Resin composition for heat dissipation gap filler, heat dissipation gap filler and article
By using maleic anhydride modified polybutadiene, hydroxy modified polybutadiene and thermally conductive filler, combined with antioxidants, the stability of the filler under high temperature and temperature changes in the prior art is solved, and the stability of the filler in the prior art is achieved. High thermal conductivity and stable heat dissipation gap filler.
Patent Information
- Application Number
- CN202280067309.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-26
- Filing Date
- 2022-09-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-09-29
AI Technical Summary
The existing heat dissipation gap fillers are prone to rupture or peel off when exposed to high temperatures for a long time or undergo sharp temperature changes, and there are problems of thermal conductivity and volume shrinkage.
The composition using maleic anhydride modified polybutadiene, hydroxy modified polybutadiene, thermal conductivity filler and antioxidant has an antioxidant content of more than 0.01%, and the thermal conductivity after curing reaches more than 1.0W/m·K , by adjusting the proportion and types of components to improve thermal conductivity and stability.
It significantly reduces the risk of cracking or peeling of fillers under high temperature and temperature changes, maintains high thermal conductivity and stable curing properties, and avoids void and volume shrinkage problems.
Smart Images

Figure BDA0004775071360000171 
Figure BDA0004775071360000181 
Figure BDA0004775071360000191
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition for a heat dissipating gap filler, a heat dissipating gap filler and an article. Background Art
[0002] In recent years, the heat dissipation from electronic devices such as digital home appliances, lithium-ion secondary batteries, and vehicle-mounted power modules has been increasing due to their large capacity and high functionality. On the other hand, in order to miniaturize, lighten, and thinn these electronic devices, the replacement of metal components with resin is underway. Since resin generally has lower thermal conductivity than metal, it is important to efficiently dissipate heat from its components in order to suppress the heat rise of electronic devices.
[0003] Therefore, as a method for efficient heat dissipation, a method of using a filler or adhesive with high thermal conductivity between the components is known. Such a filler or adhesive is called a gap filler, and is generally a material containing a metal oxide with high thermal conductivity in a resin component, but because it is in liquid form, it can be applied in a complex shape and has the characteristic of being able to be automatically installed by a coating device such as a dispenser.
[0004] As the resin component of such gap fillers, silicone or polyurethane has been conventionally used.
[0005] Silicone can have elastomeric properties suitable for this purpose, but when used near electrical contacts such as battery cells, contact failures may occur due to the volatile silicone contained therein and the low molecular weight siloxanes produced therefrom. In addition, since it is a moisture curing reaction, water is sometimes added, but the generation of voids caused by water will lead to a decrease in thermal conductivity. In addition, the volume shrinkage problem caused by the volatilization of volatile silicone, low molecular weight siloxane and water, and the problem of reduced storage stability caused by water separation of the liquid before curing are also pointed out.
[0006] Polyurethane can also exert excellent elastomeric properties, but the isocyanate as its raw material not only has toxic concerns, but also reacts with water to form carbon dioxide voids. Therefore, in order not to generate voids that hinder thermal conductivity, it is necessary to carry out the curing reaction in the absence of water. On the other hand, it is necessary to contain a high concentration of high surface area (small particle size) inorganic filler in the heat dissipation gap filler, but such inorganic filler will inevitably absorb moisture during normal processing, so a thorough and therefore expensive drying process or treatment is required.
[0007] Therefore, various studies have been conducted on heat-dissipating gap fillers using resins other than silicone and polyurethane.
[0008] For example, Patent Document 1 describes “a two-component epoxy resin composition for casting, comprising: a main component, the main component comprising (A) a liquid epoxy resin, (B) an inorganic filler, (C) a phosphate ester wetting dispersant, and (D) a urea compound; and a curing agent component, the curing agent component comprising (E) a curing agent and (F) a curing accelerator, wherein the content of the (C) phosphate ester wetting dispersant is 0.1 to 5 parts by mass relative to 100 parts by mass of the (A) liquid epoxy resin, and the ratio of the (C) phosphate ester wetting dispersant to the (D) urea compound ((C) / (D)) is 0.1 / 1 to 1.5 / 1”, and describes that “a two-component epoxy resin composition for casting in which the filler is difficult to settle, the high thermal conductivity and electrical insulation of the cured product are maintained, and the mechanical strength is excellent, and an electronic component formed by casting the epoxy resin composition”.
[0009] In addition, Patent Document 2 describes a composition, which is "a two-component curable composition that cures and molds a thermally conductive cured product, comprising a first part and a second part, wherein the first part comprises: (i) at least one polymerizable (meth)acrylate monomer component; (ii) a peroxide-based curing agent component; (iii) one or more co-curable components selected from the group consisting of compounds containing primary amines, secondary amines or tertiary amines or -CONHNH- groups; (iv) a stabilizing component; and (v) a filler component, and the second part comprises: (i) at least one polymerizable (meth)acrylate monomer component; (ii) a catalyst component that catalyzes the curing reaction; (iii) a stabilizing component, and (iv) a thermally conductive filler component, at least one part of the composition has a filler component containing a thermally conductive filler", and describes that the composition described in Patent Document 2 is useful for bonding heat-generating components such as electrical components to a substrate such as a heat sink.
[0010] Furthermore, Patent Document 3 describes a thermally conductive gap filler comprising an aziridine-functional polyether polymer and at least 30 volume % of a thermally conductive filler based on the total volume of the gap filler. The thermally conductive gap filler of Patent Document 3 can be suitable for use in electronic applications such as battery components.
[0011] Recently, a curable composition is described in the published patent document 4, which includes a polyol component containing one or more polyols, a functional butadiene component, and a thermally conductive filler present in an amount of at least 20 weight % based on the total weight of the curable composition, and the curable composition has a thermal conductivity of at least 0.5 W / (mK) after curing. It is also described that the curable composition of patent document 4 can be used as a thermally conductive gap filler, for example, and can be suitable for use in electronic technology applications such as battery components.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent document 1: Japanese Patent Application Publication No. 2016-60826.
[0015] Patent Document 2: Japanese Patent Application Publication No. 2007-528437.
[0016] Patent document 3: Japanese Patent Application Publication No. 2020-511732.
[0017] Patent document 4: Japanese Patent Application Publication No. 2022-507500. Summary of the invention
[0018] Problems to be solved by the invention
[0019] However, for the epoxy system of patent document 1, at least when the curing agent described in its embodiment is anhydride, curing at room temperature takes a long time, so it is necessary to cure under high temperature conditions. In addition, usually, liquid epoxy compounds are mostly compounds that are concerned about mutagenicity. The acrylic acid system of patent document 2 cannot be kept under temperature conditions exceeding the decomposition temperature of the peroxide as a curing agent, and in order to obtain stable performance with the cured product, the curing temperature must be strictly managed. In addition, (meth) acrylate compounds are mostly compounds with skin sensitization, and there are concerns about the safety of operators. In patent document 3, there are concerns about the toxicity caused by aziridine, which is usually a water-soluble resin. Therefore, the possibility of containing a large amount of water in the system is high, which will lead to the generation of voids or volume shrinkage.
[0020] It can be said that the gap filler of Patent Document 4 improves the shortcomings of the aforementioned silicone or polyurethane, or even the epoxy, acrylic or aziridine-functional polyether polymers of Patent Documents 1 to 3. However, when exposed to high temperatures for a long time or subjected to rapid temperature changes, it sometimes cracks or peels off.
[0021] Therefore, an object of the present invention is to provide a resin composition for a heat-dissipating gap filler, which can reduce the occurrence of cracks or peeling even when the heat-dissipating gap filler is exposed to high temperature conditions for a long time or is subjected to a sudden temperature change.
[0022] Means for solving problems
[0023] The present inventors have conducted intensive studies and, as a result, have found a resin composition for a heat dissipation gap filler, which is a resin composition for a heat dissipation gap filler comprising maleic anhydride-modified polybutadiene, hydroxyl-modified polybutadiene, a thermally conductive filler, and an antioxidant, wherein the content of the antioxidant is 0.01% by mass or more when the total amount of the resin composition for a heat dissipation gap filler is set to 100% by mass, the thermal conductivity of the resin composition for a heat dissipation gap filler after curing is 1.0 W / m·K or more, and the heat dissipation gap filler can reduce the occurrence of cracks or peeling even when it is exposed to high temperature conditions for a long time or subjected to rapid temperature changes, thereby completing the present invention.
[0024] That is, according to the present invention, there are provided the following resin composition for a heat-dissipating gap filler, a heat-dissipating gap filler, and an article.
[0025] [1] A heat dissipation gap filler resin composition comprising maleic anhydride-modified polybutadiene, hydroxyl-modified polybutadiene, a thermally conductive filler, and an antioxidant, wherein the content of the antioxidant is 0.01% by mass or more when the total amount of the heat dissipation gap filler resin composition is 100% by mass, and the heat conductivity of the heat dissipation gap filler resin composition after curing is 1.0 W / m·K or more.
[0026] [2] The resin composition for heat dissipating gap fillers according to [1] above, wherein the content of the thermally conductive filler is 70% by mass or more when the total amount of the resin composition for heat dissipating gap fillers is 100% by mass.
[0027] [3] The resin composition for heat-dissipating gap fillers according to [1] or [2], wherein the antioxidant includes at least one selected from the group consisting of phenolic antioxidants and phosphorus antioxidants.
[0028] [4] The resin composition for heat-dissipating gap fillers according to [3] above, wherein the antioxidant comprises a phenolic antioxidant.
[0029] [5] The heat-dissipating gap filler resin composition according to any one of [1] to [4], further comprising a curing accelerator.
[0030] [6] The resin composition for heat-dissipating gap fillers according to [5] above, wherein the curing accelerator comprises an amine-based curing accelerator.
[0031] [7] The resin composition for heat-dissipating gap fillers according to [6] above, wherein the pKa of the amine-based curing accelerator is 8.0 or more.
[0032] [8] The heat dissipating gap filler resin composition according to any one of [1] to [7], wherein the heat dissipating gap filler resin composition is a two-component heat dissipating gap filler resin composition.
[0033] [9] The resin composition for heat dissipating gap filler according to [8] above, wherein the resin composition for heat dissipating gap filler comprises liquid A and liquid B, wherein liquid A comprises the maleic anhydride-modified polybutadiene and the thermally conductive filler, and liquid B comprises the hydroxyl-modified polybutadiene and the thermally conductive filler.
[0034]
[10] A heat dissipating gap filler, wherein the heat dissipating gap filler is obtained by curing the resin composition for heat dissipating gap filler according to any one of [1] to [9].
[0035]
[11] An article comprising the heat dissipating gap filler according to
[10] .
[0036] Effects of the Invention
[0037] According to the present invention, it is possible to provide a resin composition for a heat dissipation gap filler, which can reduce the occurrence of cracks or peeling even when the heat dissipation gap filler is exposed to high temperature conditions for a long time or is subjected to a sudden temperature change. DETAILED DESCRIPTION
[0038] Hereinafter, the mode for implementing the present invention will be described in detail. It should be noted that this embodiment is only one embodiment for implementing the present invention, and the present invention is not limited by this embodiment, and various changes in the embodiment can be made within the scope of the gist of the present invention. It should be noted that, if not otherwise specified, the "~" between the numbers in the text means above to below.
[0039] [Resin composition for heat dissipating gap filler]
[0040] The heat dissipation gap filler resin composition of the present embodiment is a heat dissipation gap filler resin composition comprising maleic anhydride-modified polybutadiene, hydroxyl-modified polybutadiene, a thermally conductive filler and an antioxidant. When the total amount of the heat dissipation gap filler resin composition is set to 100 mass%, the content of the antioxidant is 0.01 mass% or more, and the heat conductivity of the heat dissipation gap filler resin composition after curing is 1.0 W / m·K or more.
[0041] The thermal conductivity of the heat dissipation gap filler resin composition of the present embodiment after curing is 1.0 W / m·K or more. From the viewpoint of further improving thermal conductivity, the thermal conductivity of the heat dissipation gap filler resin composition of the present embodiment after curing is preferably 1.5 W / m·K or more, more preferably 2.3 W / m·K or more, further preferably 2.5 W / m·K or more, and further preferably 2.7 W / m·K or more. There is no particular limitation on the upper limit, and for example, it may be 10.0 W / m·K or less, 8.0 W / m·K or less, or 5.0 W / m·K or less.
[0042] For example, by adjusting the type and content of the thermally conductive filler, the type and content of the maleic anhydride-modified polybutadiene and the hydroxy-modified polybutadiene, the thermal conductivity of the heat-dissipating gap filler resin composition of the present embodiment after curing can be within the range of the present embodiment.
[0043] The thermal conductivity of the heat-dissipating gap filler resin composition after curing indicates a value measured by the method described in Examples.
[0044] From the viewpoint of further reducing the occurrence of cracks or peeling of the heat-dissipating gap filler, the hardness of the resin composition for heat-dissipating gap filler of the present embodiment is preferably 80 or less, more preferably 75 or less, and even more preferably 70 or less on the Shore OO scale as measured in accordance with ASTM D2240. The lower limit is not particularly limited, and may be, for example, 40 or more, or 43 or more.
[0045] The hardness in this specification refers to the hardness of a sample prepared by the method described in the Examples.
[0046] From the viewpoint of further reducing the occurrence of cracks or peeling of the heat-dissipating gap filler, the Shore O hardness of the heat-dissipating gap filler resin composition of the present embodiment measured in accordance with ASTM D2240 is preferably 50 or less, more preferably 45 or less, and even more preferably 40 or less. The lower limit is not particularly limited, and for example, may be 10 or more, or 13 or more.
[0047] The heat dissipating gap filler resin composition of the present embodiment is preferably a two-component heat dissipating gap filler resin composition. When the heat dissipating gap filler resin composition is a two-component heat dissipating gap filler resin composition, the storage stability of the heat dissipating gap filler resin composition before curing is further improved.
[0048] When the heat dissipating gap filler resin composition of the present embodiment is a two-component heat dissipating gap filler resin composition, it preferably includes liquid A and liquid B. The liquid A includes maleic anhydride-modified polybutadiene and a thermally conductive filler, and the liquid B includes hydroxyl-modified polybutadiene and a thermally conductive filler.
[0049] Preferably, when the resin composition for heat dissipating gap filler of the present embodiment is cured at room temperature, the maleic anhydride-modified polybutadiene and the hydroxy-modified polybutadiene as the resin components are not mixed during storage but are mixed before use. That is, the liquid A containing maleic anhydride-modified polybutadiene and the liquid B containing hydroxy-modified polybutadiene are stored separately, mixed before use, and then injected and applied, and cured to form a heat dissipating gap filler.
[0050] In the case where the heat dissipating gap filler is a two-component type, from the viewpoint of further improving the supply stability of the pump in the coating device when coating the heat dissipating gap filler, the viscosity of liquid A is preferably 500 Pa·s or less, more preferably 400 Pa·s or less, further preferably 300 Pa·s or less, further preferably 280 Pa·s or less, and from the viewpoint of further improving operability, it is preferably 10 Pa·s or more, more preferably 20 Pa·s or more, further preferably 50 Pa·s or more, further preferably 100 Pa·s or more, further preferably 200 Pa·s or more.
[0051] In the case where the heat dissipating gap filler is a two-liquid type, from the viewpoint of further improving the supply stability of the pump in the coating device when coating the heat dissipating gap filler, the viscosity of liquid B is preferably 500 Pa·s or less, more preferably 400 Pa·s or less, further preferably 300 Pa·s or less, further preferably 280 Pa·s or less, and from the viewpoint of further improving operability, it is preferably 10 Pa·s or more, more preferably 20 Pa·s or more, further preferably 50 Pa·s or more, further preferably 100 Pa·s or more, further preferably 200 Pa·s or more.
[0052] The viscosities of liquid A and liquid B in this specification represent values measured by the method described in Examples.
[0053] In the case where the heat dissipating gap filler is a two-component type, from the viewpoint of further improving thermal conductivity, the thermal conductivity of liquid A is preferably 1.0 W / m·K or more, more preferably 1.5 W / m·K or more, more preferably 2.0 W / m·K or more, more preferably 2.5 W / m·K or more, more preferably 2.7 W / m·K or more, more preferably 3.0 W / m·K or more, and more preferably 3.5 W / m·K or more. The upper limit is not particularly limited, and for example, it may be 10.0 W / m·K or less, 8.0 W / m·K or less, or 5.0 W / m·K or less.
[0054] In the case where the heat dissipating gap filler is a two-component type, from the viewpoint of further improving thermal conductivity, the thermal conductivity of liquid B is preferably 1.0 W / m·K or more, more preferably 1.5 W / m·K or more, more preferably 2.0 W / m·K or more, more preferably 2.5 W / m·K or more, more preferably 2.7 W / m·K or more, more preferably 3.0 W / m·K or more, and more preferably 3.5 W / m·K or more. The upper limit is not particularly limited, and for example, it may be 10.0 W / m·K or less, 8.0 W / m·K or less, or 5.0 W / m·K or less.
[0055] The thermal conductivities of liquid A and liquid B in this specification represent values measured by the method described in Examples.
[0056] Hereinafter, each component constituting the heat-dissipating gap filler resin composition will be described.
[0057] <Maleic anhydride modified polybutadiene>
[0058] The maleic anhydride-modified polybutadiene of the present embodiment is produced by modifying a butadiene homopolymer with maleic anhydride, and specific examples thereof include RICON 130MA8, RICON 131MA5, RICOBOND 1731, and RICOBOND 1756 from Clay Valley Company and POLYVESTMA75 from Evonik Corporation.
[0059] When the total amount of the heat-dissipating gap filler resin composition of the present embodiment is 100% by mass, from the viewpoint of further improving the performance balance between handleability and sheet moldability, the content of the maleic anhydride-modified polybutadiene of the present embodiment is preferably 0.2% by mass or more, more preferably 0.5% by mass or more, further preferably 1.0% by mass or more, further preferably 1.2% by mass or more, and from the viewpoint of setting the viscosity in a more appropriate range, it is preferably 10.0% by mass or less, more preferably 7.0% by mass or less, further preferably 6.0% by mass or less, further preferably 5.5% by mass or less.
[0060] In the case where the heat dissipating gap filler is a two-component type, when the total amount of liquid A is set to 100 mass%, from the viewpoint of further improving the workability, the content of maleic anhydride-modified polybutadiene contained in liquid A is preferably 0.5 mass% or more, more preferably 1.0 mass% or more, further preferably 2.0 mass% or more, further preferably 2.4 mass% or more, and from the viewpoint of setting the viscosity to a more appropriate range, it is preferably 20.0 mass% or less, more preferably 14.0 mass% or less, further preferably 12.0 mass% or less, further preferably 11.0 mass% or less.
[0061] <Hydroxy-modified polybutadiene>
[0062] The hydroxy-modified polybutadiene of the present embodiment is obtained by oxidizing polybutadiene, and specifically, Poly bd R-20LM of Clay Valley Company, Poly bd R-15HT and Poly bd R-45HT of Idemitsu Kosan Co., Ltd., POLYVEST HT of Evonik Corporation, NISSO-PB G-1000, NISSO-PB G-2000 and NISSO-PB G-3000 of Nippon Soda Co., Ltd., and hydroxy-terminated polymer butadiene of Zibo Corporation are exemplified.
[0063] When the total amount of the resin composition for heat dissipating gap fillers of the present embodiment is 100% by mass, from the viewpoint of further improving the workability, the content of the hydroxy-modified polybutadiene of the present embodiment is preferably 0.2% by mass or more, more preferably 0.3% by mass or more, further preferably 0.4% by mass or more, further preferably 0.5% by mass or more, and from the viewpoint of setting the viscosity in a more appropriate range, it is preferably 10.0% by mass or less, more preferably 7.0% by mass or less, further preferably 5.0% by mass or less, further preferably 3.0% by mass or less, further preferably 2.0% by mass or less, further preferably 1.8% by mass or less.
[0064] In the case where the heat dissipating gap filler is a two-component type, when the total amount of liquid B is set to 100 mass%, from the viewpoint of further improving workability, the content of hydroxy-modified polybutadiene contained in liquid B is preferably 0.5 mass% or more, more preferably 0.7 mass% or more, more preferably 1.0 mass% or more, and from the viewpoint of setting the viscosity to a more appropriate range, it is preferably 20.0 mass% or less, more preferably 14.0 mass% or less, further preferably 10.0 mass% or less, further preferably 6.0 mass% or less, further preferably 4.0 mass% or less, further preferably 3.6 mass% or less.
[0065] The content of the maleic anhydride-modified polybutadiene and the hydroxy-modified polybutadiene of the present embodiment is determined by taking into account the number of maleic anhydride residues of the maleic anhydride-modified polybutadiene participating in the reaction, the number of hydroxyl groups of the hydroxy-modified polybutadiene, and the physical properties of the resin obtained after the reaction. When the total amount of the resin composition for heat dissipation gap filler of the present embodiment is set to 100% by mass, the total content of the maleic anhydride-modified polybutadiene and the hydroxy-modified polybutadiene of the present embodiment is, for example, 0.01 to 25% by mass, preferably 0.5 to 25% by mass.
[0066] When the total amount of the heat dissipating gap filler resin composition of the present embodiment is 100% by mass, from the viewpoint of further improving the workability, the total content of the maleic anhydride-modified polybutadiene of the present embodiment and the hydroxy-modified polybutadiene of the present embodiment is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, further preferably 0.5% by mass or more, further preferably 1.0% by mass or more, further preferably 2.0% by mass or more, further preferably 3.0% by mass or more, and from the viewpoint of setting the viscosity in a more appropriate range, it is preferably 25% by mass or less, more preferably 20% by mass or less, further preferably 15% by mass or less, further preferably 10% by mass or less.
[0067] <Thermal conductive filler>
[0068] As the thermally conductive filler of the present embodiment, any known thermally conductive filler can be used. However, when there is a concern about breakdown voltage, an electrically insulating thermally conductive filler is preferred.
[0069] As electrically insulating thermally conductive fillers, inorganic particles such as oxides, hydrates, nitrides, carbonates, and carbides can be cited. Among oxides, for example, silicon oxide, aluminum oxide, magnesium oxide, zinc oxide, etc. are preferably used. Among hydrates, for example, aluminum hydroxide, magnesium hydroxide, etc. are preferably used. As nitrides, for example, boron nitride and aluminum nitride are preferably used. As carbonates, for example, magnesium carbonate and anhydrous magnesium carbonate are preferably used. As carbides, for example, silicon carbide is preferably used. In addition, if electrical insulation is not considered, metals such as graphite, carbon nanotubes, and aluminum can also be used.
[0070] The thermally conductive filler of the present embodiment preferably includes at least one selected from the group consisting of aluminum oxide, aluminum hydroxide, aluminum nitride, zinc oxide, anhydrous magnesium carbonate, and silicon carbide.
[0071] When the total amount of the resin composition for heat dissipating gap fillers of the present invention is set to 100 mass%, from the viewpoint of further improving thermal conductivity, the content of the thermally conductive filler of the present embodiment is preferably 70 mass% or more, more preferably 75 mass% or more, further preferably 80 mass% or more, further preferably 85 mass% or more, and from the viewpoint of further improving handleability, it is preferably 99 mass% or less, more preferably 97 mass% or less, further preferably 95 mass% or less.
[0072] When the heat dissipating gap filler is a two-liquid type, the thermally conductive filler is preferably contained in liquid A and liquid B. By containing the thermally conductive filler in liquid A and liquid B, the viscosity balance of liquid A and liquid B can be made more appropriate, and the workability when mixing liquid A and liquid B can be further improved.
[0073] In the case where the heat dissipating gap filler is of a two-component type, when the total amount of liquid A is set to 100 mass%, from the viewpoint of further improving thermal conductivity, the content of the thermally conductive filler contained in liquid A is preferably 70 mass% or more, more preferably 75 mass% or more, further preferably 80 mass% or more, further preferably 85 mass% or more, and from the viewpoint of further improving operability, it is preferably 99 mass% or less, more preferably 97 mass% or less, further preferably 95 mass% or less.
[0074] In the case where the heat dissipating gap filler is of a two-component type, when the total amount of liquid B is set to 100 mass%, from the viewpoint of further improving thermal conductivity, the content of the thermally conductive filler contained in liquid B is preferably 70 mass% or more, more preferably 75 mass% or more, further preferably 80 mass% or more, further preferably 85 mass% or more, and from the viewpoint of further improving operability, it is preferably 99 mass% or less, more preferably 97 mass% or less, further preferably 95 mass% or less.
[0075] By using one or more of these thermally conductive fillers, or using the same inorganic particles with different particle sizes in combination, or adjusting their content, it is possible to control the thermal conductivity or the viscosity of the resin composition, with the goal of maximizing thermal conductivity, and in order to control the viscosity of the resin composition for heat dissipation gap filler within a range that allows easy injection and coating, it is preferred to use inorganic particles with different particle sizes in combination. In this way, it is possible to adjust to an appropriate viscosity and further improve thermal conductivity. It should be noted that in the case of imparting flame retardancy, for example, hydrates can also be used to select aluminum hydroxide and magnesium hydroxide instead of oxides.
[0076] <Antioxidants>
[0077] Since the purpose of the heat dissipation gap filler is to dissipate heat, it is naturally used in places where it is exposed to high temperature conditions for a long time or repeatedly exposed to high temperature and room temperature.
[0078] The heat dissipation gap filler resin composition of the present embodiment not only causes thermal degradation of the double bonds from the butadiene chain due to heat, water, oxygen, etc., but also easily causes crosslinking reaction between butadiene chains, resulting in the obtained heat dissipation gap filler becoming hard and brittle, causing cracking or peeling. In order to further reduce the cracking or peeling, the heat dissipation gap filler resin composition of the present embodiment contains an antioxidant.
[0079] The antioxidant may be a known antioxidant, and preferably includes at least one selected from the group consisting of phenolic antioxidants, phosphorus-based antioxidants, thiol-based antioxidants, diphenylamine-based antioxidants, ascorbic acid-based antioxidants and hindered amine-based antioxidants, more preferably includes at least one selected from the group consisting of phenolic antioxidants and phosphorus-based antioxidants, and further preferably includes a phenolic antioxidant.
[0080] It is preferred that the antioxidant be one or more of a primary antioxidant and / or a secondary antioxidant.
[0081] The primary antioxidant captures peroxy radicals and prevents oxidative degradation of the resin. The primary antioxidant can be a known primary antioxidant, preferably a phenolic antioxidant, and examples thereof include hexamethylenebis[(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 4,4'-thiobis(6-tert-butyl-m-cresol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), bis[3,3-bis(4-hydroxy-3-tert-butylphenyl)butyric acid] glycol ester, 2,2'-ethylenebis(4,6-di-tert-butylphenol), 2,2'-ethylenebis(4-sec-butyl-6-tert-butylphenol), 1,1,3-Tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, bis[2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl]terephthalate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-2,4,6-trimethylbenzene, 1,3,5-tris[(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxyethyl]isocyanurate, 2-tert-butyl-4-methyl-6-(2-acryloyloxy-3-tert-butyl-5-methylbenzyl) )phenol, 3,9-bis[1,1-dimethyl-2-{(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, triethylene glycol bis[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate], n-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenyl)butane, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], diethylenethiobis[3-(3,5-di-tert-butyl -4-hydroxyphenyl) propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-hydroxyphenyl) propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)trione, 3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropionate, phenylpropionic acid 3,5-bis(1,1-dimethylethyl)-4-hydroxy-C7-C9 side chain alkyl ester, 4,6-bis(octylthiomethyl)-o-cresol, etc. From the viewpoint of further suppressing cracking or peeling of the heat dissipating gap filler and maintaining appropriate hardness, the phenolic antioxidant preferably contains at least one selected from the group consisting of 4,4'-thiobis(6-tert-butyl-m-cresol), thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 4,6-bis(octylthiomethyl)-o-cresol.
[0082] The secondary antioxidant decomposes hydroxide radicals generated by oxidation of double bonds to prevent oxidative degradation of the resin. As the secondary antioxidant, a conventionally known secondary antioxidant can be used, preferably a phosphorus-based antioxidant, and examples thereof include trisnonylphenyl phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris[2-tert-butyl-4-(3-tert-butyl-4-hydroxy-5-methylphenylthio)-5-methylphenyl]phosphite, tridecylphosphite, octyldiphenylphosphite, di(decyl)monophenylphosphite, di(tridecyl)pentaerythritol diphosphite, distearylpentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4,6-tri-tert-butylphenyl)pentaerythritol diphosphite, tetra(tridecyl)isopropylidene diphenol diphosphite, tetra(tridecyl)-4,4'-n-butylidenebis(2-tert-butyl-5-methylphenol) diphosphite, hexa(tridecyl)-1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane triphosphite, tetra(2,4-di-tert-butylphenyl)biphenylene diphosphite, 9,10-dihydro-9-oxy-10-phosphaphenanthrene-10-oxide, 2,2'-methylenebis(4-methyl-6-tert-butylphenyl)-2-ethylhexyl phosphite, 4-[3-[(2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphapine)-6-yloxy]propyl]-2-methyl-6-tert-butylphenol, and the like.
[0083] In order to exhibit an antioxidant effect without sacrificing other properties, the content of these antioxidants is, for example, 0.01 to 20 mass %, or preferably 0.4 to 20 mass %, when the total amount of the heat-dissipating gap filler resin composition of the present embodiment is 100 mass %.
[0084] When the total amount of the resin composition for heat dissipating gap fillers of the present embodiment is 100% by mass, the content of the antioxidant is 0.01% by mass or more, and from the viewpoint of further improving the antioxidant effect, it is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, further preferably 0.4% by mass or more, further preferably 0.5% by mass or more, and from the viewpoint of further improving the balance between thermal conductivity, workability, etc., it is preferably 20.0% by mass or less, more preferably 15.0% by mass or less, further preferably 10.0% by mass or less, further preferably 8.0% by mass or less, further preferably 5.0% by mass or less, further preferably 3.0% by mass or less, further preferably 1.0% by mass or less.
[0085] When the heat-dissipating gap filler is a two-component type, the antioxidant may be contained in only one of the A liquid and the B liquid, or may be contained in both the A liquid and the B liquid.
[0086] When the total amount of liquid A is 100% by mass, from the viewpoint of further improving the antioxidant effect, the content of the antioxidant contained in liquid A is preferably 0.025% by mass or more, more preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and more preferably 0.2% by mass or more. Furthermore, from the viewpoint of further improving the balance between thermal conductivity, workability, etc., it is preferably 25.0% by mass or less, more preferably 20.0% by mass or less, more preferably 15.0% by mass or less, more preferably 10.0% by mass or less, more preferably 8.0% by mass or less, more preferably 5.0% by mass or less, more preferably 3.0% by mass or less, more preferably 1.5% by mass or less, more preferably 1.0% by mass or less, and more preferably 0.5% by mass or less.
[0087] When the total amount of liquid B is 100% by mass, from the viewpoint of further improving the antioxidant effect, the content of the antioxidant contained in liquid B is preferably 0.025% by mass or more, more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, further preferably 0.2% by mass or more, and from the viewpoint of further improving the balance between thermal conductivity, workability, etc., it is preferably 25.0% by mass or less, more preferably 20.0% by mass or less, further preferably 15.0% by mass or less, further preferably 10.0% by mass or less, further preferably 8.0% by mass or less, further preferably 5.0% by mass or less, further preferably 3.0% by mass or less, further preferably 1.5% by mass or less, further preferably 1.0% by mass or less, further preferably 0.5% by mass or less.
[0088] <Curing accelerator>
[0089] From the viewpoint of promoting the curing reaction, the heat-dissipating gap filler resin composition of the present embodiment preferably further contains a curing accelerator.
[0090] The curing accelerator is not particularly limited as long as it has the function of promoting the curing reaction, and an amine-based curing accelerator is preferred. Among them, the pKa of the amine-based curing accelerator is preferably 8.0 or more, more preferably 9.0 or more, and further preferably 9.5 or more. Specifically, 2-ethyl-4-ethylimidazole, 1-cyanoethyl-2-ethyl-4-ethylimidazole and other imidazoles, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), 1,5-diazabicyclo(4,3,0)nonene-5 (DBN), hexahydro-1,3,5-tris(3-dimethyl)phenol, Tertiary amines such as N,N,N',N", N"-pentamethyldiethylenetriamine, N,N,N',N'-tetramethylhexamethylenediamine, and N-methyldicyclohexylamine, secondary amines such as 4,4'-methylenebis(N-sec-butylcyclohexaneamine) and N,N'-di-sec-butyl-p-phenylenediamine, octanoate of DBU or DBN, and 1,1,3,3-tetramethylguanidine.
[0091] In view of adjusting the initial curing time to be appropriate, the content of these curing accelerators is preferably 0.01 to 5% by mass based on the total amount of the resin composition for heat dissipating gap fillers of the present invention.
[0092] <Plasticizer>
[0093] From the viewpoint of adjusting the viscosity of the resin, the heat-dissipating gap filler resin composition of the present embodiment preferably further contains a plasticizer.
[0094] It is preferred that the plasticizer is a liquid at room temperature with a flash point of 200° C. or more so as to remain inside the cured product. As long as it is a liquid that does not hinder the curing reaction, one or more of them can be used. For example, esters such as di-2-ethylhexyl phthalate (DOP), diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), di-2-ethylhexyl adipate (DOA), diisononyl adipate (DINA), tri-2-ethylhexyl trimellitate (TOTM), tricresyl phosphate (TCP), and fatty acid esters modified with animal and plant oils can be cited.
[0095] When the total amount of the resin composition for heat dissipating gap fillers of the present embodiment is set to 100 mass%, from the viewpoint of setting the viscosity of the resin in a more appropriate range, the content of the plasticizer of the present embodiment is preferably 1 mass% or more, more preferably 2 mass% or more, and further preferably 3 mass% or more, and from the viewpoint of further improving the balance between thermal conductivity, workability, etc., it is preferably 10 mass% or less, more preferably 9 mass% or less, and further preferably 8 mass% or less.
[0096] <Dispersant>
[0097] From the viewpoint of further improving the dispersibility of the thermally conductive filler, the heat-dissipating gap filler resin composition of the present embodiment preferably further contains a dispersant.
[0098] The dispersant is not particularly limited as long as it is for the purpose of surface modification of the thermally conductive filler and has the function of helping to improve the wettability with the resin and improving the dispersibility. For example, cationic, anionic, nonionic and amphoteric surfactants can be cited, and one or more of them can be used. Specifically, KP (manufactured by Shin-Etsu Chemical Co., Ltd.), Flowlen (manufactured by Kyoeisha Chemical Co., Ltd.), Solsperse (manufactured by Lubrizol Corporation), EFKA (manufactured by BASF), Ajisper (manufactured by Ajinomoto Fine Chemicals Co., Ltd.), Disperbyk and BYK (manufactured by BYK Chemical Co., Ltd.), MALIALIM (manufactured by NOF Corporation), and Disparlon (manufactured by Kusumoto Chemicals Co., Ltd.) can be cited. They can be mixed when manufacturing liquid A or liquid B, or they can be pre-treated into fillers.
[0099] When the total amount of the resin composition for heat dissipating gap fillers of the present embodiment is set to 100 mass%, from the viewpoint of further improving the dispersibility of the thermally conductive filler, the content of the dispersant of the present embodiment is preferably 0.05 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.2 mass% or more, and from the viewpoint of further improving the balance between thermal conductivity, handleability, etc., it is preferably 1.0 mass% or less, more preferably 0.8 mass% or less, and even more preferably 0.6 mass% or less.
[0100] <Other ingredients>
[0101] Furthermore, in addition to the above-mentioned additives, the composition may contain a coupling agent, a rheology control agent, a defoaming agent, a flame retardant, an anti-settling agent, a colorant, etc., which are usually compounded, as required, within a range not hindering the effects of the present invention.
[0102] [Method for producing resin composition for heat dissipating gap filler]
[0103] The resin composition for heat-dissipating gap fillers of the present embodiment can be obtained by mixing the respective materials using a high-viscosity kneading machine such as a ball mill, a three-roll mill, a kneader, a planetary mixer, or a screw extruder.
[0104] When the heat-dissipating gap filler is a two-component type, the materials of liquid A and liquid B are mixed using a high-viscosity kneading machine such as a ball mill, a three-roll mill, a kneader, a planetary mixer, or a screw extruder.
[0105] [Method of using the resin composition for heat dissipating gap filler]
[0106] The heat dissipating gap filler resin composition is used, for example, by injecting the heat dissipating gap filler resin composition into the gap between articles or applying the heat dissipating gap filler resin composition and then bonding the articles together with the applied surfaces.
[0107] In the case of a two-component heat dissipating gap filler, for example, liquid A and liquid B are mixed at a volume ratio of 1:1 and injected into the gap between the articles or applied and then the articles are bonded together with the applied surface. Of course, mixing by weight ratio is also possible, but in such an operation, the mixing method by measuring volume is usually used for simplicity.
[0108] [Heat dissipation gap filler]
[0109] The heat dissipating gap filler of the present embodiment is obtained by curing the heat dissipating gap filler resin composition of the present embodiment. The heat dissipating gap filler of the present embodiment may be obtained by curing at least a portion of the heat dissipating gap filler resin composition of the present embodiment.
[0110] The heat-dissipating gap filler of the present embodiment is obtained, for example, by curing the resin composition for heat-dissipating gap filler of the present embodiment at room temperature (for example, 21° C. or higher and 25° C. or lower).
[0111] In the case of a two-component heat dissipation gap filler, the initial curing time from the mixing of liquid A and liquid B varies depending on the type, amount, and temperature of the curing accelerator. In the present invention, it can be controlled to 5 to 60 minutes under the practically preferred room temperature (e.g., above 21°C and below 25°C), and then it takes about 1 to 3 days until it is completely cured. In addition, after curing, it has excellent adhesion and moderate flexibility, so it will not peel off or crack for a long time under harsh conditions.
[0112] [thing]
[0113] The article of this embodiment includes the heat-dissipating gap filler of this embodiment.
[0114] The article of this embodiment is electronic equipment such as a digital home appliance, a lithium-ion secondary battery, and a vehicle-mounted power module.
[0115] Example
[0116] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples. It should be noted that in the examples, "parts" means "parts by mass".
[0117] Production Example 1
[0118] (Manufacturing of A-1 solution)
[0119] 2.70 parts of RICON130MA8 (maleic anhydride-modified polybutadiene manufactured by Cray Valley Company), 6.00 parts of diisononyl phthalate (plasticizer manufactured by Shin Nippon Rika Co., Ltd.), 25 parts of B-325 (aluminum hydroxide manufactured by ALMORIXL T.), 31 parts of T-60 75MY (aluminum oxide manufactured by Almatis Company), 25 parts of LS-210B (aluminum oxide manufactured by Nippon Light Metal Co., Ltd.) and 10.3 parts of ASFP-20 (aluminum oxide manufactured by Denki Kagaku Kogyo Co., Ltd.) were mixed and stirred using a rotation-revolution mixer ARE-310 manufactured by THINKY CORPORATION to obtain 100 parts of A-1 liquid.
[0120] Production Example 2
[0121] (Manufacturing of B-1 solution)
[0122] Using a rotation-revolution mixer ARE-310 from THINKY CORPORATION, 1.05 parts of Polybd R-20LM (Cray Valley Company, hydroxyl-modified polybutadiene), 0.02 parts of Lupragen N700 (BASF, curing accelerator), 6.63 parts of diisononyl phthalate (New Japan Chemical Co., Ltd., plasticizer), 25 parts of B-325 (Almorix Ltd., aluminum hydroxide), 25 parts of T-6075MY (Almatis Ltd., aluminum hydroxide) and 1.06 parts of 1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1.5-1 Company), alumina), 31 parts, LS-210B (alumina, manufactured by Nippon Light Metal Co., Ltd.), 25 parts, ASFP-20 (alumina, manufactured by Denki Kagaku Kogyo Co., Ltd.), 10.3 parts, and DISPERBYK-145 (dispersant, manufactured by BYK Chemical Co., Ltd.) were mixed and stirred to obtain 100 parts of B-1 liquid.
[0123] According to the formulations in Table 1, the same operation as in Preparation Example 1 was performed to obtain A-2 liquid to A-8 liquid, and according to the formulations in Table 2, Table 3 and Table 4, the same operation as in Preparation Example 2 was performed to obtain B-2 liquid to B-33 liquid. It should be noted that the average particle size of inorganic particles such as alumina described in Tables 1 to 4 is the catalog value of each manufacturer.
[0124] Table 1
[0125]
[0126] Table 2
[0127]
[0128] Table 3
[0129]
[0130] Table 4
[0131]
[0132] The 8 types of A solutions and 33 types of B solutions were stored at 60°C for one month and examined for changes in viscosity and properties. No viscosity change or property change greater than ±20% was observed.
[0133] Example 1: Mixing of A-1 solution and B-3 solution and preparation of sheet
[0134] The 100 mL tanks on both sides of a 200 mL Nordson two-liquid parallel box were filled with A-1 liquid and B-3 liquid, respectively, and the A-1 liquid and B-3 liquid were mixed in a volume ratio of 1:1 using a 24-stage disposable spiral mixer (static mixer).
[0135] The obtained mixed solution was applied on a glass plate and pressed with an aluminum plate having spacers of 1 mm thickness at both ends, thereby preparing a sheet having the AB mixed solution of 1 mm thickness sandwiched between the glass plate and the aluminum plate.
[0136] By the same operation as in Example 1, liquid A and liquid B were mixed according to the formulations in Tables 5 and 6 to obtain AB mixed liquids and sheets of Examples 1 to 24 and Comparative Examples 1 to 4.
[0137] The AB mixed solutions and sheets obtained in Examples 1 to 24 and Comparative Examples 1 to 4 were subjected to the tests of the items listed in Tables 5 and 6 (thermal conductivity, hardness, initial curing time, complete curing time, thermal shock test, and aging test), and the results of Tables 5 and 6 were obtained. It should be noted that the viscosity and thermal conductivity tests were respectively conducted on the A solution and the B solution, and the results are listed in Tables 1 to 4.
[0138] Table 5
[0139]
[0140] Table 6
[0141]
[0142] "Viscosity"
[0143] The rheometers MCR302 and PP25 manufactured by Anton Paar of Austria were used for measurement at a measurement temperature of 23° C. and a shear rate of 1 (1 / s).
[0144] Thermal conductivity
[0145] The thermal conductivity was measured using a TIM tester from LINSEIS company in Germany according to ASTM D5470. In Examples 1 to 24 and Comparative Examples 1 to 4, the thermal conductivity was measured using samples obtained by curing the above-mentioned sheets. The sheets were cured at a curing temperature of 25°C and a curing time equal to the complete curing time listed in Tables 5 and 6.
[0146] "hardness"
[0147] The hardness was measured using a Shore OO hardness tester (manufactured by Teclock Company, trade name: Teclock Hardness Tester GS-754G) and a Shore O hardness tester (manufactured by Teclock Company, trade name: Teclock Hardness Tester GS-753G) in accordance with ASTM D2240. In Examples 1 to 24 and Comparative Examples 1 to 4, the samples for hardness measurement were samples obtained by curing the above-mentioned sheets. The sheets were cured at a curing temperature of 25° C. and a curing time of the complete curing time described in Tables 5 and 6.
[0148] Initial curing time
[0149] The viscosity of the AB mixed solution at 23°C is the time it takes for the initial viscosity after mixing to double.
[0150] “Full cure time”
[0151] The time (days) required for the hardness of the AB mixed liquids obtained in Examples and Comparative Examples to become constant when left at 23°C was used.
[0152] Thermal shock test
[0153] The sheets obtained in Examples and Comparative Examples were kept at -40°C for 20 minutes, heated to 100°C in 10 minutes and kept for 20 minutes, and cooled to -40°C in 10 minutes for a total of 60 minutes. After 2000 cycles, the degree of cracking and peeling was evaluated according to the following indexes.
[0154] A (very good): There is neither cracking nor peeling.
[0155] B (good): Only one of cracking or peeling was observed.
[0156] C (poor): Both cracking and peeling were observed.
[0157] "Weathering Tests: Cracking and Peeling"
[0158] The sheets obtained in Examples and Comparative Examples were placed in an oven at 100° C. for 2000 hours, and the extent of cracking and peeling was visually observed and evaluated based on the following indices.
[0159] A (very good): There is neither cracking nor peeling.
[0160] B (good): Only one of cracking or peeling was observed.
[0161] C (poor): Both cracking and peeling were observed.
[0162] "Aging Test: Brittleness"
[0163] <Brittleness 1>
[0164] The hardness after the aging test was measured by the same method as the "hardness" described above, and the brittleness 1 was evaluated according to the following index. It should be noted that when the hardness is 85 or more in Shore OO, it becomes hard, and thus tends to be easily broken when bent. When the hardness is greater than 90 in Shore OO or greater than 70 in Shore O, it is confirmed that it is too hard and breaks in almost all cases when bent.
[0165] A (very good): less than 85 on the Shore OO scale.
[0166] B (good): 85 or more on the Shore OO scale.
[0167] C (bad): greater than 90 on the Shore OO scale or greater than 70 on the Shore O scale.
[0168] <Brittleness 2>
[0169] In the method for preparing the sheets of the embodiments and comparative examples, a sheet containing an AB mixture having a thickness of 3 mm was prepared by changing the thickness of the spacer to 3 mm. The hardness of the sheet containing an AB mixture having a thickness of 3 mm was measured by the same method as the aforementioned "hardness". When measuring the hardness, the part of the pressure needle (pressure needle shape: hemispherical, front end R1.19 mm) inserted into the hardness tester was magnified 40 times and observed using an optical microscope. Brittleness 2 is used as an evaluation standard for brittleness under a stricter standard than brittleness 1. Brittleness 2 is evaluated according to the following indicators.
[0170] A (very good): There is no crack on the surface, and it is soft and concave.
[0171] B (good): Slight cracks on the surface are observed, but the cracks can be repaired by pressing.
[0172] C (bad): A state where cracks are observed on the surface.
[0173] <Comprehensive evaluation of brittleness>
[0174] The brittleness is comprehensively evaluated according to the following indicators.
[0175] AA (best): Both brittleness 1 and brittleness 2 were rated A.
[0176] A (very good): The evaluation of brittleness 1 was A, and the evaluation of brittleness 2 was B.
[0177] BB (better): The evaluation of brittleness 1 was B, and the evaluation of brittleness 2 was B.
[0178] B (good): The evaluation of brittleness 1 was A or B, and the evaluation of brittleness 2 was C.
[0179] C (poor): The evaluations of brittleness 1 and brittleness 2 were C.
[0180] As described above, the evaluation of cracking and peeling after the thermal shock test, the evaluation of cracking and peeling after the aging test, and the evaluation of brittleness of the examples are better than those of the comparative examples. That is, according to the resin composition for heat dissipation gap filler of this embodiment, the heat dissipation gap filler can reduce the occurrence of cracking or peeling even if it is exposed to high temperature conditions for a long time or subjected to a sudden temperature change.
[0181] In addition, it is possible to maintain appropriate hardness under conditions corresponding to actual usage scenes.
[0182] Furthermore, it is found that the two-component heat-dissipating gap filler resin composition has good storage stability before mixing liquid A and liquid B, and has moderate room temperature curability with an initial curing time of 5 to 60 minutes at room temperature after mixing, and therefore has good workability.
[0183] The heat-dissipating gap-filler resin composition of the present embodiment may not contain volatile silicone or low-molecular siloxane that may cause contact failure, and therefore, voids are not generated due to water or gas existing in the system or generated during the curing reaction.
[0184] This application is based on Japanese patent application No. 2021-163412 filed on October 4, 2021 and Japanese patent application No. 2022-072233 filed on April 26, 2022, and claims the priority of the Japanese patent applications. The entire contents of the Japanese patent applications are hereby introduced into this application.
Claims
1. A resin composition for heat dissipation gap filler, comprising maleic anhydride-modified polybutadiene, hydroxyl-modified polybutadiene, a thermally conductive filler and an antioxidant, wherein: When the total amount of the heat dissipating gap filler resin composition is 100 mass %, the content of the antioxidant is 0.01 mass % or more, The heat conductivity of the resin composition for heat dissipating gap filler after curing is 1.0 W / m·K or more. The resin composition for heat dissipation gap filler is a two-component resin composition for heat dissipation gap filler, The two-component heat-dissipating gap filler resin composition comprises liquid A and liquid B. Liquid A comprises the maleic anhydride-modified polybutadiene and the thermally conductive filler, Liquid B contains the hydroxy-modified polybutadiene and the thermally conductive filler.
2. The resin composition for heat dissipating gap filler according to claim 1, wherein When the total amount of the heat-dissipating gap-filler resin composition is 100% by mass, the content of the thermally conductive filler is 70% by mass or more.
3. The resin composition for heat dissipating gap filler according to claim 1 or 2, wherein: The antioxidant includes at least one selected from the group consisting of phenolic antioxidants and phosphorus antioxidants.
4. The resin composition for heat dissipating gap filler according to claim 3, wherein The antioxidant comprises a phenolic antioxidant.
5. The resin composition for heat dissipating gap filler according to claim 1 or 2, wherein: The heat-dissipating gap-filler resin composition further includes a curing accelerator.
6. The resin composition for heat dissipating gap filler according to claim 5, wherein The curing accelerator comprises an amine-based curing accelerator.
7. The resin composition for heat dissipating gap filler according to claim 6, wherein The pKa of the amine-based curing accelerator is 8.0 or more.
8. A heat dissipating gap filler, wherein: The heat dissipating gap filler is obtained by curing the resin composition for heat dissipating gap filler according to any one of claims 1 to 7.
9. An article, wherein The article comprises the heat dissipating gap filler of claim 8.