-metallic inclusion detection data of 05Cr17Ni4Cu4Nb stainless steel ingots prepared in Examples 1 to 3 and Comparative Examples 1 to 4

[0141] Inclusion Type A B C D Ds Original Standard ≤2 ≤2 ≤2 ≤2 Current Standard ≤1.5 ≤1.5 ≤1.5 ≤1.5 Example 1 ≤0.5 ≤1.0 ≤0.5 ≤1.0 ≤1.5 Example 2 ≤0.5 ≤1.0 ≤0.5 ≤1.0 ≤1.5 Example 3 ≤0.5 ≤1.0 ≤0.5 ≤1.0 ≤1.5 Comparative Example 1 ≤1.0 ≤1.5 ≤1.0 ≤1.5 Comparative Example 2 ≤1.0 ≤1.0 ≤1.0 ≤1.0 Comparative Example 3 ≤1.0 ≤1.0 ≤1.0 ≤1.0 Comparative Example 4 ≤1.0 ≤1.0 ≤1.0 ≤1.0

[0142] It can be seen from Table 2 that the preparation method provided by the present invention can greatly improve the inclusion level of 05Cr17Ni4Cu4Nb stainless steel, so that it can meet the application in the field of ultra-thin plates; it can be seen from Example 1 and Comparative Examples 1 to 4 that by adding Mn and CaF2, a synergistic effect can be formed with the 7Al2O3·12CaO pre-molten slag, thereby further improving the deoxidation effect and further improving the inclusion level.

[0143] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment, comprising the following steps: (1) smelting scrap steel in an electric arc furnace to obtain molten steel; (2) refining the molten steel obtained in step (1) in a vacuum refining furnace to obtain refined molten steel; (3) pouring and heat treating the refined molten steel obtained in step (2) in sequence to obtain 05Cr17Ni4Cu4Nb stainless steel ingots for ultra-thin diaphragm ship power equipment; The electric arc furnace smelting in step (1) comprises a melting period, an oxidation period and a reduction period which are carried out in sequence; During the melting period, a slag-making agent is added and carbon and oxygen are co-sprayed to form foamed slag; The oxidation period is carried out under oxygen blowing conditions; During the reduction period, alloy raw materials and composite deoxidizer are added; The composite deoxidizer comprises the following components in mass percentage: 40-50% Al, 1-3% 7Al2O3·12CaO, 5-8% CaCO3, 10-20% Fe, 20-30% CaF2 and 1-3% Mn.

2. The preparation method according to claim 1, characterized in that: The carbon injection amount during the carbon and oxygen co-injection is 3-8 kg / t; the time for the carbon and oxygen co-injection to form the foamed slag is 8-10 minutes.

3. The preparation method according to claim 1, characterized in that: The pressure of the oxygen blowing is 1-2 MPa.

4. The preparation method according to claim 1, characterized in that: During the reduction period, thin slag material, deoxidizer, alloy raw material, reducing agent and composite deoxidizer are added in sequence.

5. The preparation method according to claim 4, characterized in that: The thin slag material includes lime and fluorite; the deoxidizer includes silicon manganese and ferromanganese; the alloy raw materials include ferrochrome and nickel plate; the reducing agent includes at least one of ferrosilicon powder, calcium carbide, carbon powder and AD powder.

6. The preparation method according to claim 1 or 4, characterized in that: The composite deoxidizer comprises the following components in mass percentage: 42-48% Al, 1.5-2.5% 7Al2O3·12CaO, 6-7% CaCO3, 12-18% Fe, 22-28% CaF2 and 1.5-2.5% Mn.

7. The preparation method according to claim 1, characterized in that: The vacuum refining furnace refining in step (2) includes a VOD stage, a VCD stage, a VOH stage and a VD stage which are performed in sequence.

8. The preparation method according to claim 1, characterized in that: In the step (3), the pouring temperature is 1550° C., the pouring flow rate is 1-2 t / min, and the pouring is carried out under argon protection.

9. 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment prepared by the preparation method according to any one of claims 1 to 8.

10. Application of the 05Cr17Ni4Cu4Nb stainless steel ingot for ultra-thin diaphragm ship power equipment as claimed in claim 9 in diaphragms for ship power equipment.