A positive electrode active material additive and its preparation method and application

By PEDOT coating of rice husk-based activated carbon, a positive electrode active material additive with a dense structure is solved, and the problems of poor conductivity of lead-acid batteries and easy oxide substances fall off are significantly improved, and the circulation performance and life of the battery are simplified. Craft.

CN118016885BActive Publication Date: 2024-11-19JIANGXI GOLDEN CHAFF NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410143068.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-01
Publication Date
2024-11-19
Estimated Expiration
2044-02-01

AI Technical Summary

Technical Problem

Lead acid batteries and lead carbon batteries have insufficient performance problems in terms of poor conductivity and easy removal of oxide substances, resulting in high weight, low energy density and short cycle life.

Method used

PEDOT is used to coat rice husk-based activated carbon to form a dense structure of positive electrode active material additive (PEDOT@RHAC). The surface modification of conductive polymer materials makes rice husk-activated carbon aggregate, enhance the conductivity of the positive electrode plate, and improve the The composite material is processed to improve electrochemical properties.

Benefits of technology

It significantly improves the deep cycle performance of lead-acid batteries (lead-containing carbon batteries), reduces charge transfer and ion exchange resistance, extends the cycle life of the battery, simplifies the preparation process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118016885B_ABST
    Figure CN118016885B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of battery materials, and provides a positive electrode active material additive, a preparation method and application thereof. The positive electrode active material additive of the present invention is prepared by coating rice husk-based activated carbon (RHAC) with a conductive polymer material (PEDOT). The positive electrode active material additive (PEDOT@RHAC) can aggregate RHAC together to form a dense structure through surface modification of PEDOT, thereby enhancing the conductivity of the positive electrode plate; the lead-acid battery with PEDOT@RHAC added to the positive electrode plate exhibits excellent electrochemical properties such as significantly reduced charge transfer resistance and ion exchange resistance, and significantly improved cycle performance, and is widely used in positive electrode materials of lead-acid batteries (including lead-carbon batteries).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials and relates to a positive electrode active material additive and a preparation method and application thereof. Background Art

[0002] At present, despite the emergence of new battery technologies, lead-acid batteries are still widely used due to their technical stability, cost-effectiveness and reliability. However, technically, it still faces many problems to be solved, such as high weight, low energy density and short cycle life. Among them, the positive plate, as its key component, has a great impact on battery performance. In order to enhance the market competitiveness of lead-acid batteries and lead-carbon batteries, the optimization and research and development of the conductivity of the positive plate and the easy shedding of its oxide material has become an urgent need.

[0003] Poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS) is a commonly used conductive polymer that has been widely used in a variety of organic electronic devices, flexible electronics and bioelectronics due to its unique physical, chemical and mechanical properties.

[0004] Chinese invention patent application CN116884776A discloses a graphene / poly 3,4-ethylenedioxythiophene composite material and its preparation method and application. The composite material is prepared by reacting graphene oxide, aminomethyl EDOT, and dicyclohexylcarbodiimide, reducing to obtain aminomethyl EDOT functionalized graphene, and then in-situ polymerizing it with 3,4-ethylenedioxythiophene; the graphene / PEDOT composite material can effectively alleviate the problem of capacity attenuation caused by the volume shrinkage and expansion of PEDOT during long-term charging and discharging. The electrode material prepared by using the composite material has high specific capacitance and excellent cycle stability, and can be used in supercapacitors. However, the preparation process is relatively complicated.

[0005] Carbon materials such as rice husk-based activated carbon (RHAC), graphite, carbon fiber and carbon nanotubes have shown significant effects as positive electrode additives in many studies. Among them, rice husk-based activated carbon has attracted great attention due to its low cost, recyclability, high specific surface area and good pore structure. Chinese invention patent application CN110571433A discloses a negative electrode carbon additive for improving the charging acceptance of lead-carbon batteries and its application, using rice husk-based porous carbon to provide a good ion conductor for energy storage devices and improve the kinetic activity of electrochemical reactions; at the same time, the rice husk-based porous carbon is mixed with one or more of activated carbon, carbon black, graphite, expanded graphite, graphene, single-walled carbon nanotubes, multi-walled carbon nanotubes, etc., to further enhance the conductivity of the negative electrode carbon additive; it can effectively improve the charging acceptance of lead-carbon batteries, inhibit the sulfation phenomenon of the negative electrode of lead-acid batteries in partial state of charge (PSoC) and extend the cycle life of the battery in PSoC.

[0006] Therefore, compounding rice husk activated carbon with carbon materials such as graphite, carbon fiber and carbon nanotubes, combining it with conductive polymers such as poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate, and preparing composite materials through process improvement will hopefully solve the problems of poor conductivity of lead-acid batteries (including lead-carbon batteries) and easy shedding of their oxide substances, and improve their electrical properties. Summary of the invention

[0007] The present invention aims to solve the problems existing in the prior art and provides a positive electrode active material additive and a preparation method and application thereof. The PEDOT-modified RHAC positive electrode active material additive (PEDOT@RHAC) can aggregate RHAC together to form a dense structure through surface modification of PEDOT, thereby enhancing the conductivity of the positive electrode plate. The lead-acid battery with PEDOT@RHAC added to the positive electrode plate exhibits excellent electrochemical properties such as reduced charge transfer resistance and ion exchange resistance, thereby significantly improving its deep cycle performance.

[0008] To achieve the above object, the technical solution of the present invention is as follows:

[0009] A positive electrode active material additive is prepared by coating rice husk-based activated carbon with a conductive polymer material.

[0010] Furthermore, the rice husk activated carbon preparation method is as follows:

[0011] S1: carbonizing rice husk under an inert atmosphere to obtain rice husk char;

[0012] S2: mixing rice husk char with an activating agent and pyrolyzing and activating the char under an inert atmosphere;

[0013] S3: After washing and drying, the product is obtained.

[0014] Furthermore, the inert atmosphere includes any one of nitrogen, argon and carbon dioxide.

[0015] Furthermore, the activator is NaOH and / or KOH.

[0016] Furthermore, the mass ratio of the rice husk char to the activator is 1:2.5-4.

[0017] Furthermore, the carbonization temperature is 450-550° C., and the carbonization time is 1-2 hours.

[0018] Furthermore, the pyrolysis activation temperature is 700-850° C., and the pyrolysis activation time is 1-2 hours.

[0019] Furthermore, the conductive polymer material is selected from polyethylene dioxythiophene and / or polystyrene sulfonate.

[0020] The present invention also provides a method for preparing the above-mentioned positive electrode active material additive, which specifically comprises the following steps:

[0021] (1) Add rice husk activated carbon and protonic acid into water and disperse them;

[0022] (2) Adding the monomer of the conductive polymer material under light-proof conditions, heating and stirring;

[0023] (3) adding an initiator to carry out an in-situ polymerization reaction;

[0024] (4) After the reaction is completed, the product is centrifuged, washed and dried.

[0025] Furthermore, the protonic acid is sodium dodecyl sulfate; the concentration in water is 0.005-0.02 mol / L.

[0026] Furthermore, the initiator is ammonium persulfate, and the concentration in water is 1-4 mol / L.

[0027] Furthermore, the mass ratio of the monomer of the polymer material to the rice husk activated carbon is 1:0.05-0.2; preferably 1:0.08-0.17; further preferably 1:0.08.

[0028] Furthermore, in step (2), the heating temperature is 35-50° C. and the stirring time is 0.5-1 h.

[0029] Furthermore, in step (3), the in-situ polymerization reaction time is 10-12 hours.

[0030] The present invention also provides the use of the positive electrode active material additive or the positive electrode active material additive prepared by the above preparation method in the preparation of positive electrode materials for lead-acid batteries.

[0031] In the present invention, the lead-acid battery includes a lead-carbon battery.

[0032] The present invention also provides a positive electrode lead paste for a lead-acid battery, wherein the positive electrode lead paste for the lead-acid battery comprises any one of the positive electrode active material additives described above.

[0033] Furthermore, the mass percentage of the positive electrode active material additive in the positive electrode lead paste of the lead-acid battery is 0.1-0.8%.

[0034] Furthermore, the lead paste for the positive electrode of the lead-acid battery also includes: lead powder, short fibers, paste sulfuric acid and deionized water.

[0035] Furthermore, the lead paste for positive electrode of lead-acid battery comprises, by weight: 0.2-0.8 parts of positive electrode active material additive, 90-120 parts of lead powder, 0.05-0.15 parts of short fiber, 8-10 parts of paste sulfuric acid and 8-11 parts of deionized water.

[0036] In some embodiments of the present invention, the positive electrode paste of the lead-acid battery is used as a raw material, and a positive electrode plate containing a rice husk-based activated carbon additive is prepared according to conventional battery pasting and curing processes.

[0037] In some embodiments of the present invention, the positive electrode plate containing the positive electrode active material additive can be assembled and formed with the negative electrode plate, separator and electrolyte according to the battery process to obtain a lead-acid battery with a positive electrode containing rice husk-based activated carbon additive.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) The present invention uses rice husk activated carbon and uses a conductive polymer material to coat the positive electrode active material additive (PEDOT@RHAC). The specific surface area of ​​the coated material is reduced, and the pore volume is reduced, which indicates the effective coating of the conductive polymer material. The surface modification of PEDOT can make RHAC aggregate together to form a dense structure, which is conducive to the interconnection between RHAC to form a conductive path, thereby enhancing the conductivity of the positive electrode plate.

[0040] (2) Lead-acid batteries (lead-carbon batteries) with PEDOT@RHAC added to the positive plate exhibit excellent electrochemical properties: it increases the oxygen evolution potential (OEP) and can further avoid the problem of easy shedding of the positive electrode active material, thereby maintaining the performance of the battery, and reduces the charge transfer resistance and ion exchange resistance, and its deep cycle performance is also significantly improved.

[0041] (3) The preparation process of the rice husk activated carbon and the conductive polymer material coated rice husk activated carbon of the present invention is simple and low in cost, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a high rate cycle life diagram of the lead-acid battery prepared by the present invention;

[0043] Figure 2 This is a deep cycle life diagram of the lead-acid battery prepared by the present invention;

[0044] Figure 3 This is a test chart of the discharge capacity of the lead-acid electrode prepared by the present invention. DETAILED DESCRIPTION

[0045] The following non-limiting examples can enable those skilled in the art to more fully understand the present invention, but do not limit the present invention in any way. The following content is merely an exemplary description of the scope of the present invention, and those skilled in the art can make various changes and modifications to the present invention based on the disclosed content, which should also fall within the scope of the present invention.

[0046] Embodiment 1:

[0047] (1) Preparation of rice husk activated carbon:

[0048] First, 10g of rice husk was placed in a nickel ark and put into a tubular furnace, and N2 was introduced. Carbonization was carried out at 500℃, and the obtained product was rice husk char. Then, NaOH was used as an activator for activation. First, rice husk char and NaOH particles were mixed in a mortar at a mass ratio of 1:3. After sufficient mixing, the mixture was placed in a nickel ark and put into a tubular furnace. Pyrolysis was carried out at 800℃ for 1h under N2 atmosphere. The obtained char was washed and dried to obtain rice husk-based activated carbon.

[0049] (2) Conductive polymer material coated rice husk activated carbon:

[0050] Use a measuring cylinder to measure 20mL of 0.01mol / L sodium dodecylbenzene sulfonate (SDS) solution in a 100mL round-bottom flask, add 0.5g of rice husk-based activated carbon, stir and mix, let the rice husk activated carbon evenly disperse in the solution, then add 64μL of 3,4-ethylenedioxythiophene (EDOT), stir and mix magnetically for 1h in a light-proof, 40℃ water bath. After stirring evenly, add 600μL of 2mol / L ammonium persulfate (APS) solution to the system, stir and react magnetically for 12h, and the reaction liquid changes from colorless to black. Take the reaction solution in a 50mL centrifuge tube, centrifuge at 12500r / min for 30min, remove the supernatant, repeat water washing 3 times, and dry to obtain the rice husk-based activated carbon composite material PEDOT@RHAC.

[0051] (3) Preparation of positive lead paste for lead-acid batteries:

[0052] 100 g of lead powder, 0.075 g of short fibers, and 0.5 g of PEDOT@RHAC were mixed in a paste mixer for 1 h. Subsequently, 10 g of deionized water and 9 g of sulfuric acid (1.32 g / mL) were slowly added in sequence while stirring to obtain a positive electrode lead paste for a lead-acid battery.

[0053] (4) Lead-acid battery preparation:

[0054] 1.2 g of the prepared lead-acid battery positive electrode lead paste was applied to the lead alloy grid and then cured. The curing procedure was as follows: first, the temperature was maintained at 50°C and the humidity was 98% for 1 hour, then the temperature was changed to 60°C and maintained for 1 hour; then the temperature was changed to 65°C and maintained for 48 hours; finally, it was dried at 70°C for 3 hours and then cooled to room temperature. Two commercial lead-acid battery negative plates and one positive plate (prepared from the lead-acid battery positive electrode lead paste obtained in step (3)) were assembled into a lead-acid battery.

[0055] The battery is subjected to a cycle life test, which is divided into a deep cycle 100% DOD test and a high rate HRPSoC test.

[0056] The deep cycle 100% DOD test starts with charging to 2.4V at a 0.5C rate current, and then charging at a constant voltage of 2.4V for 4 hours. Subsequently, the discharge part is run at 100% DOD at a constant current of 1C to 1.75V until the discharge capacity is 80% of the first discharge capacity. The cycle test is terminated, and the cycle life can reach 52 times.

[0057] The high-rate HRPSoC test starts with charging at a constant current of 1C to a voltage of 2.4V, then charging at a constant voltage of 2.35V until the current reaches 5mA, then discharging at a constant current to half of the capacity, standing for 10 minutes, and then discharging at a constant current of 1C. When the charging voltage or cut-off voltage of the battery during the test is higher than 2.9V or lower than 1.6V, the test is stopped. The number of cycles is 1958.

[0058] Embodiment 2:

[0059] (1) Preparation of rice husk activated carbon:

[0060] First, 10g of rice husk was placed in a nickel ark and put into a tubular furnace, and N2 was introduced. Carbonization was carried out at 500℃, and the obtained product was rice husk char. Then, NaOH was used as an activator for activation. First, rice husk char and KOH particles were mixed in a mortar at a ratio of 1:4. After sufficient mixing, the mixture was placed in a nickel ark and put into a tubular furnace. Pyrolysis was carried out at 700℃ for 2h under N2 atmosphere. The obtained char was washed with water and dried to obtain rice husk-based activated carbon.

[0061] (2) Conductive polymer material coated rice husk activated carbon:

[0062] Use a measuring cylinder to measure 20mL of 0.01mol / L SDS solution in a 100mL round-bottom flask, add 1g of rice husk-based activated carbon, stir and mix, let the rice husk activated carbon evenly disperse in the solution, then add 64μL EDOT, stir and mix magnetically in a light-proof, 40℃ water bath for 1h. After stirring evenly, add 600μL of 2mol / L APS solution to the system, stir and react magnetically for 12h, and the reaction liquid changes from colorless to black. Take the reaction solution in a 50mL centrifuge tube, centrifuge at 12500r / min for 30min, remove the supernatant, repeat washing 3 times, and dry to obtain the rice husk-based activated carbon composite material PEDOT@RHACⅡ.

[0063] (3) Preparation of positive lead paste for lead-acid batteries:

[0064] 100 g of lead powder, 0.075 g of short fibers, and 0.5 g of PEDOT@RHACⅡ were mixed in a paste mixer for 1 h. Subsequently, 10 g of deionized water and 9 g of sulfuric acid (1.32 g / mL) were slowly added in sequence while stirring to obtain a positive electrode lead paste for a lead-acid battery.

[0065] (4) Lead-acid battery preparation:

[0066] 1.2 g of the prepared lead-acid battery positive electrode lead paste was applied to the lead alloy grid and then cured. The curing procedure was as follows: first, the temperature was maintained at 50°C and the humidity was 98% for 1 hour, then the temperature was changed to 60°C and maintained for 1 hour; then the temperature was changed to 65°C and maintained for 48 hours; finally, it was dried at 70°C for 3 hours and then cooled to room temperature. Two commercial lead-acid battery negative plates and one positive plate (prepared from the lead-acid battery positive electrode lead paste obtained in step (3)) were assembled into a lead-acid battery.

[0067] The cycle life test method for the battery is the same as that in Example 1. The cycle life of the deep cycle 100% DOD test can reach 46 times; the cycle number of the high rate HRPSoC test is 1367 times.

[0068] The pore structure parameters of the rice husk activated carbon after NaOH activation and the PEDOT@RHAC and PEDOT@RHACⅡ prepared in Examples 1 and 2 are shown in Table 1.

[0069] Table 1 Pore structure parameters of positive electrode additives

[0070]

[0071] It can be seen from the above table that the specific surface area of ​​the material decreases after coating, and the micropore volume, mesopore volume and total pore volume all decrease, indicating the effective coating of the conductive polymer material.

[0072] The high rate cycle life, deep cycle life and discharge capacity test results of the blank sample without any additives added to the positive electrode, the rice husk activated carbon after NaOH activation, and the PEDOT@RHAC and PEDOT@RHACⅡ prepared in Examples 1 and 2 are shown in Figure 1-3 It can be seen that compared with the blank sample without any additives and the rice husk activated carbon after NaOH activation, the high-rate cycle life, deep cycle life and charge-discharge capacity of the RHAC coated with PEDOT are significantly improved.

[0073] Comparative Example 1

[0074] Compared with Example 1, the only difference is that the positive electrode active material additive is prepared by coating graphene with a conductive polymer material, and the specific steps are as follows:

[0075] Use a measuring cylinder to measure 20mL of 0.01mol / L SDS solution in a 100mL round-bottom flask, add 0.5g of graphene, stir and mix, let the graphene be evenly dispersed in the solution, then add 64μL EDOT, stir and mix magnetically in a light-proof, 40℃ water bath for 1h. After stirring evenly, add 600μL of 2mol / L APS solution to the system, stir and react magnetically for 12h, and the reaction liquid changes from colorless to black. Take the reaction solution in a 50mL centrifuge tube, centrifuge at 12500r / min for 30min, remove the supernatant, repeat washing 3 times, and after drying, you can get rice husk-based activated carbon composite material PEDOT@graphene.

[0076] The other steps are the same as in Example 1.

[0077] Comparative Example 2

[0078] Compared with Example 1, the only difference is that the positive electrode active material additive is prepared by coating graphene oxide with a conductive polymer material, and the specific steps are as follows:

[0079] Use a measuring cylinder to measure 20mL of 0.01mol / L SDS solution in a 100mL round-bottom flask, add 0.5g of graphene oxide, stir and mix, let the graphene oxide be evenly dispersed in the solution, then add 64μL EDOT, stir and mix magnetically in a light-proof, 40℃ water bath for 1h. After stirring evenly, add 600μL of 2mol / L APS solution to the system, stir and react magnetically for 12h, and the reaction liquid changes from colorless to black. Take the reaction solution in a 50mL centrifuge tube, centrifuge at 12500r / min for 30min, remove the supernatant, repeat washing 3 times, and after drying, you can get rice husk-based activated carbon composite material PEDOT@graphene oxide.

[0080] The other steps are the same as in Example 1.

[0081] Comparative Example 3

[0082] Compared with Example 1, the only difference is that the conductive polymer material is replaced by polypyrrole instead of poly 3,4-ethylenedioxythiophene. The specific steps are as follows:

[0083] Use a measuring cylinder to measure 20mL of 0.01mol / L SDS solution in a 100mL round-bottom flask, add 1g of rice husk-based activated carbon, stir and mix, let the rice husk activated carbon evenly disperse in the solution, then add 41μL of pyrrole, stir and mix magnetically for 1h in a light-proof, 40℃ water bath. After stirring evenly, add 600μL of 2mol / L APS solution to the system, stir and react magnetically for 12h, and the reaction liquid changes from colorless to black. Take the reaction solution in a 50mL centrifuge tube, centrifuge at 12500r / min for 30min, remove the supernatant, repeat washing 3 times, and dry to obtain the rice husk-based activated carbon composite material PEDOT@RHACⅡ.

[0084] The other steps are the same as in Example 1.

[0085] Comparative Example 4

[0086] Compared with Example 1, the only difference is that in step (2), the amount of 3,4-ethylenedioxythiophene (EDOT) used is 35 μm.

[0087] The other steps are the same as in Example 1.

[0088] Comparative Example 5

[0089] Compared with Example 1, the only difference is that in step (2), the amount of 3,4-ethylenedioxythiophene (EDOT) used is 180 μm.

[0090] The other steps are the same as in Example 1.

[0091] Comparative Example 6

[0092] Compared with Example 1, the only difference is that in step (1), the mass ratio of rice husk char to NaOH particles is 1:2.

[0093] Comparative Example 7

[0094] Compared with Example 1, the only difference is that in step (1), the mass ratio of rice husk char to NaOH particles is 1:5.

[0095] Comparative Example 8

[0096] Compared with Example 1, the only difference is that the specific operation of step (1) is as follows:

[0097] Use a measuring cylinder to measure 20mL of 0.01mol / L SDS solution in a 100mL round-bottom flask, add 1g rice husk-based activated carbon, 64μL EDOT, and 600μL of 2mol / L APS solution in a light-proof, 40℃ water bath, and stir magnetically for 12h. The reaction liquid changes from colorless to black. Take the reaction solution in a 50mL centrifuge tube, centrifuge at 12500r / min for 30min, remove the supernatant, repeat washing 3 times, and dry to obtain a rice husk-based activated carbon composite material.

[0098] Table 2 Pore structure parameters of positive electrode additives

[0099]

[0100] The cycle life test results of the lead-acid batteries prepared in the above embodiments and comparative examples are shown in Table 3.

[0101] Table 3 Lead-acid battery cycle life test results

[0102]

[0103]

[0104] It can be seen from the above table that the positive electrode active material additive prepared by the present invention through the selection of activated carbon (RHAC) and conductive polymer material (PEDOT) and the optimization of the amount of the two in the preparation process significantly improves the cycle performance of the lead-acid battery. At the same time, the coating preparation process further improves the conductivity of the positive electrode active material additive, thereby improving the cycle performance of the lead-acid battery; the positive electrode active material additive of the present invention exhibits the same performance in lead-carbon batteries.

[0105] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.

Claims

1. A positive electrode active material additive, characterized in that: The positive electrode active material additive is prepared by coating rice husk activated carbon with a conductive polymer material; the conductive polymer material is polyethylene dioxythiophene; The rice husk activated carbon preparation method is as follows: S1: carbonizing rice husk under an inert atmosphere to obtain rice husk char; S2: mixing rice husk char with an activating agent and pyrolyzing and activating the char under an inert atmosphere; S3: finally washed and dried to obtain; The activator is NaOH and / or KOH; the mass ratio of the rice husk coke to the activator is 1:2.5-4; The method for preparing the positive electrode active material additive comprises the following steps: (1) Add rice husk activated carbon and protonic acid into water and disperse them; (2) Adding the monomer of the conductive polymer material under light-proof conditions, heating and stirring; (3) adding an initiator to carry out an in-situ polymerization reaction; (4) After the reaction is completed, centrifuge, wash and dry to obtain; The mass ratio of the rice husk activated carbon to the monomer of the conductive polymer material is 1:0.05-0.

2.

2. The positive electrode active material additive according to claim 1, characterized in that: The carbonization temperature is 450-550°C and the carbonization time is 1-2h; The pyrolysis activation temperature is 700-850° C., and the pyrolysis activation time is 1-2 hours.

3. The method for preparing the positive electrode active material additive according to any one of claims 1 to 2, characterized in that: The following steps are involved: (1) Add rice husk activated carbon and protonic acid into water and disperse them; (2) Adding the monomer of the conductive polymer material under light-proof conditions, heating and stirring; (3) adding an initiator to carry out an in-situ polymerization reaction; (4) After the reaction is completed, the product is centrifuged, washed and dried.

4. The preparation method according to claim 3, characterized in that: The protonic acid is sodium dodecyl sulfonate solution with a concentration of 0.005-0.02 mol / L; the initiator is ammonium persulfate solution with a concentration of 1-4 mol / L.

5. The preparation method according to claim 3, characterized in that: The mass ratio of the rice husk activated carbon to the monomer of the conductive polymer material is 1:0.08-0.

17.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the rice husk activated carbon to the monomer of the conductive polymer material is 1:0.

08.

7. The preparation method according to claim 3, characterized in that: In step (2), the heating temperature is 35-50° C. and the stirring time is 0.5-1 h. In step (3), the in-situ polymerization reaction time is 10-12 h.

8. Use of the positive electrode active material additive according to any one of claims 1-2 or the positive electrode active material additive prepared by the preparation method according to any one of claims 3-7 in preparing positive electrode materials for lead-acid batteries.

9. A lead paste for positive electrode of a lead-acid battery, characterized in that: The positive electrode lead paste comprises: lead powder, short fibers, paste sulfuric acid, deionized water and positive electrode active material additives; The positive electrode active material additive is the positive electrode active material additive according to any one of claims 1 to 2 or the positive electrode active material additive prepared by the preparation method according to any one of claims 3 to 7.

10. The positive electrode lead paste for lead-acid batteries according to claim 9, characterized in that: The mass percentage of the positive electrode active material additive in the positive electrode lead paste of the battery is 0.1-0.8%.

Citation Information

Cited By

  • Lead-acid battery positive electrode additive derived from rice hull ash and preparation method of lead-acid battery positive electrode additive

    CN122659118A