A MOF material and its application in lithium-ion battery negative electrode

By self-assembly using copper elements and trianylline tripyridine to form Cu-MOF material, the problems of low capacity and complex preparation of lithium-ion battery negative electrode materials are solved, efficient electrochemical performance and simplified preparation process are achieved, and lithium ion is significantly improved The battery cycle life and stability.

CN118063786BActive Publication Date: 2024-11-08SOOCHOW MOFS SCI & TECH LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410339483.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-25
Publication Date
2024-11-08
Estimated Expiration
2044-03-25

AI Technical Summary

Technical Problem

The negative electrode material graphite of the existing lithium-ion battery has a low theoretical capacity and cannot meet market demand. The existing MOFs material preparation method is complex, so it needs to simplify and improve electrical performance.

Method used

Cu-MOF material was formed by self-assembly using copper elements and triphenylamine tripyridine as ligands, and prepared by solvent diffusion method and precipitation method to form MOF material with porous structure and excellent electrochemical properties.

Benefits of technology

Cu-MOF materials show good cycling performance and electrochemical stability, can quickly conduct ions and electrons, extend the cycle life of lithium-ion batteries, and simplify the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118063786B_ABST
    Figure CN118063786B_ABST
Patent Text Reader

Abstract

The invention discloses a novel MOF material and its application in the negative electrode of a lithium ion battery, which belongs to the field of lithium ion batteries and is prepared by a self-assembly coordination reaction of triphenylamine tripyridine and copper nitrate. The metal organic framework material (MOFs) provided by the invention generates a large number of pores during self-assembly, which can store a large number of lithium ions. In addition, each pore is closely connected to each other, which can conduct ions and electrons more quickly. Compared with other MOF negative electrode materials, the novel MOF material has a longer cycle life and better stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium ion batteries, and in particular relates to a MOF material and an application thereof in a negative electrode of a lithium ion battery. Background Art

[0002] With the rapid development of portable consumer electronics and electric vehicles, lithium-ion batteries have gradually come into people's view. With its advantages of high energy density, no memory effect, high operating voltage, and low self-discharge, it has quickly become a mainstream commercial product. However, the negative electrode material of commercial lithium-ion batteries is graphite, which has a low theoretical capacity (372mAhg -1 ) cannot meet the market demand. Therefore, developing new negative electrode materials to replace graphite is the key to improving the overall performance of lithium-ion batteries.

[0003] Metal-organic framework materials (MOFs) are favored by many researchers due to their large specific surface area, rich porosity and adjustable structure. MOFs materials are a type of porous crystalline materials generated by self-assembly reactions between metal ions and organic ligands. They have been widely used in electrochemical energy storage, electrocatalysis, drug transport, adsorption and separation, etc. The diversity of the selection of metal ions and organic ligands determines the diversity of MOFs materials. Therefore, the selection of suitable organic ligands and metal ions has become the key to determining the function of MOFs materials.

[0004] Patent CN 112708143 A discloses a method for preparing a novel MOFs lithium battery negative electrode material, comprising the following steps: dissolving phenyl acid and nitrate in water to obtain a mixed solution, adding an alkaline reagent to adjust the pH of the mixed solution to 2-5; adding the mixed solution to a reactor for hydrothermal reaction, cooling to room temperature after the reaction, and separating to obtain MOFs crystals; drying the MOFs crystals and grinding them evenly to obtain the MOFs lithium battery negative electrode material. The MOFs material prepared by the prior art using carboxylic acid compounds as organic ligands is a two-dimensional planar network with quadruple metals as nodes. The material is applied to the negative electrode material of a lithium battery, and the 200-cycle specific capacity is tested at a current density of 500mA / g at 25°C. The preferred discharge specific capacity is 846mAh / g, and the capacity after 200 cycles is 729mAh / g, which proves that it has good electrical properties. However, in order to expand the application scope of MOFs materials in the battery field, it is still necessary to continue to improve their electrical properties. From the perspective of production and preparation, the field also urgently needs a simpler method for preparing MOFs materials. Summary of the invention

[0005] The purpose of the present invention is to provide a MOF material and its application in the negative electrode of a lithium ion battery to solve the problems existing in the above-mentioned prior art. The present invention selects copper element as the metal center and triphenylamine tripyridine as the ligand, mainly because Cu ions have multiple valences and good redox activity, multiple valence states make redox reactions easy to occur, and triphenylamine tripyridine ligands have good stability. Combining the two to self-assemble to form Cu-MOF and using it as a negative electrode material for lithium ion batteries can show excellent electrochemical performance. Its unique porous structure can quickly conduct ions and greatly alleviate volume expansion. In addition, the four ligands on Cu-MOF have large steric hindrance, which makes the MOF material have excellent cycle performance.

[0006] One of the technical solutions provided by the present invention:

[0007] A MOF material is prepared by a self-assembly coordination reaction of triphenylamine tripyridine and copper nitrate.

[0008] The second technical solution provided by the present invention is:

[0009] A method for preparing a MOF material, characterized by comprising a solvent diffusion method and a precipitation method.

[0010] Preferably, the solvent diffusion method comprises the following steps: dripping an intermediate layer on the triphenylamine tripyridine solution, then adding a copper nitrate solution on the intermediate layer, sealing, standing in the dark, taking out the precipitated green block crystals, washing and drying to obtain the MOF material.

[0011] More preferably, the intermediate layer is a mixed solution of chloroform and methanol in equal volumes.

[0012] More preferably, the standing time is 3 weeks.

[0013] More preferably, the drying temperature is 60°C-70°C and the drying time is 6-10 hours.

[0014] Preferably, the precipitation method comprises the following steps: mixing a triphenylamine tripyridine solution and a copper nitrate solution, stirring, aging, filtering, and drying to prepare the MOF material.

[0015] More preferably, the solvent in the triphenylamine tripyridine solution is one or more of dichloromethane, chloroform and acetonitrile; the solvent in the copper nitrate solution is one or more of methanol, ethanol and water.

[0016] More preferably, the volume ratio of the triphenylamine tripyridine solution to the copper nitrate solution is (1:2)-(2:1); the molar ratio of the triphenylamine tripyridine to copper nitrate is (3.5:1)-(4.5:1).

[0017] The molar ratio of triphenylamine tripyridine to copper nitrate is limited to (3.5:1)-(4.5:1) based on the following reason: within this ligand range, the organic ligand reacts with the metal ion without generating impurities; when the molar ratio of the two is greater than 4.5:1, an excess of organic ligand leads to the generation of triphenylamine tripyridine impurities; and when the ratio is less than 3.5:1, an excess of metal salt leads to the generation of copper nitrate impurities.

[0018] More preferably, the stirring time is 5-8 hours; the aging time is 6-10 hours.

[0019] More preferably, the drying temperature is 60°C-70°C and the drying time is 6-10 hours.

[0020] The third technical solution provided by the present invention is:

[0021] An application of the above MOF material in preparing a negative electrode of a lithium ion battery.

[0022] Beneficial effects of the present invention:

[0023] The MOF material provided by the present invention has a porous structure, shortens the transmission path of ions and electrons, and has a larger diffusion coefficient. The ligand used in the present invention is triphenylamine tripyridine, which coordinates with copper ions to form a Cu-MOF structure with good stability and exhibits excellent cycle performance.

[0024] The MOF material provided by the present invention has a novel structure and a simple synthesis method, and more importantly, has excellent electrochemical stability and economic value when used in the negative electrode of a lithium-ion battery.

[0025] The metal organic framework material (MOFs) provided by the present invention generates a large number of pores when self-assembling, which can store a large number of lithium ions. In addition, the pores are closely connected to each other, which can conduct ions and electrons more quickly. Compared with other MOF negative electrode materials, the MOF material has a longer cycle life and better stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1The single crystal X-ray diffraction measurement diagram of the MOF material prepared in Example 1 and the XRD diagram of the MOF materials prepared in Examples 1 and 2, wherein (a) is a coordination environment diagram, and (b) is a one-dimensional plane diagram; (c) is an XRD diagram of the MOF materials prepared in Examples 1 and 2;

[0028] Figure 2 The SEM and EDS characterization images of the MOF material prepared in Example 2, wherein (a) is the SEM image, (b) is the EDS spectrum, and (c) is the mapping spectrum;

[0029] Figure 3 This is a graph of the electrochemical performance of the negative electrode of a lithium-ion battery prepared from the MOF material in Example 2 when the electrolyte is LB063 solution;

[0030] Figure 4 The negative electrode of the lithium-ion battery prepared by the MOF material in Example 2 is 0.1A g -1 The charge and discharge curves and cycle performance diagrams under current, where (a) is the charge and discharge curve and (b) is 0.1A g -1 Cycle performance diagram of

[0031] Figure 5 The cycle performance diagram of the negative electrode of the lithium-ion battery prepared by the MOF material in Example 2 when the electrolyte is LB007 solution, where (a) is at 0.5A g -1 Cyclic performance diagram under current density; (b) at 1Ag -1 Cycling performance at different current densities. DETAILED DESCRIPTION

[0032] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0033] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0034] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0035] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0036] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0037] The room temperature in the present invention refers to 25±2°C.

[0038] All raw materials in the examples of the present invention were purchased.

[0039] In the embodiments of the present invention, single crystals and powders of MOF were synthesized by solvent diffusion method and precipitation method respectively, wherein the single crystal structure was analyzed by single crystal X-ray diffractometer. The MOF powder was used as a negative electrode material and exhibited good electrochemical properties.

[0040] In order to characterize the crystal structure of the MOF material provided by the present invention, the MOF material was prepared by a solvent diffusion method, as shown in Example 1 for details.

[0041] Example 1 A method for preparing MOF material (solvent diffusion method)

[0042] Dissolve 47.6 mg of triphenylamine tripyridine (0.1 mmol) in 6 mL of chloroform and place it at the bottom of a test tube. Add 6 mL of chloroform / methanol mixed solution (volume ratio 1:1) as an intermediate layer (to play a buffering role), and then continue to add 6 mL of copper nitrate methanol solution (18.8 mg of copper nitrate, 0.1 mmol) on the intermediate layer. Seal the mouth of the test tube with plastic wrap and place it in a dark place. After standing for 3 weeks, green block crystals suitable for X-ray structure analysis are precipitated on the wall of the test tube. After taking it out, wash it with methanol and water three times each, and then dry it in an oven (65°C) for 8 hours. Finally, the green crystals are obtained, which are MOF materials.

[0043] The MOF material prepared by the solvent diffusion method of Example 1 and the MOF material prepared by the precipitation method are the same substance. The only difference between the two is the size of the crystal particles. This difference does not affect its performance as a negative electrode material for lithium-ion batteries, because the factors that determine its electrochemical performance lie in the structure and composition of the MOFs material, and the MOF materials prepared by the chemical precipitation method and the solvent diffusion method are the same in structure and composition. Considering the preparation time and preparation cost, the MOF material of the present invention prepared by the precipitation method is preferred.

[0044] Example 2 A method for preparing MOF material (precipitation method)

[0045] S1. Dissolve 190.4 mg of triphenylamine tripyridine (0.4 mmol) in 60 mL of chloroform, and dissolve 18.8 mg of copper nitrate (0.1 mmol) in 30 mL of methanol, and mix the two solutions.

[0046] S2. The mixed solution obtained in S1 was magnetically stirred at room temperature for 6 hours, aged for 8 hours, filtered, and then dried in an oven (65°C) for 8 hours to obtain a green powder, which is the MOF material.

[0047] Example 3 A method for preparing MOF material (precipitation method)

[0048] S1. Dissolve 166.6 mg of triphenylamine tripyridine (0.35 mmol) in 60 mL of dichloromethane and dissolve 18.8 mg of copper nitrate (0.1 mmol) in 60 mL of water, and mix the two solutions.

[0049] S2. The mixed solution obtained in S1 was magnetically stirred at room temperature for 5 hours, aged for 6 hours, filtered, and then dried in an oven (60°C) for 10 hours to obtain a green powder, which is the MOF material.

[0050] Example 4

[0051] S1. Dissolve 214.2 mg of triphenylamine tripyridine (0.45 mmol) in 60 mL of acetonitrile, and dissolve 18.8 mg of copper nitrate (0.1 mmol) in 120 mL of ethanol, and mix the two solutions.

[0052] S2. The mixed solution obtained in S1 was magnetically stirred at room temperature for 8 hours, aged for 10 hours, filtered, and then dried in an oven (70°C) for 6 hours to obtain a green powder, which is the MOF material.

[0053] Performance Testing

[0054] 1) Crystal structure determination of MOF materials

[0055] Based on the MOF material prepared by the solvent diffusion method in Example 1, its crystal structure was analyzed using a single crystal X-ray diffractometer. The results are as follows Figure 1 As shown: the MOF material prepared in Example 1 is monoclinic and belongs to the P21 / c space group. Figure 1 (a) is the coordination environment diagram of MOF. The central atom is Cu atom. Four triphenylamine tripyridine molecules remove one hydrogen atom respectively and then combine with Cu atom. Figure 1 (b) shows a one-dimensional plane image of MOF, from which relatively regular quadrilateral pores can be seen. Two adjacent Cu-MOF molecules do not overlap, showing a dispersed arrangement.

[0056] The MOF materials prepared in Example 1 and Example 2 were characterized by XRD. Figure 1 (c) is the XRD pattern of MOF materials prepared in Example 1 and Example 2. The single crystal prepared in Example 1 (with Figure 1 (c) corresponds to the simulated) and the powder sample prepared in Example 2 (corresponding to Figure 1 The experimental counterpart in (c) has similar diffraction peaks, proving that they are the same substance and the powder sample has a high phase purity.

[0057] 2) SEM and EDS characterization experiments

[0058] The MOF material prepared in Example 2 was characterized by SEM and EDS. Figure 2 (a) is a SEM image of the MOF prepared in Example 2, from which it is not difficult to see that the product presents a regular brick-like structure, adjacent brick-like structures have appropriate gaps, and the surface of the material is relatively smooth; Figure 2 (b) is the EDS spectrum of the MOF prepared in Example 2. It can be seen that the elements C, N, O, and Cu are evenly distributed; Figure 2 (c) is the mapping map, and it can also be seen that the elements C, N, O, and Cu are evenly distributed in MOF.

[0059] Application Examples

[0060] Preparation of lithium-ion battery negative electrode and battery assembly:

[0061] The MOF material prepared in Example 2 is in powder form, and is used as a raw material to prepare a negative electrode for a lithium-ion battery. The powdered MOF material, acetylene black and PVDF are mixed in a mass ratio of 6:3:1 (total mass is 20 mg), and 3 mL of N-methylpyrrolidone solvent is added to mix them evenly to obtain a slurry. The obtained slurry is evenly coated on a copper foil by a coater, dried at 65°C in a vacuum oven for 12 hours, and then cut into a negative electrode sheet with a diameter of 12 cm. The negative electrode sheet is used as a working electrode, a PP / PE composite film is used as a diaphragm, a metal lithium sheet is used as a counter electrode, and the electrolyte is a lithium battery electrolyte LB063 and LB007, and assembled into a button half-cell in a glove box filled with high-purity argon.

[0062] The electrochemical properties of MOF powder were tested: the electrochemical properties were measured at room temperature using Shanghai Chenhua CHI660E electrochemical workstation and Blue Electric system; a series of electrochemical performance graphs were tested using LB063 solution as the electrolyte.

[0063] 0.1ms -1 The CV test results are as follows: Figure 3 As shown, from Figure 3 It can be seen that except for the irreversible process of the electrode material in the first scan (mainly attributed to the formation of the SEI film and the initial decomposition of the electrolyte), there is no obvious change in the subsequent second and third cycles, showing good cycle stability and reversibility. Figure 4 The negative electrode of the lithium ion battery prepared by the MOF material in Example 2 is 0.1Ag -1 The charge and discharge curve and cycle performance diagram under current, Figure 4 (a) is the charge and discharge curve. It can be seen from the figure that the first discharge capacity is 727 mAh g -1 The first charge capacity is 218mA hg -1 , the first Coulombic efficiency was 29.9%. Figure 4 (b) is 0.1A g -1 The cycle performance diagram shows that the discharge capacity is basically maintained at 250mA hg -1 about.

[0064] The electrolyte was LB007 solution, at 0.5A g -1 and 1A g -1 The cycling performance diagram at the current density is shown in Figure 5 As shown in the figure, it can be seen that the capacity increases slightly with the increase of the number of cycles. Figure 5 (a) is 0.5A g -1 Cycling performance under current density, after 500 cycles, the battery capacity increased from 129mAhg -1 Up to 232 mAhg-1 The Coulomb efficiency is basically close to 100%, showing good cycle stability. Figure 5 (b) is at 1Ag -1 Cyclic performance under current density, after 762 cycles, the discharge capacity increased from 115mA hg -1 Up to 238mA hg -1 , and still exhibits good fast charge and discharge performance under high current conditions.

[0065] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. An application of a MOF material in preparing a negative electrode of a lithium-ion battery, characterized in that: The preparation method of the MOF material comprises the following steps: S1. Dissolve 190.4 mg of triphenylamine tripyridine in 60 mL of chloroform, dissolve 18.8 mg of copper nitrate in 30 mL of methanol, and mix the two solutions; S2. The mixed solution obtained in S1 was magnetically stirred at room temperature for 6 hours, aged for 8 hours, and then filtered. It was then dried in an oven at 65°C for 8 hours to obtain a green powder, which is the MOF material.

Citation Information

Patent Citations

  • Novel MOFs lithium battery negative electrode material as well as preparation method and application thereof

    CN112708143A

  • Mn(II) complex multiphoton absorption material as well as preparation method and application thereof