Preparation method of sodium ion battery negative electrode material and prepared negative electrode material

Through the porous MoS2 hollow monoshell or multishell spherical structure doped with Fe single atom, the problem of poor cycling stability and rate performance of MoS2 anode material in sodium ion batteries is solved, and high specific capacity and excellent electricity are achieved Chemical properties.

CN118919666AActive Publication Date: 2024-11-08HEBEI AGRICULTURAL UNIV.

Patent Information

Application Number
CN202410249560.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-05
Publication Date
2024-11-08
Estimated Expiration
2044-03-05

AI Technical Summary

Technical Problem

As a negative electrode material for sodium ion batteries, MoS2 has problems such as loss of active area, structural collapse, poor performance in charge and discharge cycles, especially the slow reaction kinetics under high current density, resulting in cycle stability and magnification. Poor performance.

Method used

Using a porous MoS2 hollow monoshell or multi-shell spherical structure doped with Fe single atom, the preparation, vulcanization and chemical etching method of Fe2 (MoO4)3 hollow monoshell or multi-shell spherical spheres are formed with high specific capacity. and sodium ion battery negative electrode material with excellent rate performance.

Benefits of technology

It realizes high specific capacity and excellent rate performance under high current density, and maintains good electrochemical stability in multiple cycles, showing the initial specific capacity of 462.6mAh·g-1 and at 5A·g- 1 The capacity of 259.4mAh·g-1 is still maintained after 500 cycles at the current density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919666A_ABST
    Figure CN118919666A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a sodium ion battery negative electrode material, which comprises the following steps: firstly, vulcanizing Fe2 (MoO4) 3 hollow single-shell or multi-shell spheres and S powder in an inert atmosphere at 330-370 DEG C according to a weight ratio of 1: (4-6) to obtain FeS2 / MoS2 hollow single-shell or multi-shell spheres; then placing the FeS2 / MoS2 hollow single-shell or multi-shell sphere in a ferric ion solution for reaction, enabling FeS2 and ferric ions to be subjected to chemical reaction so as to remove FeS2, separating precipitate, and calcining in an inert atmosphere of 800 DEG C to obtain the Fe monatomic doped porous MoS2 hollow single-shell or multi-shell sphere sodium ion battery negative electrode material. As a sodium-ion battery negative electrode material, the material has relatively high specific capacity, excellent rate capability and good cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a method for preparing a negative electrode material for a sodium ion battery and the prepared negative electrode material. Background Art

[0002] As a typical transition metal disulfide, MoS2 combines S-Mo-S together through van der Waals forces, giving it a suitable interlayer spacing of 0.62 nm, which can achieve Na + Reversible insertion / extraction, with a theoretical specific capacity of up to 670 mAh g -1 Therefore, MoS2 has attracted extensive attention as a negative electrode material for sodium ion batteries due to its high specific capacity, abundant resources, environmental friendliness and low cost. However, MoS2 as a negative electrode material still has the following four shortcomings: (1) MoS2 will gradually aggregate together during the charge and discharge cycle, resulting in the loss of its active area; (2) The volume change during the charge and discharge process will cause the structure to collapse, which will greatly affect its cycle stability; (3) At high current density, the slow electrons and Na + Diffusion kinetics leads to low specific capacity; (4) The reaction of MoS2 during sodium insertion is carried out in two steps, as shown in the following two equations. According to the second equation, MoS2 is eventually converted into Na2S during discharge, and Na2S is converted into sodium polysulfide. The shuttle effect of sodium polysulfide inhibits the reversible electrochemical reaction, resulting in poor rate performance. Therefore, it is necessary to further improve the electrochemical performance of MoS2 as a negative electrode material for sodium batteries.

[0003] MoS2 + xNa = NaxMoS2 (greater than 0.4 V, x < 2) (1)

[0004] Na x MoS2 + (4-x)Na = Mo + 2Na2S (less than 0.4 V) (2)

[0005] Well-designed nanostructures are effective in improving the structural stability and reaction kinetics of materials. Among them, hollow multi-shell structures (HoMS) with multiple shells and cavities have great application prospects in rechargeable batteries, electromagnetic wave absorption, catalysis, sensors, and drug delivery. Especially as electrode materials for high-energy-density batteries, HoMS can effectively regulate volume changes and stress changes during charge and discharge, thereby improving cycle stability. In addition, it can shorten the charge diffusion path, thereby improving rate performance.

[0006] In addition to structural engineering, composition regulation also shows great power in improving performance. In general, strategies to modify catalytic sites in electrode materials can significantly improve reaction kinetics and thus significantly improve rate performance. For example, iron single-atom catalysts have strong chemical catalysis and can anchor Na2S, promoting the rapid and reversible conversion of Mo and Na2S into MoS2. Combining structural design with composition regulation is beneficial to improving cycle stability and rate performance.

[0007] Therefore, constructing a porous MoS2 multi-shell hollow spherical structure doped with single Fe atoms is an important way to improve the performance of MoS2 anode materials for sodium-ion batteries. Summary of the invention

[0008] An object of the present invention is to provide a method for preparing a negative electrode material for a sodium ion battery, which can prepare porous MoS2 hollow single-shell or multi-shell spheres doped with single iron atoms, which are used as negative electrode materials for sodium ion batteries and have high specific capacity, excellent rate performance and good cycle stability.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] A method for preparing a negative electrode material for a sodium ion battery comprises the following steps:

[0011] Step S1: sulfiding Fe2(MoO4)3 hollow single-shell or multi-shell spheres with S powder at a weight ratio of 1:4-6 at 330-370° C. in an inert atmosphere to obtain FeS2 / MoS2 hollow single-shell or multi-shell spheres;

[0012] Step S2: Place the FeS2 / MoS2 hollow single-shell or multi-shell sphere in a trivalent iron ion solution for reaction, so that FeS2 reacts chemically with the trivalent iron ions to remove FeS2, separate the precipitate and calcine it at 800°C in an inert atmosphere to obtain Fe single-atom doped porous MoS2 hollow single-shell or multi-shell sphere sodium ion battery negative electrode material. Preferably, it also includes step S0: The preparation steps of the Fe2(MoO4)3 hollow single-shell or multi-shell sphere are as follows:

[0013] (NH4)2MoO4·4H2O, citric acid and FeCl3·6H2O are dissolved in water or a mixed solvent of water and ethanol to obtain a solution, and then carbon spheres are added to the solution and adsorb metal ions for several hours, the precursor is separated and the precursor is calcined in a muffle furnace at 440-460°C to obtain Fe2(MoO4)3 hollow single-shell or multi-shell spheres, and the number of shells of the Fe2(MoO4)3 hollow single-shell or multi-shell spheres is adjusted by the volume ratio of water to ethanol in the solution and the time and temperature for adsorbing metal ions.

[0014] Preferably, the weight ratio of the (NH4)2MoO4·4H2O, citric acid and FeCl3·6H2O is 2.9-3:1.8-1.9:8.2-8.4, the adsorption is carried out at a temperature of 30-50°C, and the solution uses water or a mixed solvent with a volume ratio of water to ethanol of 3:1.

[0015] Preferably, in step S2, the ferric iron solution is a Fe2(SO4)3 solution.

[0016] The inert atmosphere is nitrogen or argon.

[0017] Another object of the present invention is to provide a negative electrode material for a sodium ion battery, which is prepared by the above-mentioned preparation method.

[0018] The beneficial effect of the present invention is that, by adopting an improved sequential template method, a single-shell or multi-shell Fe2(MoO4)3 hollow sphere template is prepared, sulfurized, chemically etched with a trivalent iron solution and calcined at high temperature, and a porous MoS2 hollow single-shell or multi-shell sphere doped with iron is synthesized. The sphere not only has a unique single-shell or multi-shell structure, but also generates a large number of holes on the surface of the shell during the chemical etching process. This structure makes it easy for the electrolyte to penetrate from the surface to the inside, thereby promoting the contact between the material and the electrolyte, providing more active sites for the redox reaction, and shortening the transmission path of ions and electrons. At the same time, during the charge and discharge process, the free space between the shells can release the volume change, the inner shell can support the outer shell, and the outer shell can also protect the inner shell, ensuring that the structure remains stable during the sodium insertion and de-sodiumization reaction. When the porous MoS2 hollow multi-shell sphere doped with iron single atoms has four shells, it can be used as a negative electrode material for sodium ion batteries at 0.1A·g -1 At a current density of 1.34 mAh g, after four cycles, it showed a current density of 462.6 mAh g -1 High specific capacity, even at 5, 10, 20 and 30 A g -1 At ultra-high current densities, they still showed 300.0, 269.3, 239.8 and 213.3 mAh·g -1 The specific capacity shows excellent rate performance; at 0.1A·g -1 After 100 cycles at a current density of 1.5 %, it can retain 442 mAh g -1 The specific capacity at 5A·g -1 After 500 cycles at a high current density, it can still maintain 259.4 mAh g -1 The specific capacity shows excellent cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1(a) XRD spectra of Fe2(MoO4)3 hollow single-shell or multi-shell spheres (HoMS); (b) XRD patterns of MoS2 / FeS x XRD spectrum of HoMS.

[0020] Figure 2 XRD patterns of Fe-M-HoMS with different shell layers.

[0021] Figure 3 High-resolution transmission electron microscopy (HRTEM) image of Fe-M-HoMS-Q.

[0022] Figure 4 (a) Nitrogen adsorption-desorption isotherms and (b) pore size distribution curves of Fe-M-HoMS-Q, MF-HoMS-Q and FMO-HoMS-Q.

[0023] Figure 5 Scanning electron microscopy images (SEM) of (a) Fe-M-HoMS-S, (b) Fe-M-HoMS-D, (c) Fe-M-HoMS-T and transmission electron microscopy images (TEM) of (d) Fe-M-HoMS-S, (e) Fe-M-HoMS-D, (f) Fe-M-HoMS-T.

[0024] Figure 6 Energy dispersive spectroscopy analysis of Fe-M-HoMS-Q.

[0025] Figure 7 Morphology and electronic structure of Fe-M-HoMS-Q, (a) scanning electron microscopy (SEM), (b) transmission electron microscopy (TEM), (c) element distribution, (d) low-pass filtered atomic resolution STEM-ADF, (e) Figure 7 Enlarged portion marked by the box in d; Mo k-edge (f) XANES and (h) EXAFS analysis spectra of Fe-M-HoMS-Q, and Fe k-edge (g) XANES and (i) EXAFS analysis spectra.

[0026] Figure 8 Atomically resolved electron energy loss spectrum of Fe-M-HoMS-Q.

[0027] Fig. 9Fitting results of the experimental EXAFS function (solid line) and the calculated Mo-Mo and Mo-S contributions (dotted lines), (a) Mo EXAFS spectrum of Mo foil in K space, (b) Mo EXAFS spectrum of MoS2 in K space, (c) Mo EXAFS spectrum of Fe-M-HoMS-Q in K space, (d) Mo EXAFS spectrum of Mo foil in K space, (e) Mo EXAFS spectrum of MoS2 in R space, (f) Mo EXAFS spectrum of Fe-M-HoMS-Q in R space.

[0028] Fig.10 Fitting results of the experimental EXAFS function (solid line) and the calculated Fe-Fe, Fe-O and Fe-S contributions (dotted lines), (a) Fe EXAFS spectrum of Fe foil in K space, (b) Fe EXAFS spectrum of FeS2 in K space, (c) Fe EXAFS spectrum of Fe-M-HoMS-Q in K space, (d) EXAFS spectrum of Fe foil in R space, (e) Fe EXAFS spectrum of FeS2 in R space, (f) Fe EXAFS spectrum of Fe-M-HoMS-Q in R space.

[0029] Fig.11 Electrochemical impedance spectroscopy of Fe-M-HoMS.

[0030] Fig.12 Electrochemical performances of Fe-M-HoMS in half-cell system (ag) and Fe-M-HoMS / / NVP@C full-cell system (hj). (a) MoS2, MF-HoMS-Q and Fe-M-HoMS-Q at 0.1, 0.2, 0.5, 1.0, 2.0, 5.0, 10.0, 20.0, 30.0 and 0.1 A g -1 The rate performance at a current density of (a) 0.1 A g -1 Cycling stability under different current densities, (c) the difference in peak current density and voltage between the anodic peak and the cathodic peak in the CV curve, (d) the current density is 0.1 A g -1 Cyclic stability of Fe-M-HoMS with different shells at current densities of 0.1, 0.2, 0.5, 1.0, 2.0, 5.0, 10.0, 20.0, 30.0 and 0.1 A g -1 (f) Rate performance comparison with other MoS2 composite materials, (g) Fe-M-HoMS-Q at 5Ag -1 Cycling stability under current density, (h) schematic diagram of Fe-M-HoMS / / NVP@C full cell, (i) CV curves of the full cell at different scan rates, (j) rate performance of the full cell.

[0031] Fig.13 CV curves of the third cycle of Fe-M-HoMS with different shell layers.

[0032] Fig.14 Fe-M-HoMS-Q at 0.1A·g -1 Constant current charge and discharge test at current density. DETAILED DESCRIPTION

[0033] The present invention is further described below through specific examples and electrochemical effect tests.

[0034] Example 1

[0035] Step S0: Preparation of Fe2(MoO4)3 hollow four-shell spheres (FMO-HoMS-Q):

[0036] 2.94g (0.00238mol) (NH4)2MoO4·4H2O, 1.8g (0.00856mol) citric acid and 8.2g (0.03034mol) FeCl3·6H2O were dissolved in 22.5mL deionized water in turn. After complete dissolution, 7.5mL anhydrous ethanol was added and stirred evenly. Then 0.6g carbon spheres were added to the above solution and ultrasonicated for 15min. Then, the metal ions were adsorbed at a constant temperature of 50℃ in a water bath for 24 hours. After the reaction was completed, the material was separated by suction filtration and washed alternately with water and ethanol. The separated material was dried and ground to obtain a brown powdery precursor. The collected precursor was quenched in a muffle furnace at 1℃ min -1 The heating rate was increased to 450℃ and calcined for 1h to obtain Fe2(MoO4)3 hollow four-shell spheres (FMO-HoMS-Q).

[0037] Step S1: Fe2(MoO4)3 hollow four-shell spheres and S powder were placed on both sides of a quartz boat at a weight ratio of 1:4, and then heated to 350℃ in a nitrogen atmosphere and calcined for 2h for sulfurization at a heating rate of 5℃ min -1 , and finally FeS2 / MoS2 hollow four-shell spheres (MF-HoMS-Q) were obtained.

[0038] Step S2: Place the FeS2 / MoS2 hollow four-shell sphere in a Fe2(SO4)3 solution and keep it in a 30°C water bath for 24 hours to allow FeS2 to react with trivalent iron ions to generate FeSO4 that dissolves in the aqueous solution and remove FeS2. After the reaction is complete, separate it with a centrifuge and wash it twice (9000 r min -1 , 10min), oven dried. Then at 5℃ min -1The material was calcined at a heating rate of 800 °C in a nitrogen atmosphere for 2 h to obtain Fe single atom-doped porous MoS2 hollow four-shell sphere (Fe-M-HoMS-Q) sodium ion battery negative electrode material, which was in the form of black powder.

[0039] Example 2

[0040] Step S0: Preparation of Fe2(MoO4)3 hollow four-shell spheres (FMO-HoMS-Q):

[0041] 2.9g (0.00234mol) (NH4) 2MoO4·4H2O, 1.9g (0.00904mol) citric acid and 8g (0.02959mol) FeCl3·6H2O were dissolved in 22.5mL deionized water in turn. After complete dissolution, 7.5mL anhydrous ethanol was added and stirred evenly. Then 0.6g carbon spheres were added to the above solution and ultrasonicated for 15min. Then, the metal ions were adsorbed at a constant temperature of 50°C for 24 hours. After the reaction was completed, the material was separated by suction filtration and washed alternately with water and ethanol. The separated material was dried and ground to obtain a brown powder precursor. The collected precursor was quenched in a muffle furnace at 1°C min -1 The heating rate was increased to 440 °C and calcined for 1 h.

[0042] Step S1: Fe2(MoO4)3 hollow four-shell spheres and S powder were placed on both sides of a quartz boat at a weight ratio of 1:5, and then heated to 330°C in a nitrogen atmosphere and calcined for 2 h for sulfurization at a heating rate of 4°C min -1 , and finally FeS2 / MoS2 hollow four-shell spheres (MF-HoMS-Q) were obtained.

[0043] Step S2: Place the FeS2 / MoS2 hollow four-shell sphere in a Fe2(SO4)3 solution and keep it in a 30°C water bath for 24 hours to allow FeS2 to react with trivalent iron ions to generate FeSO4 that dissolves in the aqueous solution and remove FeS2. After the reaction is complete, separate it with a centrifuge and wash it twice (9000 r min -1 , 10min), oven dried. Then at 5℃ min -1 The material was calcined at a heating rate of 800 °C in a nitrogen atmosphere for 2 h to obtain Fe single atom-doped porous MoS2 hollow four-shell sphere (Fe-M-HoMS-Q) sodium ion battery negative electrode material, which was in the form of black powder.

[0044] Example 3

[0045] Step S0: Preparation of Fe2(MoO4)3 hollow four-shell spheres (FMO-HoMS-Q):

[0046] 3g (0.00242mol) (NH4) 2MoO4.4H2O, 1.8g (0.00856mol) citric acid and 8.4g (0.03107mol) FeCl3.6H2O were dissolved in 22.5mL deionized water in turn. After complete dissolution, 7.5mL anhydrous ethanol was added and stirred evenly. Then 0.6g carbon spheres were added to the above solution and ultrasonicated for 15min. Then, the metal ions were adsorbed at a constant temperature of 50°C for 24 hours. After the reaction was completed, the material was separated by suction filtration and washed alternately with water and ethanol. The separated material was dried and ground to obtain a brown powder precursor. The collected precursor was quenched in a muffle furnace at 1°C min -1 The heating rate was increased to 460 °C and calcined for 1 h.

[0047] Step S1: Fe2(MoO4)3 hollow multi-shell spheres and S powder were placed on both sides of a quartz boat at a weight ratio of 1:6, and then heated to 370°C in a nitrogen atmosphere and calcined for 2 h for sulfurization at a heating rate of 6°C min -1 , and obtained FeS2 / MoS2 hollow four-shell spheres (MF-HoMS-Q).

[0048] Step S2: Place the FeS2 / MoS2 hollow four-shell sphere in a Fe2(SO4)3 solution and keep it in a 30°C water bath for 24 hours to allow FeS2 to react with trivalent iron ions to generate FeSO4 that dissolves in the aqueous solution and remove FeS2. After the reaction is complete, separate it with a centrifuge and wash it twice (9000 r min -1 , 10min), oven dried. Then at 5℃ min -1 The material was calcined at a heating rate of 800 °C in a nitrogen atmosphere for 2 h to obtain Fe single atom-doped porous MoS2 hollow four-shell sphere (Fe-M-HoMS-Q) sodium ion battery negative electrode material, which was in the form of black powder.

[0049] Example 4

[0050] Step S0: Preparation of Fe2(MoO4)3 hollow single shell spheres (FMO-HoMS-S):

[0051] 2.94g (0.00238mol) (NH4) 2MoO4.4H2O, 1.8g (0.00856mol) citric acid and 8.2g (0.03034mol) FeCl3.6H2O were dissolved in 30mL deionized water, and then 0.6g carbon spheres were added to the above solution and ultrasonicated for 15min. Then, the metal ions were adsorbed in a 30℃ water bath for 6 hours. After the reaction was completed, the material was separated by suction filtration and washed with water. The separated material was dried and ground to obtain a brown powder precursor. The collected precursor was precipitated in a muffle furnace at 1℃ min -1The heating rate was increased to 450 °C and calcined for 1 h.

[0052] Step S1: Fe2(MoO4)3 hollow single-shell spheres and S powder were placed on both sides of a quartz boat at a weight ratio of 1:4, and then heated to 350℃ in a nitrogen atmosphere and calcined for 2h for sulfurization at a heating rate of 5℃ min -1 , and finally FeS2 / MoS2 hollow single-shell spheres (MF-HoMS-S) were obtained.

[0053] Step S2: Place the FeS2 / MoS2 hollow single-shell sphere in a Fe2(SO4)3 solution and react at 30°C for 24 hours to allow FeS2 to react with trivalent iron ions to generate FeSO4 that dissolves in the aqueous solution and remove FeS2. After the reaction is complete, separate the FeS2 / MoS2 hollow single-shell sphere with a centrifuge and wash it twice with water (9000 rmin). -1 , 10min), oven dried. Then at 5℃ min -1 The material was calcined at a heating rate of 800 °C in a nitrogen atmosphere for 2 h to obtain Fe single atom-doped porous MoS2 hollow single-shell sphere (Fe-M-HoMS-S) sodium ion battery negative electrode material, which was in the form of black powder.

[0054] Example 5

[0055] Step S0: Preparation of Fe2(MoO4)3 hollow double shell spheres (FMO-HoMS-D):

[0056] 2.94g (0.00238mol) (NH4) 2MoO4.4H2O, 1.8g (0.00856mol) citric acid and 8.2g (0.03034mol) FeCl3.6H2O were dissolved in 30mL deionized water, and then 0.6g carbon spheres were added to the above solution and ultrasonicated for 15min. After constant temperature adsorption of metal ions in a 30℃ water bath for 24 hours, the metal ions were filtered and washed with water for separation. The separated material was dried and ground to obtain a brown powder precursor. The collected precursor was heated in a muffle furnace at 1℃ min -1 The heating rate was increased to 450 °C and calcined for 1 h.

[0057] Step S1: Fe2(MoO4)3 hollow double-shell spheres and S powder were placed on both sides of a quartz boat at a weight ratio of 1:4, and then heated to 350℃ in a nitrogen atmosphere and calcined for 2h for sulfurization at a heating rate of 5℃ min -1 , FeS2 / MoS2 hollow double-shell spheres (MF-HoMS-D) were obtained.

[0058] Step S2: Place the FeS2 / MoS2 hollow double-shell sphere in a Fe2(SO4)3 solution and keep it in a constant temperature at 30°C for 24 hours to allow FeS2 to react with trivalent iron ions to generate FeSO4 that dissolves in the aqueous solution and remove FeS2. After the reaction is complete, separate the FeS2 / MoS2 hollow double-shell sphere with a centrifuge and wash it twice with water (9000 r min). -1 , 10min), oven dried. Then at 5℃ min -1 The material was calcined at a heating rate of 800 °C in a nitrogen atmosphere for 2 h to obtain Fe single atom-doped porous MoS2 hollow double-shell spheres (Fe-M-HoMS-D) as sodium ion battery negative electrode material, and the material was in the form of black powder.

[0059] Example 6

[0060] Step S0: Preparation of Fe2(MoO4)3 hollow three-shell spheres (FMO-HoMS-T):

[0061] 2.94g (0.00238mol) (NH4) 2MoO4.4H2O, 1.8g (0.00856mol) citric acid and 8.2g (0.03034mol) FeCl3.6H2O were dissolved in 30mL deionized water, and then 0.6g carbon spheres were added to the above solution and ultrasonicated for 15min, followed by constant temperature adsorption of metal ions at 50°C for 24 hours. After the reaction was completed, the material was separated by suction filtration and washed with water. The separated material was dried and ground to obtain a brown powdery precursor. The collected precursor was quenched in a muffle furnace at 1°C min -1 The heating rate was increased to 450 °C and calcined for 1 h.

[0062] Step S1: Fe2(MoO4)3 hollow three-shell spheres and S powder were placed on both sides of a quartz boat at a weight ratio of 1:4, and then heated to 350℃ in a nitrogen atmosphere and calcined for 2h for sulfurization at a heating rate of 5℃ min -1 , and obtained FeS2 / MoS2 hollow three-shell spheres (MF-HoMS-T).

[0063] Step S2: Place the FeS2 / MoS2 hollow three-shell sphere in a Fe2(SO4)3 solution and react at 30°C for 24 hours to allow FeS2 to react with trivalent iron ions to generate FeSO4 that dissolves in the aqueous solution and remove FeS2. After the reaction is complete, separate the FeS2 / MoS2 hollow three-shell sphere with a centrifuge and wash it twice with water (9000 r min). -1 , 10min), oven dried. Then at 5℃ min -1 The material was calcined at a heating rate of 800 °C in a nitrogen atmosphere for 2 h to obtain Fe single atom-doped porous MoS2 hollow three-shell spheres (Fe-M-HoMS-T) as a negative electrode material for sodium ion batteries, and the material was in the form of black powder.

[0064] XRD tests were performed on FMO-HoMS-Q, MF-HoMS-Q, Fe-M-HoMS-Q in Example 1, FMO-HoMS-(S,D,T), MF-HoMS-(S,D,T), Fe-M-HoMS-(S,D,T) in Examples 4-6, and the test results are shown in Figure 1 , Figure 2 .from Figure 1 From the XRD spectrum of a, it can be seen that the characteristic peaks of FMO-HoMS with different shells are consistent with the standard card of Fe2(MoO4)3, which proves the successful synthesis of Fe2(MoO4)3. x The XRD spectrum of HoMS (MF-HoMS-Q) is shown in Figure 1 As shown in b, it proves that MoS2 and FeS are successfully synthesized after sulfurization. x . Figure 2 The XRD spectrum of Fe-M-HoMS is shown in Figure 2. Its characteristic peaks are consistent with those of the standard card (PDF#83-1701) of 2H-MoS2 and are confirmed by high-resolution transmission electron microscopy (HRTEM). Figure 3 As shown in the figure, the lattice spacing is 0.613nm, which corresponds to the (002) crystal plane of 2H-MoS2. In addition, no characteristic peaks of Fe and its compounds were observed in the spectrum. Therefore, it can be proved that FeS x After the redox reaction with Fe2(SO4)3, FeS x is removed while 2H-MoS2 is retained.

[0065] The porous multi-shell structure obtained after chemical etching can be confirmed by nitrogen adsorption-desorption curves, pore size distribution curves, scanning electron microscopy and transmission electron microscopy. Figure 4 a, 4b are the nitrogen adsorption and desorption isotherms and pore size distribution curves of Fe-M-HoMS-Q, MF-HoMS-Q and FMO-HoMS-Q in Example 1. It can be seen from the figure that the specific surface area and pore volume of Fe-M-HoMS-Q are 48.95m 2 g -1 and 0.173cm 3 g -1 The Fe-M-HoMS-Q in Example 1 and the Fe-M-HoMS-(S,D,T) in Examples 4-6 were characterized by scanning (SEM) and transmission (TEM). The characterization results are shown in Figure 5 , 7a, 7b. SEM and TEM images prove the successful synthesis of hollow sphere structures with different shell layers. It can also be seen from the figure that the HoMS structure is not destroyed after chemical etching. In addition, due to the FeS x The loss of , the shell surface formed abundant pores, this result also proved the formation of porous multilayer structure. Figure 6 Energy dispersive spectroscopy (EDS), the element distribution shown in 7c, and the element composition shown in Table 1 prove that in addition to molybdenum and sulfur, iron is also uniformly dispersed in the porous MoS2.

[0066] Table 1 Elemental composition of Fe-M-HoMS-Q

[0067]

[0068] In order to further prove the doping of Fe single atoms and explore the specific occupation position of Fe single atoms in MoS2, atomic resolution STEM-ADF imaging was performed ( Figure 7 d) Analysis. No particles or clusters belonging to metallic iron or iron compounds were detected, which proves the presence of single iron atoms. In addition, the single substitution defects observed in the figure are caused by the doping of Fe single atoms into MoS2. Figure 7 e is Figure 7 d is a partial enlarged view of the boxed part. Figure 7 As shown in Figure e, S (darker) and Mo (brighter) atoms are clearly observed in the MoS2 lattice according to the atomic number (Z) comparison. However, the originally ordered Mo atoms become disordered in the honeycomb atomic structure of MoS2. This phenomenon can be attributed to the doping of Fe single atoms. In the atomic-scale STEM-EELS analysis, the L2,3 edge features of Fe atoms further confirmed this phenomenon ( Figure 8 The electronic structure information of Fe and Mo atoms was detected by extended X-ray absorption fine structure (EXAFS) and X-ray absorption near edge structure (XANES). Figure 7 As shown in f, the Mo k-edge XANES spectrum of Fe-M-HoMS-Q is located between the Mo foil and standard MoS2, which indicates that the valence state of Mo is reduced due to the formation of defects caused by Fe atom doping. Fe k-edge XANES spectrum of Fe-M-HoMS-Q ( Figure 7 g) is close to standard FeS2, indicating that the valence states of Fe include +2 and +3. At the same time, the R-space EXAFS spectrum of Fe-M-HoMS-Q ( Figure 7 h and Figure 7The strength of Mo-S and Mo-Mo in i) is lower than that of pure MoS2, indicating the formation of defects and edges. In particular, no Fe-Fe bonds were found, confirming that the Fe atoms in Fe-M-HoMS exist in single atomic form. In addition, using metal foil and metal sulfide as standard states ( Fig. 9 and Fig.10 ), the specific coordination number was further proved by fitting the EXAFS spectra in R space and K space, among which, it was further proved that the coordination ratio of single Fe atom to S and O was 1 / 2 (marked as FeO4), as shown in Table 2. Therefore, it can be concluded that single Fe atoms are doped into the MoS2 lattice in Fe-M-HoMS, which leads to the formation of defects and the change of coordination environment, promoting the electrochemical reaction to obtain excellent rate performance.

[0069] Table 2 EXAFS spectrum fitting results of Fe-M-HoMS-Q in R space and K space

[0070]

[0071] By assembling 2032-type button cells in a glove box with an oxygen and water content of 0.1 ppm, the effect of Fe single atoms on the electrochemical performance was investigated using pure MoS2 and MF-HoMS-Q as comparisons. Fig.12 a, the current densities are 0.1, 0.2, 0.5, 1.0, 2.0, 5.0, 10.0, 20.0, 30.0 and 0.1A respectively -1 The constant current charge and discharge experiments verified the rate performance of the material. Obviously, the specific capacities of Fe-M-HoMS-Q at different current densities are 498.9, 414.4, 383.6, 357.7, 333.1, 300.0, 269.3, 239.8, 213.3 and 417.1 mAh g -1 , which is higher than that of MoS2 and MF-HoMS-Q, showing better rate performance. In addition, Fe-M-HoMS-Q has a higher rate performance at a current density of 0.1 A g -1 In the case of -1 The initial specific capacity of the battery is higher than that of the battery with a lower attenuation rate during the cycle. After 100 cycles, a higher capacity is retained ( Fig.12 b), which indicates that Fe-M-HoMS-Q has better cycling stability.

[0072] In addition, the effect of structural design on the electrochemical performance of SIB negative electrode was studied. First, electrochemical impedance spectroscopy was performed on the material. Fig.11 As shown, Fe-M-HoMS-Q exhibits the smallest charge transfer resistance (Rct) between the electrolyte and electrode materials. Fig.12 c is the difference in peak current density and voltage between the anodic peak and the cathodic peak (according to Fig.13 The CV curves of different shells are summarized, and the voltage window is 0.1-2.8V). It can be seen from the figure that the potential difference between the oxidation peak and the reduction peak decreases with the increase of the number of shells, that is, the polarization becomes smaller. The peak current increases with the increase of the number of shells, indicating that the specific capacity increases. In addition, the constant current charge and discharge test confirms that Fe-M-HoMS-Q has a higher specific capacity than other shells ( Fig.14 ). In addition, Fe-M-HoMS-Q has good cycling stability. -1 In the case of the fourth cycle, the specific capacity is 462.6 mAhg -1 , the specific capacity after 100 cycles is 442 mAh g -1 ( Fig.12 d), superior to other shells. Even at 5A g -1 At a high current density of 2.5, 259.4 mAh g-1 was retained after 500 cycles. -1 (83.68%) Fig.12 g) In addition, if Fig.12 As shown in e, all Fe-M-HoMS materials exhibit excellent rate performance. In particular, Fe-M-HoMS-Q -1 The specific capacity is as high as 498.9 mAh g -1 , at 30A g -1 At an ultra-high current density of 213.3 mAh g -1 When the current density returns to 0.1A g -1 417.1mAh g was restored -1 The specific capacity shows excellent rate performance, which is better than most reported MoS2-based anode materials ( Fig.12 f). Therefore, Fe-M-HoMS-Q has a shorter Na + Diffusion path, with excellent rate performance. In addition, due to the unique HoMS structure, Fe-M-HoMS-Q has the property of buffering volume expansion and has excellent cycle stability.

[0073] In order to further explore the practical value of Fe-M-HoMS-Q, a Fe-M-HoMS-Q / / NVP@C full battery was assembled with homemade NVP@C as the positive electrode ( Fig.12 h) Test the battery's charge and discharge rate performance by performing CV tests at different scan rates and constant current charge and discharge tests at different current densities. Fig.12 As shown in Fig. 1, as the scan rate increases from 0.1 mV s -1 Increase to 0.3mV s-1 , the slight change in the peak position demonstrates the excellent rate performance. -1 At this current density, the specific capacity of the cathode reaches 129.4 mAh g -1 ( Fig.12 j), in 2A g -1 At a high current density, the specific capacity remains at 55.0 mAh g -1 In particular, when the current density returns to 0.05A g -1 When the battery is charged, it can still reach 128.4mAh g -1 , which means excellent rate performance.

[0074] In summary, Fe-M-HoMS-Q as a negative electrode material for sodium-ion batteries has high specific capacity, excellent cycle stability and rate performance.

Claims

1. A method for preparing a negative electrode material for a sodium ion battery, characterized in that The steps include: Step S1: sulfiding Fe2(MoO4)3 hollow single-shell or multi-shell spheres with S powder at a weight ratio of 1:4-6 at 330-370° C. in an inert atmosphere to obtain FeS2 / MoS2 hollow single-shell or multi-shell spheres; Step S2: placing the FeS2 / MoS2 hollow single-shell or multi-shell sphere in a trivalent iron ion solution for reaction, so that FeS2 reacts chemically with the trivalent iron ions to remove FeS2, separating the precipitate and calcining it at 800°C in an inert atmosphere to obtain a Fe single-atom doped porous MoS2 hollow single-shell or multi-shell sphere sodium ion battery negative electrode material.

2. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, wherein: The method further comprises step S0: the preparation steps of the Fe2(MoO4)3 hollow single-shell or multi-shell spheres are as follows: (NH4)2MoO4·4H2O, citric acid and FeCl3·6H2O are dissolved in water or a mixed solvent of water and ethanol to obtain a solution, and then carbon spheres are added to the solution and adsorb metal ions for several hours, the precursor is separated and the precursor is calcined in a muffle furnace at 440-460°C to obtain Fe2(MoO4)3 hollow single-shell or multi-shell spheres, and the number of shells of the Fe2(MoO4)3 hollow single-shell or multi-shell spheres is adjusted by the volume ratio of water to ethanol in the solution and the time and temperature for adsorbing metal ions.

3. The method for preparing a negative electrode material for a sodium ion battery according to claim 2, characterized in that: The weight ratio of the (NH4)2MoO4·4H2O, citric acid and FeCl3·6H2O is 2.9-3:1.8-1.9:8.2-8.4, the adsorption is carried out at a temperature of 30-50°C, and the solution uses water or a mixed solvent with a volume ratio of water to ethanol of 3:

1.

4. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, wherein: In step S2, the ferric iron solution is a Fe2(SO4)3 solution.

5. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, wherein: The inert atmosphere is nitrogen or argon.

6. A negative electrode material for a sodium ion battery, characterized in that It is prepared by the preparation method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Cobaltosic oxide multi-shell hollow sphere cathode material for lithium ion battery and preparation method thereof

    CN103247777A

  • Double metal selenide Fe2CoSe4 material of porous structure and preparation method and application thereof

    CN108892111A

  • MoS1.5 Se0.5 coated VS2 composite material and preparation method thereof

    CN116632199A

  • Conductive paste based on nano-hybrid materials

    US20210380814A1

Cited By

  • Preparation method of sodium sulfide carbon confinement pre-sodium coating based on monatomic catalysis

    CN120978015A