A preparation method of nano antimony trioxide

Petal-shaped nano-antimony trioxide is prepared through the hydrolysis reaction of alcohol solvent and morphology control agent, which solves the problems of toxic pollution and low conductivity, improves electrochemical performance and is suitable for industrial production.

CN118062890BActive Publication Date: 2024-10-29HUNAN LOUDI HUAXING ANTIMONY IND
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410182264.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-19
Publication Date
2024-10-29
Estimated Expiration
2044-02-19

AI Technical Summary

Technical Problem

The existing technology uses the toxic organic substance 2-methylimidazole when preparing antimony trioxide with a flower-like structure, which causes environmental pollution and is not suitable for large-scale industrial production. Its low conductivity limits its application.

Method used

Use alcohol solvents and morphology control agents (such as metal halides, organic acids and surfactants) for hydrolysis reactions to generate petal-like structure of nano-antimony trioxide, using halogen ions as the medium, combined with the pH adjustment of organic acids and surface The stabilizing effect of the active agent avoids the use of toxic substances.

Benefits of technology

It improves the electrochemical performance of nano-antimony trioxide and enhances the ability of charge and ion transmission channels. It is suitable for large-scale industrial production and has no risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118062890B_ABST
    Figure CN118062890B_ABST
Patent Text Reader

Abstract

The invention relates to the field of nano inorganic materials, and in particular to a method for preparing nano antimony trioxide. The method comprises the steps of dissolving micron-level antimony trioxide in an alcohol solvent, adding a morphology control agent and water, performing a hydrolysis reaction for more than 1 hour, centrifuging, collecting the product, washing it, and drying it to obtain nano antimony trioxide with a petal-shaped structure. The morphology control agent comprises a metal halide, an organic acid, and a surfactant. The method does not use a toxic organic substance, 2-methylimidazole, and is more suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of nano inorganic materials, in particular to a method for preparing nano antimony trioxide. Background Art

[0002] Sb2O3 has a high theoretical capacity, low price, abundant reserves, and relatively stable cycle performance. It is a very promising pseudocapacitor electrode material. However, its low conductivity is the main reason that hinders its application. Controlling the synthesis of nanostructures is one of the effective ways to improve its conductivity and electrochemical performance.

[0003] References: Liu Jingqiang, Chen Han, Zhu Yirong, Zhou Wei, Xiang Kaixiong. Preparation of flower-like antimony trioxide and its application in supercapacitors [J]. Journal of Packaging, 2019, (Issue 6) discloses a method for preparing flower-like antimony trioxide, which has high specific capacity and conductivity and is a very promising pseudocapacitor positive electrode material. However, the toxic organic substance 2-methylimidazole is used in the preparation process of flower-like antimony trioxide, which will cause environmental pollution and is not suitable for large-scale industrial production. Summary of the invention

[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a method for preparing nano antimony trioxide.

[0005] The technical solutions adopted are as follows:

[0006] A method for preparing nano antimony trioxide is as follows:

[0007] Dissolve micron-sized antimony trioxide in an alcohol solvent, add a morphology control agent and water, perform hydrolysis reaction for more than 1 hour, centrifuge, collect the product, wash it, and dry it to obtain nano antimony trioxide with a petal-like structure;

[0008] The morphology control agent includes metal halide, organic acid and surfactant.

[0009] The preparation method of the above-mentioned nano antimony trioxide is as follows:

[0010] The alcohol solvent is heated to 60-80°C, micron-sized antimony trioxide is added, stirred to dissolve, and then a morphology control agent and water are added. The hydrolysis reaction is performed for more than 1 hour, and the product is collected, washed, and dried to obtain nano antimony trioxide with a petal-like structure.

[0011] Furthermore, the weight ratio of the metal halide, the organic acid and the surfactant is 1:1-5:5-10.

[0012] Furthermore, the metal halide is any one or more combinations of sodium fluoride, potassium fluoride, sodium chloride, potassium chloride, sodium bromide, potassium bromide, sodium iodide or potassium iodide.

[0013] Furthermore, the organic acid is any one or more combinations of tartaric acid, oxalic acid, malic acid, citric acid, and ascorbic acid.

[0014] Furthermore, the surfactant is OP-10 and / or polyethylene glycol-400.

[0015] Further, the alcohol solvent is a mixture of ethylene glycol and isopropanol;

[0016] The volume fraction of ethylene glycol in the alcohol solvent is ≥70%.

[0017] Furthermore, the amount of the morphology control agent used is 10-50% of the weight of the micron-sized antimony trioxide.

[0018] Furthermore, the weight ratio of micron-sized antimony trioxide to alcohol solvent is 1:10-50.

[0019] Furthermore, during washing, deionized water and ethanol are used in sequence.

[0020] Beneficial effects of the present invention:

[0021] The invention provides a method for preparing nano antimony trioxide. The method utilizes the hydrolysis reaction of ethylene glycol antimony in water to generate nano antimony trioxide, takes halogen ions as the medium for the etching of the complex, the pH regulation and corrosion inhibition of organic acids, and the surfactant as a stabilizer for nano materials to inhibit agglomeration and guide the accumulation direction of grains. The petal-shaped structure formed can store more charges and ions and can also provide more transmission channels for them, thereby improving the electrochemical performance of the nano antimony trioxide. Compared with reference documents, the invention does not use the toxic organic 2-methylimidazole and is more suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the SEM image of the nano antimony trioxide prepared in Example 1;

[0023] Figure 2 This is the SEM image of the nano antimony trioxide prepared in Comparative Example 1;

[0024] Figure 3 This is the SEM image of the nano antimony trioxide prepared in Comparative Example 2;

[0025] Figure 4 This is the SEM image of the nano antimony trioxide prepared in Comparative Example 3;

[0026] Depend on Figure 1-4 From the comparison, it can be seen that the petal-shaped nano antimony trioxide can be generated only under the joint action of sodium fluoride, tartaric acid and polyethylene glycol-400. DETAILED DESCRIPTION

[0027] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0028] Embodiment 1:

[0029] A preparation method of nano antimony trioxide:

[0030] Add 160 ml of ethylene glycol and 40 ml of isopropanol into a three-necked flask with a condenser, a thermometer and a stirrer, stir and mix, then add 10 g of micron-sized antimony trioxide, turn on the heating to raise the temperature of the mixed solution to 80°C, stir for 30 minutes to dissolve the micron-sized antimony trioxide, then add 0.5 g of sodium fluoride, 1 g of tartaric acid, 2.5 g of polyethylene glycol-400 and 100 ml of deionized water, stir and hydrolyze for 2 hours, turn off the heating and cool naturally to room temperature, then centrifuge, collect the product, wash with deionized water and ethanol in turn, and dry at 60°C for 24 hours to obtain petal-shaped nano antimony trioxide.

[0031] Embodiment 2:

[0032] A preparation method of nano antimony trioxide:

[0033] Add 160 ml of ethylene glycol and 40 ml of isopropanol into a three-necked flask with a condenser, a thermometer and a stirrer, stir and mix, then add 10 g of micron-sized antimony trioxide, turn on the heating to raise the temperature of the mixed solution to 70°C, stir for 30 minutes to dissolve the micron-sized antimony trioxide, then add 0.5 g of sodium fluoride, 1 g of tartaric acid, 2.5 g of polyethylene glycol-400 and 100 ml of deionized water, stir and hydrolyze for 2 hours, turn off the heating and cool naturally to room temperature, then centrifuge, collect the product, wash with deionized water and ethanol in turn, and dry at 60°C for 24 hours to obtain petal-shaped nano antimony trioxide.

[0034] Embodiment 3:

[0035] A preparation method of nano antimony trioxide:

[0036] Add 160 ml of ethylene glycol and 40 ml of isopropanol into a three-necked flask with a condenser, a thermometer and a stirrer, stir and mix, then add 10 g of micron-sized antimony trioxide, turn on the heating to raise the temperature of the mixed solution to 60°C, stir for 30 minutes to dissolve the micron-sized antimony trioxide, then add 0.5 g of sodium fluoride, 1 g of tartaric acid, 2.5 g of polyethylene glycol-400 and 100 ml of deionized water, stir and hydrolyze for 2 hours, turn off the heating and cool naturally to room temperature, then centrifuge, collect the product, wash with deionized water and ethanol in turn, and dry at 60°C for 24 hours to obtain petal-shaped nano antimony trioxide.

[0037] Comparative Example 1:

[0038] The method is substantially the same as Example 1, except that sodium fluoride is not added.

[0039] Comparative Example 2:

[0040] The same as Example 1, except that tartaric acid is not added.

[0041] Comparative Example 3:

[0042] The method is substantially the same as Example 1, except that polyethylene glycol-400 is not added.

[0043] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing nano antimony trioxide, It is characterized in that The details are as follows: The alcohol solvent is heated to 60-80°C, micron-sized antimony trioxide is added, stirred to dissolve, and then a morphology control agent and water are added. The hydrolysis reaction is performed for more than 1 hour, centrifuged, and the product is collected, washed, and dried to obtain nano antimony trioxide with a petal-like structure. The morphology control agent includes metal halide, organic acid and surfactant; The amount of the morphology control agent used is 10-50% of the weight of the micron-sized antimony trioxide; The weight ratio of the metal halide, the organic acid and the surfactant is 1:1-5:5-10; The metal halide is any one or more combinations of sodium fluoride, potassium fluoride, sodium chloride, potassium chloride, sodium bromide, potassium bromide, sodium iodide or potassium iodide; The organic acid is any one or more combinations of tartaric acid, oxalic acid, malic acid, citric acid, and ascorbic acid; The surfactant is OP-10 and / or polyethylene glycol-400; The alcohol solvent is a mixture of ethylene glycol and isopropanol; The volume fraction of ethylene glycol in the alcohol solvent is ≥70%.

2. The method for preparing nano antimony trioxide according to claim 1, It is characterized in that The weight ratio of micron-sized antimony trioxide to alcohol solvent is 1:10-50.

3. The method for preparing nano antimony trioxide according to claim 1, It is characterized in that When washing, use deionized water and ethanol in sequence.

Citation Information

Patent Citations

  • Preparation method of nano antimony trioxide

    CN108557883A

  • Antimony trioxide applied to negative electrode materials for lithium ion batteries and method for preparing antimony trioxide