Heat-resistant, waterproof and high-hardness ink for helmets and preparation method thereof

By introducing the polymerization reaction of naphthalene ring and silicone group into polyurethane ink, a temperature-resistant and water-resistant high-hardness ink is prepared, which solves the problem of insufficient temperature resistance and hardness performance of polyurethane ink in outdoor applications, and significantly improves the water resistance of the ink and heat resistance have expanded its application in helmets and other fields.

CN118063999BActive Publication Date: 2024-11-19DONGGUAN WUREN NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410210057.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2024-11-19
Estimated Expiration
2044-02-26

AI Technical Summary

Technical Problem

Traditional polyurethane inks have poor temperature resistance and poor hardness and tensile properties in outdoor applications, resulting in aging and cracking of the ink, affecting the appearance and performance of the material.

Method used

By introducing a polyurethane ink linker with naphthalene ring and siloxane groups, 2,2-dihydroxymethylpropionic acid, isocyanate monomer, polyester polyol and 1.3-bis(3-hydroxypropylnaphthalene)tetramethyl Disiloxane is polymerized and combined with color paste, defoaming agent and leveling agent to prepare temperature-resistant, waterproof and high hardness ink.

Benefits of technology

It improves the peel strength, hardness and tensile properties of ink, reduces water absorption, improves water and heat resistance, and expands the application of polyurethane ink in outdoor materials such as helmets and signs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004714561130000021
    Figure BDA0004714561130000021
  • Figure BDA0004714561130000061
    Figure BDA0004714561130000061
Patent Text Reader

Abstract

The invention relates to the technical field of inks, and discloses a heat-resistant, waterproof, high-hardness ink for helmets and a preparation method thereof. The invention introduces naphthalene rings and siloxane groups into the main chain of the polyurethane ink linker molecule. The naphthalene rings have the characteristics of high rigidity, high thermal stability and strong structural stability; the siloxane groups have the characteristics of good toughness, high water resistance, strong temperature resistance, etc., which improve the peel strength, hardness and tensile properties of the polyurethane ink. At the same time, the water absorption rate of the polyurethane ink is reduced, the initial thermal decomposition temperature is increased, and good water-resistant, waterproof and heat-resistant properties are exhibited. The practical application of polyurethane ink in outdoor materials such as helmets, safety helmets, and signboards is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inks, in particular to a heat-resistant, waterproof and high-hardness ink for helmets and a preparation method thereof. Background Art

[0002] Polyurethane ink has good film-forming properties, good gloss and excellent elasticity, and is widely used in helmets, signboards, packaging bags, printing, etc. At present, polyurethane ink mainly uses toluene, butanone, etc. as solvents, which are highly toxic and do not meet environmental protection requirements.

[0003] In recent years, the development of environmentally friendly water-based polyurethane inks has been a research hotspot, but water-based polyurethanes have poor water resistance and waterproof performance, poor temperature resistance and other problems; for example, materials such as helmets, safety helmets, and signboards are often outdoors for a long time, and are exposed to long-term heat and rain. The ink or paint on the surface is prone to aging and cracking, which affects the appearance and performance of the materials and is not conducive to the practical application of water-based polyurethane in outdoor materials such as helmets, safety helmets, and signboards. The patent with announcement number CN105778621B discloses bacterial cellulose modified with silane coupling agents and water-based polyurethane prepolymers as ink binders. The obtained water-based polyurethane ink binder has low water absorption and good water resistance. However, the patent does not improve the problems of poor hardness, tensile strength, and temperature resistance of polyurethane inks. Summary of the invention

[0004] The invention solves the problems of poor temperature resistance, hardness, tensile strength and other properties of traditional polyurethane, and expands the practical application of polyurethane ink in the fields of helmets and the like.

[0005] The technical solution of the present invention:

[0006] A method for preparing heat-resistant, waterproof and high-hardness ink:

[0007] S1. Add dehydrated polyester polyol, diisocyanate monomer, 2,2-dihydroxymethylpropionic acid into the reaction bottle, heat to 75-85°C, add catalyst dibutyltin dilaurate dropwise, react for 3-4h, then add 1.3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane as a chain extender, continue to react for 1-2h, add triethylamine after cooling, adjust the pH to 7-7.5, then add water, control the solid content to 35-45%, shear emulsify, and obtain the polyurethane ink connecting material.

[0008] S2. Add color paste, defoamer and leveling agent to the polyurethane ink vehicle, perform shear emulsification, and obtain a heat-resistant, waterproof and high-hardness ink.

[0009] Among them, the mass of 2,2-dimethylol propionic acid is 8-9.5% of the total mass of polyester polyol and diisocyanate monomer.

[0010] The mass of 1.3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane is 15-22% of the total mass of the polyester polyol and the diisocyanate monomer.

[0011] The diisocyanate monomers include toluene-2,4-diisocyanate, 4,4'-methylenebis(phenyl isocyanate), and isophorone diisocyanate.

[0012] Among them, the preparation method of 1,3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane is: add 1.3-bis(3-carboxypropyl)tetramethyldisiloxane and 3-(1-naphthyloxy)-1,2-epoxypropane to any one of toluene, xylene and 1,4-dioxane, dropwise add catalyst N,N-dimethylbenzylamine, after the reaction, rotary evaporate the solution, wash the product with methanol, and recrystallize the product from toluene to obtain 1.3-bis(3-carboxypropyl)tetramethyldisiloxane. The reaction formula is as follows:

[0013]

[0014] The masses of 3-(1-naphthyloxy)-1,2-propylene oxide and N,N-dimethylbenzylamine are 125-140% and 1.3-1.8% of the mass of 1.3-bis(3-carboxypropyl)tetramethyldisiloxane, respectively.

[0015] Wherein, in the preparation method of 1,3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane, the reaction temperature is controlled at 90-120° C. and the reaction time is 4-8 hours.

[0016] Among them, the application of heat-resistant, waterproof and high-hardness ink in helmets.

[0017] Technical effect: The present invention uses N,N-dimethylbenzylamine as a catalyst to catalyze the reaction of the epoxy groups of 1.3-bis(3-carboxypropyl)tetramethyldisiloxane and 3-(1-naphthyloxy)-1,2-epoxypropane to obtain a new diol monomer 1.3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane; as a polyurethane chain extender, it is polymerized with polyester polyols, diisocyanates, and 2,2-dihydroxymethylpropionic acid to obtain a polyurethane ink linker whose main chain contains naphthalene rings and siloxane groups, and finally mixed with color paste, defoaming agent, etc. to obtain a heat-resistant, waterproof and high-hardness ink.

[0018] The present invention introduces naphthalene rings and siloxane groups into the main chain of the polyurethane ink connecting material molecule. The naphthalene ring has the characteristics of high rigidity, high thermal stability and strong structural stability; the siloxane group has the characteristics of good toughness, high water resistance and strong temperature resistance, which improves the peel strength, hardness and tensile properties of the polyurethane ink. At the same time, the water absorption rate of the polyurethane ink is reduced, the initial thermal decomposition temperature is increased, and good water and heat resistance are shown. The practical application of polyurethane ink in outdoor materials such as helmets, safety helmets, and signboards is expanded. DETAILED DESCRIPTION

[0019] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, deformation schemes, improved schemes, equivalent schemes, and other technical solutions that do not deviate from the spirit and scope of the present invention.

[0020] The polyester polyol in the embodiment of the present invention is polyethylene adipate, with a molecular weight of 1000 and a content of ≧99%. The CAS number of 1.3-bis(3-carboxylpropyl)tetramethyldisiloxane is 3353-68-2. The color paste is water-based titanium dioxide paste-W21-SJ, the defoamer is Foamaster MO 2190, and the leveling agent is BYK-346.

[0021] Example 1

[0022] (1) Add 2 g of 1,3-bis(3-carboxypropyl)tetramethyldisiloxane and 2.5 g of 3-(1-naphthyloxy)-1,2-epoxypropane to 1,4-dioxane solvent, dropwise add 36 mg of catalyst N,N-dimethylbenzylamine, raise the temperature to 90°C, react for 8 h, rotary evaporate the solution, wash the product with methanol, and recrystallize the product from toluene to obtain 1.3-bis(3-carboxypropyl)tetramethyldisiloxane.

[0023] (2) Add 10 g of dehydrated polyester polyol (molecular weight 1000), 4.5 g of isophorone diisocyanate, and 1.5 g of 2,2-dihydroxymethylpropionic acid into a reaction bottle, raise the temperature to 75°C, add 8 mg of catalyst dibutyltin dilaurate dropwise, react for 4 h, then add 2.18 g of 1.3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane as a chain extender, continue to react for 1 h, add triethylamine after cooling, adjust the pH to 7.5, then add water to control the solid content to 35%, and shear emulsify to obtain a polyurethane ink binder.

[0024] (3) Add 12 mL of color paste, 0.3 g of defoaming agent, and 0.22 g of leveling agent to the polyurethane ink vehicle, and shear and emulsify to obtain a heat-resistant, waterproof, and high-hardness ink.

[0025] Example 2

[0026] (1) Add 2 g of 1.3-bis(3-carboxypropyl)tetramethyldisiloxane and 2.8 g of 3-(1-naphthyloxy)-1,2-epoxypropane to a toluene solvent, dropwise add 26 mg of a catalyst, N,N-dimethylbenzylamine, raise the temperature to 100° C., react for 8 h, rotary evaporate the solution, wash the product with methanol, and recrystallize the product from toluene to obtain 1.3-bis(3-carboxypropyl)tetramethyldisiloxane.

[0027] (2) Add 10 g of dehydrated polyester polyol (molecular weight 1000), 3.8 g of toluene-2,4-diisocyanate, and 1.3 g of 2,2-dihydroxymethylpropionic acid into a reaction bottle, heat to 80°C, drop 15 mg of catalyst dibutyltin dilaurate, react for 3 h, then add 2.75 g of 1.3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane as a chain extender, continue to react for 2 h, cool, add triethylamine, adjust the pH to 7, then add water to control the solid content to 45%, shear emulsify, and obtain a polyurethane ink binder.

[0028] (3) Add 12 mL of color paste, 0.3 g of defoaming agent, and 0.22 g of leveling agent to the polyurethane ink vehicle, and shear and emulsify to obtain a heat-resistant, waterproof, and high-hardness ink.

[0029] Example 3

[0030] (1) Add 2 g of 1.3-bis(3-carboxypropyl)tetramethyldisiloxane and 2.8 g of 3-(1-naphthyloxy)-1,2-epoxypropane to a xylene solvent, dropwise add 30 mg of a catalyst, N,N-dimethylbenzylamine, raise the temperature to 120° C., react for 4 h, rotary evaporate the solution, wash the product with methanol, and recrystallize the product from toluene to obtain 1.3-bis(3-carboxypropyl)tetramethyldisiloxane.

[0031] (2) Add 10 g of dehydrated polyester polyol (molecular weight 1000), 5.2 g of 4,4'-methylenebis(phenyl isocyanate), and 1.2 g of 2,2-dihydroxymethylpropionic acid into a reaction bottle, raise the temperature to 85°C, add 15 mg of catalyst dibutyltin dilaurate dropwise, react for 3 h, then add 3.34 g of 1.3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane as a chain extender, continue to react for 2 h, cool, add triethylamine, adjust the pH to 7, then add water to control the solid content to 45%, and shear emulsify to obtain a polyurethane ink binder.

[0032] (3) Add 12 mL of color paste, 0.3 g of defoaming agent, and 0.22 g of leveling agent to the polyurethane ink vehicle, and shear and emulsify to obtain a heat-resistant, waterproof, and high-hardness ink.

[0033] Comparative Example 1

[0034] The main difference between this comparative example and Example 1 is that no 1,3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane chain extender is added.

[0035] (1) Add 10 g of dehydrated polyester polyol (molecular weight 1000), 4.5 g of isophorone diisocyanate, and 1.5 g of 2,2-dimethylol propionic acid into a reaction bottle, heat to 75° C., drop 8 mg of catalyst dibutyltin dilaurate, react for 4 h, cool, add triethylamine, adjust the pH to 7.5, then add water to control the solid content to 35%, and shear emulsify to obtain a polyurethane ink binder.

[0036] (2) Add 12 mL of color paste, 0.3 g of defoaming agent, and 0.22 g of leveling agent to the polyurethane ink vehicle, and shear and emulsify to obtain a polyurethane ink.

[0037] Comparative Example 2

[0038] The main difference between this comparative example and Example 1 is that 1,3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane chain extender is not added, and 1,4-butanediol is added as a chain extender.

[0039] (1) Add 10 g of dehydrated polyester polyol (molecular weight 1000), 4.5 g of isophorone diisocyanate, and 1.5 g of 2,2-dimethylol propionic acid into a reaction bottle, heat to 75°C, drop 8 mg of catalyst dibutyltin dilaurate, react for 4 h, then add 2.18 g of 1,4-butanediol as a chain extender, continue to react for 1 h, cool, add triethylamine, adjust the pH to 7.5, then add water to control the solid content to 35%, shear emulsify, and obtain a polyurethane ink binder.

[0040] (2) Add 12 mL of color paste, 0.3 g of defoaming agent, and 0.22 g of leveling agent to the polyurethane ink vehicle, and shear and emulsify to obtain a polyurethane ink.

[0041] The peel strength of ink was tested according to GB / T 2791-1995 standard.

[0042] The polyurethane ink was dried and cured at 80℃ for 6 hours, and a certain mass (m0) of the ink curing sample was weighed and placed in distilled water for 48 hours. The curing sample was taken out, and the surface moisture was wiped with filter paper, and the weight (m1) was calculated. The water absorption rate = (m1-m0) / m0×100%. The lower the water absorption rate, the better the water resistance.

[0043] The tensile properties of the ink cured samples were tested according to the GB / T 1040.1-2006 method. The hardness of the ink cured samples was tested according to the GB / T531.1-2008 method.

[0044] Thermogravimetric analysis was used to test the thermogravimetric properties of the ink curing samples. Nitrogen was used as the test atmosphere and the heating rate was 10°C / min.

[0045] Table 1 Mechanical strength test of polyurethane ink

[0046]

[0047] Table 2 Water absorption and waterproof performance test of polyurethane ink.

[0048]

[0049]

[0050] Table 3 Thermal decomposition temperature test of polyurethane ink.

[0051] Water absorption (%) Example 1 356.1 Example 2 351.3 Example 3 362.0 Comparative Example 1 332.0 Comparative Example 2 335.4

[0052] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a heat-resistant, waterproof and high-hardness ink, characterized in that: The preparation method is: S1. Add dehydrated polyester polyol, diisocyanate monomer, and 2,2-dihydroxymethylpropionic acid to a reaction bottle, raise the temperature to 75-85°C, drop a catalyst dibutyltin dilaurate, react for 3-4 hours, then add 1,3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane as a chain extender, continue the reaction for 1-2 hours, add triethylamine after cooling, adjust the pH to 7-7.5, then add water, shear and emulsify to obtain a polyurethane ink binder; The structural formula of the 1,3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane is: ; S2, adding color paste, defoamer, and leveling agent to the polyurethane ink vehicle, shearing and emulsifying, and obtaining a heat-resistant, waterproof, and high-hardness ink; The preparation method of 1,3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane is as follows: 1,3-bis(3-carboxypropyl)tetramethyldisiloxane and 3-(1-naphthyloxy)-1,2-propylene oxide are added to a solvent, a catalyst N,N-dimethylbenzylamine is added dropwise, and after the reaction, the solution is rotary evaporated, washed, and recrystallized to obtain 1,3-bis(3-carboxypropyl)tetramethyldisiloxane; The diisocyanate monomer includes toluene-2,4-diisocyanate, 4,4'-methylenebis(phenyl isocyanate) or isophorone diisocyanate.

2. The method for preparing the heat-resistant, waterproof and high-hardness ink according to claim 1, characterized in that: The mass of the 2,2-dimethylol propionic acid is 8-9.5% of the total mass of the polyester polyol and the diisocyanate monomer.

3. The method for preparing the heat-resistant, waterproof and high-hardness ink according to claim 1, characterized in that: The mass of the 1,3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane is 15-22% of the total mass of the polyester polyol and the diisocyanate monomer.

4. The method for preparing the heat-resistant, waterproof and high-hardness ink according to claim 1, characterized in that: The solid content of the polyurethane ink vehicle is 35-45%.

5. The method for preparing the heat-resistant, waterproof and high-hardness ink according to claim 1, characterized in that: The solvent includes toluene, xylene or 1,4-dioxane.

6. The method for preparing the heat-resistant, waterproof and high-hardness ink according to claim 1, characterized in that: The masses of the 3-(1-naphthyloxy)-1,2-epoxypropane and N,N-dimethylbenzylamine are 125-140% and 1.3-1.8% of the mass of 1,3-bis(3-carboxypropyl)tetramethyldisiloxane respectively.

7. The method for preparing the heat-resistant, waterproof and high-hardness ink according to claim 1, characterized in that: In the preparation method of 1,3-bis(3-hydroxypropylnaphthalene)tetramethyldisiloxane, the reaction is controlled at 90-120° C. and the reaction time is 4-8 hours.

8. Use of the heat-resistant, waterproof and high-hardness ink obtained by the preparation method according to any one of claims 1 to 7 in a helmet.

Citation Information

Patent Citations

  • A kind of water-resistant water-based polyurethane ink binder and preparation method thereof

    CN105778621B

  • Environmentally friendly hydrophobic polyurethane ink and preparation method thereof

    CN106009907A

  • Water-resistant high-temperature-resistant single-component waterborne polyurethane adhesive and preparation method thereof

    CN108342181A

  • High-strength and high-toughness polyurethane cementing material and preparation method thereof