Used for CO x Coupled catalysts, preparation methods and applications of hydrogenation to low-carbon olefins

By mixing boron-doped modified ZSM-5 molecular sieves with metal composite oxides to form a coupled catalyst with a layered stacked structure, the problem of poor stability of catalysts for direct COx hydrogenation to low-carbon olefins was solved, and high selectivity and stable catalytic performance were achieved.

CN118022823BActive Publication Date: 2026-11-17SHANGHAI ADVANCED RES INST CHINESE ACADEMY OF SCI +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410055988.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-15
Publication Date
2026-11-17
Estimated Expiration
2044-01-15

AI Technical Summary

Technical Problem

Existing catalysts for the direct hydrogenation of COx to produce low-carbon olefins suffer from poor reaction stability. In particular, the active components of oxides are prone to migration and catalyst deactivation under high temperature and reducing atmosphere, and microporous molecular sieves are prone to carbon deposition and deactivation.

Method used

Boron-doped modified ZSM-5 molecular sieves were physically mixed with metal composite oxides. The particle size and acid distribution of the molecular sieves were controlled by changing the amount of boron source added, forming a coupled catalyst with a layered stacked structure.

Benefits of technology

It significantly improves catalyst lifetime and low-carbon olefin selectivity, exhibiting high reaction stability and selectivity, and is suitable for COx hydrogenation to low-carbon olefins reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118022823B_ABST
    Figure CN118022823B_ABST
Patent Text Reader

Abstract

This invention provides a method for CO x This invention relates to a coupled catalyst for the hydrogenation of low-carbon olefins, its preparation method, and its application. The preparation method of the coupled catalyst includes the following steps: S1, providing a metal composite oxide and boron-doped modified ZSM-5 molecular sieve; S2, physically mixing the metal composite oxide and the boron-doped modified ZSM-5 molecular sieve, then pressing and granulating the mixture to obtain the coupled catalyst. This invention uses boron doping to modify ZSM-5 molecular sieve. By changing the amount of boron source added, the particle size and acid distribution of the ZSM-5 molecular sieve can be effectively controlled, resulting in an average particle size of 0.3–20 μm and a morphology of layered twinned crystals. The coupled catalyst prepared by mixing boron-doped modified ZSM-5 molecular sieve with a metal composite oxide is applied to CO2 production. x In the catalytic reaction of hydrogenation to produce low-carbon olefins, it exhibits high selectivity for low-carbon olefins and high reaction stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of heterogeneous catalyst technology, and specifically relates to a catalyst for CO2. x Coupled catalysts, preparation methods and applications of hydrogenation to low-carbon olefins. Background Technology

[0002] Low-carbon olefins (ethylene, propylene, and butene), as fundamental bulk chemical raw materials, have a huge market demand and have attracted widespread attention. Currently, low-carbon olefins are mainly produced through naphtha cracking and coal-to-methanol processes, both of which rely on fossil resources such as petroleum and coal. The catalytic conversion of CO2 to low-carbon olefins is one of the effective ways to recycle carbon resources. Traditional thermocatalytic CO2 hydrogenation to low-carbon olefins mainly uses modified Fischer-Tropsch catalysts. In this process, low-carbon olefins are produced through a reverse water-gas shift (RWGS) reaction, passing through CO intermediates and a Fischer-Tropsch synthesis (FTS) following the Anderson-Schulz-Flory (ASF) distribution. The catalysts used are mainly alkali metal-modified iron-based catalysts. These catalysts generally have high catalytic activity, but the selectivity of low-carbon olefin products is limited by the ASF distribution, generally below 58%.

[0003] In recent years, literature has reported various oxide / molecular sieve bifunctional catalysts for CO2. x Hydrogenation to produce low-carbon olefins follows a methanol intermediate catalytic pathway: first, CO... x The process involves reducing CO2 to oxygen-containing intermediates such as methanol via metal oxides. These intermediates then migrate into the molecular sieve channels and undergo a C-C coupling reaction via methanol-to-olefins (MTO) to generate low-carbon olefins. This pathway can selectively convert CO2. x It produces low-carbon olefins with a selectivity of over 80%. However, it is used for CO2 production. x Coupled catalysts for the hydrogenation of light olefins follow a methanol-mediated route, using microporous SAPO-34 as the molecular sieve component. However, due to the diffusion limitations imposed by the micropores, SAPO-34 is prone to carbon deposition and deactivation, restricting its further application. Furthermore, the high temperatures and reducing atmospheres during the reaction process easily cause active components on oxides, such as Zn, to migrate to the molecular sieve, further leading to catalyst deactivation. Therefore, catalyst design and preparation remain significant challenges in this field, especially the construction of highly stable coupled catalytic systems.

[0004] ZSM-5 molecular sieves possess large, three-dimensional interlocking ten-membered ring channels. This channel structure enhances their resistance to carbon deposition, and the silica-to-alumina ratio of the framework can be adjusted over a wide range, making them easily modifiable. They are commonly used as catalysts for methanol-to-hydrocarbon (MTH) production. Although high-silica ZSM-5 molecular sieves are used as methanol-to-propylene (MTP) catalysts due to their high shape selectivity and stability (see patent CN112794338B), they are rarely used for CO production. x In the direct hydrogenation to low-carbon olefins reaction, Li et al. employed a multiple silanization strategy to design a ZnZrOx & Bio-ZSM-5-Si coupled catalyst, operating at 380 °C, 3 MPa, and 2000 mL gcat. -1 h -1 Under the condition, C2 = -C4 = The selectivity was 64.4%, the total C2-C4 selectivity was 94.5%, the CH4 selectivity was 5.5%, and the aromatic selectivity was <1% (ACSSustainable Chem.Eng. 2021, 9, 6446-6458). However, this method leads to a decrease in the catalytic activity and reaction stability of the bifunctional catalyst.

[0005] Therefore, it is necessary to develop a more efficient oxide / ZSM-5 catalyst and apply it to CO. x The direct hydrogenation reaction to produce light olefins with high selectivity remains a technical problem that urgently needs to be solved. Summary of the Invention

[0006] In view of the shortcomings of the prior art described above, the object of the present invention is to provide a CO x Coupled catalysts, preparation methods, and applications for hydrogenation to low-carbon olefins, aimed at solving existing problems in CO2 production. x Catalysts for the direct hydrogenation to produce low-carbon olefins suffer from poor reaction stability.

[0007] To achieve the above and other related objectives, the present invention provides a method for CO x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, the method comprising the following steps:

[0008] S1. Provide metal composite oxides and boron-doped modified ZSM-5 molecular sieves;

[0009] S2. The metal composite oxide and boron-doped modified ZSM-5 molecular sieve are physically mixed, then pressed into tablets and granulated to obtain the coupled catalyst.

[0010] Preferably, the metal composite oxide in step S1 includes ZnCrO x ZnAlO xZnGa2O4, ZnZrO x ZnFeO x One or more of them.

[0011] Preferably, the preparation method of the boron-doped modified ZSM-5 molecular sieve in step S1 includes the following steps:

[0012] S11. Mix the silicon source, aluminum source, template agent, boron source and seed crystal to obtain an initial mixture;

[0013] S12. The initial mixture is subjected to crystallization treatment, then washed and dried to obtain ZSM-5 molecular sieve precursor;

[0014] S13. The ZSM-5 molecular sieve precursor is calcined and then subjected to ammonium exchange to obtain boron-doped modified ZSM-5 molecular sieve.

[0015] Preferably, the molar ratio of the silicon source, the aluminum source, the template agent and the boron source in step S11 is 1:(0.005~0.1):(0.05~0.1):(0.1~0.5), wherein the silicon source is SiO2, the aluminum source is Al2O3 and the boron source is B2O3.

[0016] Preferably, in step S11, the amount of seed crystal added is 0-5 wt%, based on the dry weight of the SiO2.

[0017] Preferably, the silicon source in step S11 is selected from one or more of silica sol, activated silica, silica fume, and tetraethyl orthosilicate.

[0018] Preferably, the aluminum source in step S11 is selected from one or more of sodium aluminate, boehmite, activated alumina, aluminum isopropoxide, and aluminum hydroxide.

[0019] Preferably, the template agent in step S11 is selected from one or more of tetrapropylammonium bromide, tetrapropylammonium hydroxide, and n-butylamine.

[0020] Preferably, the boron source in step S11 is selected from one or more of boric acid and boron oxide.

[0021] Preferably, the crystallization treatment temperature in step S12 is 150–220°C, and the crystallization treatment time is 6–96 h.

[0022] Preferably, the washing in step S12 involves washing with water until the solution is neutral.

[0023] Preferably, the drying temperature in step S12 is 50–120°C.

[0024] Preferably, the roasting temperature in step S13 is 450-600°C, and the roasting time is 0.5-8 hours.

[0025] Preferably, the average particle size of the boron-doped modified ZSM-5 molecular sieve in step S13 is 0.3 to 20 μm.

[0026] Preferably, the boron-doped modified ZSM-5 molecular sieve in step S13 is a twin.

[0027] This invention provides a CO2 preparation method prepared according to the above-described method. x Coupled catalysts for hydrogenation to produce low-carbon olefins.

[0028] In addition, the present invention also provides a CO prepared by the preparation method described above. x Application of coupled catalysts for hydrogenation to low-carbon olefins, wherein the coupled catalysts are used in CO x Applications in the catalytic reaction of hydrogenation to produce low-carbon olefins.

[0029] As described above, the present invention is for CO x The coupled catalysts, preparation methods, and applications of hydrogenation to low-carbon olefins have the following beneficial effects:

[0030] This invention uses boron doping to modify ZSM-5 molecular sieves. By changing the amount of boron source added, the particle size, morphology and acid distribution of ZSM-5 molecular sieves can be effectively controlled. The average particle size of the boron-doped modified ZSM-5 molecular sieves prepared is 0.3 to 20 μm, and the morphology is a layered stacked structure. Furthermore, the preparation method is simple, environmentally friendly and low in cost.

[0031] This invention significantly improves the lifetime of the coupled catalyst prepared by mixing boron-doped modified ZSM-5 molecular sieve with a metal composite oxide, followed by tableting and granulation. Its application in CO2... x In the catalytic reaction of hydrogenation to produce low-carbon olefins, it exhibits high selectivity for low-carbon olefins and high reaction stability, and has broad application prospects in syngas conversion and CO2 resource utilization. Attached Figure Description

[0032] Figure 1 The image shown is a SEM image of the boron-doped modified ZSM-5 molecular sieve prepared in Example 1 of this invention.

[0033] Figure 2 The image shown is an XRD image of the boron-doped modified ZSM-5 molecular sieve prepared in Example 1 of this invention.

[0034] Figure 3 The image shown is a SEM image of the boron-doped modified ZSM-5 molecular sieve prepared in Example 2 of this invention.

[0035] Figure 4 The image shown is an XRD image of the boron-doped modified ZSM-5 molecular sieve prepared in Example 2 of this invention.

[0036] Figure 5 The image shown is a SEM image of the boron-doped modified ZSM-5 molecular sieve prepared in Example 3 of this invention.

[0037] Figure 6 The image shown is a SEM image of the undoped ZSM-5 molecular sieve prepared in Comparative Example 1 of this invention.

[0038] Figure 7 The image shown is an XRD image of the undoped ZSM-5 molecular sieve prepared in Comparative Example 1 of this invention. Detailed Implementation

[0039] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.

[0040] In order to improve the CO in existing technologies x To address the problem of poor reaction stability in direct hydrogenation catalysts for producing low-carbon olefins, this invention provides a simple, efficient, and environmentally friendly method for CO2 production. x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, the method comprising the following steps:

[0041] S1. Provide metal composite oxides and boron-doped modified ZSM-5 molecular sieves;

[0042] S2. The metal composite oxide and boron-doped modified ZSM-5 molecular sieve are physically mixed, then pressed into tablets and granulated to obtain the coupled catalyst.

[0043] Specifically, in the specific embodiments of the present invention, by changing the amount of boron source added, the particle size and acid distribution of ZSM-5 molecular sieve can be effectively controlled. The lifetime of the coupled catalyst prepared by mixing boron-doped modified ZSM-5 molecular sieve with metal composite oxide, pressing, and granulating is significantly improved, and its application in CO2... x In the catalytic reaction of hydrogenation to produce low-carbon olefins, it exhibits high selectivity for low-carbon olefins and high reaction stability.

[0044] As an example, the metal composite oxide in step S1 includes ZnCrO x ZnAlO xZnGa2O4, ZnZrO x ZnFeO x One or more of them.

[0045] Specifically, metal composite oxides refer to oxides in which two metals coexist. Since the molar ratio of the two metals in a composite oxide cannot be determined, it is represented by x.

[0046] As an example, the preparation method of boron-doped modified ZSM-5 molecular sieve in step S1 includes the following steps:

[0047] S11. Mix the silicon source, aluminum source, template agent, boron source and seed crystal to obtain an initial mixture;

[0048] S12. The initial mixture is crystallized, then washed and dried to obtain the ZSM-5 molecular sieve precursor.

[0049] S13. The ZSM-5 molecular sieve precursor was calcined and then subjected to ammonium exchange to obtain boron-doped modified ZSM-5 molecular sieve.

[0050] Specifically, in this embodiment of the invention, the ZSM-5 molecular sieve is modified by doping with the non-metallic element boron. By changing the amount of boron source added, the particle size and acid distribution of the ZSM-5 molecular sieve can be effectively controlled. The ammonium exchange in step S13 converts the synthesized ZSM-5 molecular sieve into a hydrogen-form ZSM-5 molecular sieve through ammonium nitrate ion exchange. The specific steps are as follows: the ZSM-5 molecular sieve is dispersed in a 1M NH4NO3 solution, stirred vigorously for 1 hour, dried, and then calcined in a muffle furnace to convert it into a hydrogen-form ZSM-5 molecular sieve.

[0051] As an example, in step S11, the molar ratio between the silicon source, aluminum source, template agent and boron source is 1:(0.005~0.1):(0.05~0.1):(0.1~0.5), where the silicon source is SiO2, the aluminum source is Al2O3 and the boron source is B2O3.

[0052] Specifically, the molar ratio between the silicon source, aluminum source, template agent, and boron source in step S11 can be any value within a range such as 1:0.005:0.05:0.1, 1:0.005:0.05:0.5, 1:0.005:0.1:0.1, 1:0.005:0.1:0.5, 1:0.01:0.05:0.1, 1:0.01:0.05:0.5, 1:0.01:0.1:0.1, 1:0.01:0.1:0.5, etc., and can be adjusted according to actual conditions. The amount of boron source added will affect the pH value, size, morphology, crystallinity, and Al distribution of the prepared boron-doped modified ZSM-5 molecular sieve precursor, and thus affect the catalytic performance of the finally prepared coupled catalyst obtained by the boron-doped modified ZSM-5 molecular sieve and metal composite oxide.

[0053] As an example, based on the dry weight of the silicon source, the amount of seed crystal added is 0–5 wt%.

[0054] Specifically, based on the dry weight of the silicon source, the amount of seed crystals added can be any value within the range of 0, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, etc. The seed crystals are conventional MFI type molecular sieves, including one or a combination of ZSM-5 molecular sieves and Silicate-1 molecular sieves.

[0055] As an example, in step S11, the silicon source is selected from one or more of silica sol, activated silica, fumed silica, and tetraethyl orthosilicate.

[0056] As an example, in step S11, the aluminum source is selected from one or more of sodium aluminate, boehmite, activated alumina, aluminum isopropoxide, and aluminum hydroxide.

[0057] As an example, in step S11, the template agent is selected from one or more of tetrapropylammonium bromide, tetrapropylammonium hydroxide, and n-butylamine.

[0058] As an example, in step S11, the boron source is selected from one or more of boric acid and boron oxide.

[0059] As an example, the crystallization temperature in step S12 is 150–220°C, and the crystallization time is 6–96 h.

[0060] Specifically, the temperature of the crystallization treatment in step S12 can be any value within the range of 150℃, 160℃, 180℃, 200℃, 220℃, etc., and the time of the crystallization treatment can be any value within the range of 6h, 18h, 30h, 42h, 48h, 60h, 72h, 84h, 96h, etc.; in addition, the crystallization treatment can be a single crystallization or a double crystallization.

[0061] As an example, in step S12, washing involves washing with water until the solution is neutral.

[0062] As an example, the drying temperature in step S12 is 50–120°C.

[0063] Specifically, the drying temperature in step S12 can be any value within a range such as 50°C, 60°C, 80°C, 100°C, 110°C, or 120°C.

[0064] As an example, the roasting temperature in step S13 is 450–600°C, and the roasting time is 0.5–8 hours.

[0065] Specifically, the roasting temperature in step S13 can be any value within the range of 450℃, 500℃, 550℃, 600℃, etc.; the roasting time can be any value within the range of 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc.

[0066] As an example, the average particle size of the boron-doped modified ZSM-5 molecular sieve obtained in step S13 is 0.3–20 μm.

[0067] Specifically, the average particle size of the boron-doped modified ZSM-5 molecular sieve in step S13 can be any value within any range, such as 0.3μm, 0.5μm, 1.0μm, 1.5μm, 2.0μm, 2.5μm, 3μm, 20μm, etc.

[0068] As an example, the boron-doped modified ZSM-5 molecular sieve obtained in step S13 is a twin.

[0069] The present invention also provides a method for CO x A coupled catalyst for the hydrogenation of low-carbon olefins, which is prepared by the above-described preparation method.

[0070] In addition, the present invention also provides a coupling catalyst prepared by the above preparation method in CO x Applications in the catalytic reaction of hydrogenation to produce low-carbon olefins.

[0071] Specifically, when x is 1, this invention provides an application of a coupled catalyst in the catalytic reaction of syngas conversion to low-carbon olefins; the catalytic reaction is carried out in a tubular fixed-bed reactor, where 1.0 g of the coupled catalyst is loaded into the middle of a stainless steel tube with an inner diameter of 1 cm, and the coupled catalyst is pre-exposed to a pure H2 flow of 0.1 MPa (25 mL / min). -1 The mixture was reduced in situ at 350℃ for 4 hours, then the gas was switched to a mixture of carbon dioxide and hydrogen (CO:H2 = 1:1), and the mixture was subjected to reduction at 300℃, 1.0 MPa, and 1200 mL g. cat -1 h-1 The reaction was carried out for 20 hours under space velocity conditions.

[0072] When x is 2, this invention provides an application of a coupled catalyst in the catalytic reaction of CO2 hydrogenation to produce low-carbon olefins; the catalytic reaction is carried out in a tubular fixed-bed reactor, with 1.0 g of the coupled catalyst loaded into the middle of a stainless steel tube with an inner diameter of 1 cm, and the coupled catalyst pre-exposed to a pure H2 flow of 0.1 MPa (25 mL / min). -1 The mixture was reduced in situ at 350℃ for 4 hours, then the gas was switched to a mixture of carbon dioxide and hydrogen (CO2 to H2 volume ratio of 1:3), and the mixture was subjected to 300℃, 1.0 MPa, and 1200 mL g of hydrogen. cat -1 h -1 The reaction was carried out for 20 hours under space velocity conditions.

[0073] To better understand the CO used in this invention x The coupled catalysts, preparation methods, and applications of hydrogenation to low-carbon olefins are described below with reference to specific embodiments. x The coupled catalysts, preparation methods and applications of hydrogenation to low-carbon olefins are described. It should be noted that these examples are merely descriptive and do not limit the invention in any way.

[0074] Example 1

[0075] This embodiment provides a method for CO x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, comprising the following steps:

[0076] S1, providing metal composite oxides (ZnCrO) x ) and boron-doped modified ZSM-5 molecular sieve;

[0077] The preparation method of boron-doped modified ZSM-5 molecular sieve includes the following steps:

[0078] S11. Weigh 5.4g of silica, 0.05g of sodium aluminate, 5.5g of 25% tetrapropylammonium hydroxide aqueous solution, 1.8g of boric acid and 0.05g of seed crystals and mix them to obtain the initial mixture;

[0079] S12. The initial mixture was transferred to a 100 mL reactor lined with para-polystyrene and crystallized at 205 °C for 30 h. After the reaction was completed, the mixture was cooled, filtered, washed with water until neutral, and then dried in an oven at 80 °C for 12 h to obtain the ZSM-5 molecular sieve precursor.

[0080] S13. The ZSM-5 molecular sieve precursor was calcined at 550℃ for 4h to remove the template agent. After ammonium exchange, boron-doped modified ZSM-5 molecular sieve was obtained and named Z5-1.

[0081] S2, the metal composite oxide (ZnCrO) x ZnCrO and boron-doped modified ZSM-5 molecular sieve (Z5-1) were physically mixed in an agate mortar at a mass ratio of 1:1 for 10 min. The mixture was then pressed into tablets, granulated, and sieved to 40-60 mesh under a pressure of 15 MPa to obtain the coupled catalyst, named ZnCrO. x / Z5-1.

[0082] See Figure 1 This is a SEM image of the boron-doped modified ZSM-5 molecular sieve prepared in this embodiment. As can be seen from the image, Z5-1 exhibits a layered stacked structure with an average particle size of approximately 1.4 μm; see reference... Figure 2 The image shows the XRD pattern of the boron-doped modified ZSM-5 molecular sieve prepared in this embodiment. As can be seen from the image, Z5-1 exhibits a typical MFI structure.

[0083] Example 2

[0084] This embodiment provides a method for CO x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, comprising the following steps:

[0085] S1, providing metal composite oxides (ZnAlO) x ) and boron-doped modified ZSM-5 molecular sieve;

[0086] The preparation method of boron-doped modified ZSM-5 molecular sieve includes the following steps:

[0087] S11. Weigh 5.4g of activated silica, 0.1g of boehmite, 8.5g of 25% tetrapropylammonium hydroxide aqueous solution and 0.9g of boron oxide and mix them to obtain the initial mixture;

[0088] S12. The initial mixture was transferred to a 100 mL reactor lined with para-polystyrene and crystallized at 190 °C for 48 h. After the reaction was completed, the mixture was cooled, filtered, washed with water until neutral, and then dried in an oven at 60 °C for 12 h to obtain the ZSM-5 molecular sieve precursor.

[0089] S13. The ZSM-5 molecular sieve precursor was calcined at 500℃ for 6 hours to remove the template agent. After ammonium exchange, boron-doped modified ZSM-5 molecular sieve was obtained and named Z5-2.

[0090] S2, the metal composite oxide (ZnAlO) xZnAlO and boron-doped modified ZSM-5 molecular sieve (Z5-2) were physically mixed in an agate mortar at a mass ratio of 1:1. The mixture was then pressed into tablets, granulated, and sieved to 40-60 mesh to obtain the coupled catalyst, named ZnAlO. x / Z5-2.

[0091] See Figure 3 This is a SEM image of the boron-doped modified ZSM-5 molecular sieve prepared in this embodiment. As can be seen from the image, Z5-2 exhibits a layered stacked structure with an average particle size of approximately 1.1 μm; see reference... Figure 4 The image shows the XRD pattern of the boron-doped modified ZSM-5 molecular sieve prepared in this embodiment. As can be seen from the image, Z5-2 exhibits a typical MFI structure.

[0092] Example 3

[0093] This embodiment provides a method for CO x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, comprising the following steps:

[0094] S1, providing metal composite oxides (ZnGa2O) x ) and boron-doped modified ZSM-5 molecular sieve;

[0095] The preparation method of boron-doped modified ZSM-5 molecular sieve includes the following steps:

[0096] S11. Weigh 15g of silica sol, 0.7g of aluminum hydroxide, 11.2g of tetrapropylammonium bromide and 0.6g of boric acid and mix them to obtain the initial mixture;

[0097] S12. The initial mixture was transferred to a 100 mL reactor lined with para-polystyrene and crystallized at 150 °C for 48 h. After crystallization at 200 °C for another 48 h, the mixture was removed, cooled, and filtered. The mixture was then washed with water until neutral and dried in an oven at 50 °C for 12 h to obtain the ZSM-5 molecular sieve precursor.

[0098] S13. The ZSM-5 molecular sieve precursor was calcined at 450℃ for 8 hours to remove the template agent. After ammonium exchange, boron-doped modified ZSM-5 molecular sieve was obtained and named Z5-3.

[0099] S2, the metal composite oxide (ZnGa2O) x ZnGa₂O and boron-doped modified ZSM-5 molecular sieve (Z5-3) were physically mixed in an agate mortar at a mass ratio of 1:1. The mixture was then pressed into tablets, granulated, and sieved to 40-60 mesh to obtain the coupled catalyst, named ZnGa₂O. x / Z5-3.

[0100] See Figure 5 The image shows a SEM image of the boron-doped modified ZSM-5 molecular sieve prepared in this embodiment. As can be seen from the image, Z5-3 exhibits a layered stacked structure with an average particle size of approximately 15.1 μm.

[0101] Example 4

[0102] This embodiment provides a method for CO x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, comprising the following steps:

[0103] S1, providing metal composite oxides (ZnZrO) x ) and boron-doped modified ZSM-5 molecular sieve;

[0104] The preparation method of boron-doped modified ZSM-5 molecular sieve includes the following steps:

[0105] S11. Weigh 19.0g of tetraethyl orthosilicate, 0.04g of activated alumina, 6g of n-butylamine and 3.1g of boron oxide and mix them to obtain the initial mixture;

[0106] S12. The initial mixture was transferred to a 100 mL reactor lined with para-polystyrene and crystallized at 220 °C for 12 h. After the reaction was completed, the mixture was cooled, filtered, washed with water until neutral, and then dried in an oven at 100 °C for 12 h to obtain the ZSM-5 molecular sieve precursor.

[0107] S13. The ZSM-5 molecular sieve precursor was calcined at 650℃ for 1 hour to remove the template agent. After ammonium exchange, boron-doped modified ZSM-5 molecular sieve was obtained and named Z5-4.

[0108] S2, the metal composite oxide (ZnZrO) x ZnZrO4 and boron-doped modified ZSM-5 molecular sieve (Z5-4) were physically mixed in an agate mortar at a mass ratio of 1:1. The mixture was then pressed into tablets, granulated, and sieved to 40-60 mesh to obtain the coupled catalyst, named ZnZrO4. x / Z5-4.

[0109] Example 5

[0110] This embodiment provides a method for CO x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, comprising the following steps:

[0111] S1, providing metal composite oxides (ZnFeO) x ) and boron-doped modified ZSM-5 molecular sieve;

[0112] The preparation method of boron-doped modified ZSM-5 molecular sieve includes the following steps:

[0113] S11. Weigh 5.4g of activated silicon dioxide, 0.2g of aluminum isopropoxide, 7.5g of 25% tetrapropylammonium hydroxide aqueous solution, 2g of boric acid and 0.1g of seed crystals and mix them to obtain the initial mixture;

[0114] S12. The initial mixture was transferred to a 100 mL reactor lined with para-polystyrene and crystallized at 180 °C for 48 h. After crystallization at 220 °C for 6 h, the mixture was removed, cooled, filtered, washed with water until neutral, and then dried in an oven at 70 °C for 12 h to obtain the ZSM-5 molecular sieve precursor.

[0115] S13. The ZSM-5 molecular sieve precursor was calcined at 580℃ for 3h to remove the template agent. After ammonium exchange, boron-doped modified ZSM-5 molecular sieve was obtained and named Z5-5.

[0116] S2, the metal composite oxide (ZnFeO) x ZnFeO and boron-doped modified ZSM-5 molecular sieve (Z5-5) were physically mixed in an agate mortar at a mass ratio of 1:1. The mixture was then pressed into tablets, granulated, and sieved to 40-60 mesh to obtain the coupled catalyst, named ZnFeO. x / Z5-5.

[0117] Example 6

[0118] This embodiment provides a method for CO x The preparation method of the coupling catalyst for hydrogenation to low-carbon olefins differs from that in Example 1 in that the amount of boric acid added in the preparation method of the boron-doped modified ZSM-5 molecular sieve is 0.6 g. Other methods and steps are the same as in Example 1 and will not be repeated here. The prepared boron-doped modified ZSM-5 molecular sieve is named Z5-6, and the coupling catalyst is named ZnCrO. x / Z5-6.

[0119] Example 7

[0120] This embodiment provides a method for CO x The preparation method of the coupling catalyst for hydrogenation to low-carbon olefins differs from that in Example 1 in that the amount of boric acid added in the preparation method of the boron-doped modified ZSM-5 molecular sieve is 3.0 g. Other methods and steps are the same as in Example 1 and will not be repeated here. The prepared boron-doped modified ZSM-5 molecular sieve is named Z5-7, and the coupling catalyst is named ZnCrO. x / Z5-7.

[0121] Comparative Example 1

[0122] This comparative example provides a method for CO x The preparation method of the coupling catalyst for hydrogenation to low-carbon olefins differs from that in Example 1 in that the molecular sieve provided in step S1 is ZSM-5 molecular sieve, and the preparation method differs from that of the boron-doped modified ZSM-5 molecular sieve in Example 1. Other methods and steps differ from those in Example 1 and will not be elaborated further. The prepared coupling catalyst is named ZnCrO. x / Z5-D1.

[0123] The preparation method of ZSM-5 molecular sieve in this comparative example differs from the preparation method of boron-doped modified ZSM-5 molecular sieve in Example 1 in that boric acid was not added in step S11. Other methods and steps are the same as those in the preparation method of boron-doped modified ZSM-5 molecular sieve in Example 1, and will not be repeated here.

[0124] The ZSM-5 molecular sieve prepared in this comparative example was analyzed by SEM and XRD. (See attached document.) Figure 6 The image shows a SEM image of the undoped ZSM-5 molecular sieve prepared in this comparative example. As can be seen from the image, Z5-D1 exhibits an irregular spherical morphology and a non-uniform particle size distribution. (See also...) Figure 7 The image shows the XRD pattern of the undoped ZSM-5 molecular sieve prepared in this comparative example. As can be seen from the image, Z5-D1 exhibits a typical MFI structure. Therefore, the morphology and particle size of ZSM-5 molecular sieve can be effectively controlled by doping with boron.

[0125] Application Example 1

[0126] This application example provides an application of a coupled catalyst in the catalytic reaction of CO2 hydrogenation to produce low-carbon olefins. The coupled catalysts prepared in Examples 1 to 7 and Comparative Example 1 are applied to the catalytic reaction of CO2 hydrogenation to produce low-carbon olefins.

[0127] Specifically, the catalytic reaction was carried out in a tubular fixed-bed reactor. 1.0 g of the coupled catalyst was loaded into the center of a stainless steel tube with an inner diameter of 1 cm. The coupled catalyst was pre-exposed to a pure H2 flow at 0.1 MPa (25 mL / min). -1 The mixture was reduced in situ at 350℃ for 4 hours, then the gas was switched to a mixture of carbon dioxide and hydrogen (CO2 to H2 volume ratio of 1:3), and the mixture was subjected to 300℃, 1.0 MPa, and 1200 mL g of hydrogen. cat -1 h -1The reaction was carried out at space velocity for 20 h. The reaction products were monitored by online gas chromatography. A Shimadzu GC-2014C gas chromatograph equipped with a flame ionization detector (FID) was connected to Plot-Q and HP-Pona capillary columns. H2, CH4, N2, CO and CO2 were detected by a Shimadzu GC-2014C gas chromatograph equipped with TCD and TDX-01 columns. The reaction results are shown in Table 1.

[0128] Table 1. Test results of the coupled catalysts prepared in Examples 1-7 and Comparative Example 1 applied to the catalytic reaction of CO2 hydrogenation to low-carbon olefins.

[0129]

[0130] Among them, C2 = -C4 = This refers to low-carbon olefins (ethylene, propylene, and butene), C2 0 -C4 0 Refers to low-carbon alkanes (ethane, propane, and butane), C 5+ It refers to non-aromatic hydrocarbon compounds containing ≥5 carbon atoms; Aromatic refers to aromatic hydrocarbons.

[0131] As shown in Table 1, the coupled catalyst prepared by mixing metal composite oxides with boron-doped modified ZSM-5 molecular sieves in this invention exhibits low methane selectivity (0.3%–0.6%), high CO2 conversion, and low-carbon olefin selectivity. In contrast, compared to Example 1, the coupled catalyst in Comparative Example 1, prepared by mixing undoped ZSM-5 molecular sieves with metal composite oxides, showed significantly reduced CO2 conversion and low-carbon olefin selectivity. These results indicate that the boron-doped modified ZSM-5 molecular sieves prepared in this invention effectively form a coupled catalyst for CO2 catalysis. x It exhibits excellent catalytic performance in the hydrogenation to produce low-carbon olefins.

[0132] Application Example 2

[0133] This application example provides the application of a coupled catalyst in the catalytic reaction of syngas conversion to low-carbon olefins. The coupled catalysts prepared in Examples 1 to 7 and Comparative Example 1 are applied to the catalytic reaction of syngas conversion to low-carbon olefins.

[0134] Specifically, the above reaction was carried out in a tubular fixed-bed reactor. 1.0 g of the coupled catalyst was loaded into the middle of a stainless steel tube with an inner diameter of 1 cm. The coupled catalyst was pre-exposed to a pure H2 flow at 0.1 MPa (25 mL / min). -1 The mixture was reduced in situ at 350℃ for 4 hours, then the gas was switched to a mixture of carbon dioxide and hydrogen (CO:H2 = 1:1), and the mixture was subjected to reduction at 300℃, 1.0 MPa, and 1200 mL g. cat-1 h -1 The reaction was carried out at space velocity for 20 h. The reaction products were monitored by online gas chromatography. A Shimadzu GC-2014C gas chromatograph equipped with a flame ionization detector (FID) was connected to Plot-Q and HP-Pona capillary columns. H2, CH4, N2, CO and CO2 were detected by a Shimadzu GC-2014C gas chromatograph equipped with TCD and TDX-01 columns. The reaction results are shown in Table 2.

[0135] Table 2. Test results of the coupled catalysts prepared in Examples 1-7 and Comparative Example 1 applied to the catalytic reaction of syngas conversion to low-carbon olefins.

[0136]

[0137] As can be seen from the results in Table 2, the coupled catalyst prepared by mixing metal composite oxide with boron-doped modified ZSM-5 molecular sieve in this invention has high CO conversion rate and low-carbon olefin selectivity. Compared with Example 1, the coupled catalyst of Comparative Example 1 after mixing undoped ZSM-5 molecular sieve with metal composite oxide has significantly reduced CO conversion rate and low-carbon olefin selectivity. In general, the coupled catalyst synthesized in this invention has excellent catalytic performance in the catalytic reaction of COx hydrogenation to low-carbon olefins.

[0138] In summary, this invention uses boron doping to modify ZSM-5 molecular sieves. By changing the amount of boron source added, the particle size and acid distribution of the ZSM-5 molecular sieve can be effectively controlled. The average particle size of the prepared boron-doped modified ZSM-5 molecular sieve is 0.3–3 μm, and the morphology exhibits a layered stacked structure. Furthermore, the preparation method is simple, environmentally friendly, and low-cost. The coupling catalyst prepared by mixing boron-doped modified ZSM-5 molecular sieves with metal composite oxides, pressing, and granulating significantly improves the lifetime of the catalyst. Its application in CO2... x In the catalytic reaction of hydrogenation to produce low-carbon olefins, this invention exhibits high selectivity and high reaction stability, showing broad application prospects in syngas conversion and CO2 resource utilization. Therefore, this invention effectively overcomes the various shortcomings of existing technologies and has high industrial application value.

[0139] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A method for CO x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, characterized in that, The preparation method of the coupling catalyst includes the following steps: S1. Provide a metal composite oxide and a boron-doped modified ZSM-5 molecular sieve; the metal composite oxide includes ZnCrO x ZnAlO x ZnGa2O4, ZnZrO x ZnFeO x One or more of the following; The preparation method of the boron-doped modified ZSM-5 molecular sieve includes the following steps: S11. Mix the silicon source, aluminum source, template agent, boron source, and seed crystal to obtain an initial mixture; the molar ratio between the silicon source, aluminum source, template agent, and boron source is 1:(0.005~0.1):(0.05~0.1):(0.1~0.5), wherein the silicon source is calculated as SiO2, the aluminum source as Al2O3, and the boron source as B2O3; based on the dry weight of the SiO2, the amount of seed crystal added is 0~5wt%; S12. The initial mixture is subjected to crystallization treatment, then washed and dried to obtain ZSM-5 molecular sieve precursor; S13. The ZSM-5 molecular sieve precursor is calcined and then subjected to ammonium exchange to obtain boron-doped modified ZSM-5 molecules; the average particle size of the boron-doped modified ZSM-5 molecular sieve is 0.3~20μm; the boron-doped modified ZSM-5 molecular sieve is twinned. S2. The metal composite oxide and boron-doped modified ZSM-5 molecular sieve are physically mixed, then pressed into tablets and granulated to obtain the coupled catalyst.

2. The CO2-based CO2 system according to claim 1 x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, characterized in that: Step S11 includes one or a combination of the following conditions: The silicon source is selected from one or more of silica sol, activated silica, silica fume, and tetraethyl orthosilicate. The aluminum source is selected from one or more of sodium aluminate, boehmite, activated alumina, aluminum isopropoxide, and aluminum hydroxide. The template agent is selected from one or more of tetrapropylammonium bromide, tetrapropylammonium hydroxide, and n-butylamine; The boron source is selected from one or more of boric acid and boron oxide.

3. The CO2 device according to claim 1 x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, characterized in that: Step S12 includes one or a combination of the following conditions: The crystallization treatment temperature is 150~220℃, and the crystallization treatment time is 6~96h; The washing process involves washing with water until the solution is neutral. The drying temperature is 50~120℃.

4. The CO2 device according to claim 1 x A method for preparing a coupled catalyst for hydrogenation to low-carbon olefins, characterized in that: The roasting temperature in step S13 is 450~600℃, and the roasting time is 0.5~8h.

5. A CO2-containing product prepared by the preparation method according to any one of claims 1 to 4. x Coupled catalysts for hydrogenation to produce low-carbon olefins.

6. A CO2-containing product prepared by the preparation method according to any one of claims 1 to 4 x The application of coupled catalysts for hydrogenation to low-carbon olefins is characterized by: The coupling catalyst in CO x Applications in the catalytic reaction of hydrogenation to produce low-carbon olefins.

Citation Information

Patent Citations

  • B-Al-ZSM-5 zeolite catalyst for accumulating nano grains of methanol to olefin as well as preparation method and application thereof

    CN103708497A

  • Zinc-based composite oxide-molecular sieve composite catalyst as well as preparation method and application thereof

    CN117258830A

  • Method for directly producing aromatic hydrocarbons from syngas and for producing low carbon olefins in parallel

    WO2019095405A1