Aqueous polyol dispersion and preparation method and application thereof
Through the combination of specific polycarbonate glycols and nonionic emulsifiers, a water-based polyol dispersion with excellent wear resistance and soft feel is prepared, which solves the shortcomings of existing water-based coatings in terms of wear resistance and soft feel, and achieves Improved stability and performance.
Patent Information
- Application Number
- CN202410271787.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-03-11
AI Technical Summary
Existing water-based soft-touch coatings have shortcomings in wear resistance and soft feel, especially the performance of high-demand water-based plastic coatings is not ideal.
By selecting specific polycarbonate glycols, non-ionic emulsifiers and water components, water-based polyol dispersions are prepared, combined with specific group molar ratios and emulsifier structures, to form a dispersion with excellent wear resistance and soft feel. Coating film.
It achieves high wear resistance and soft feel of the coating film in water-based coatings, while ensuring the stability of the dispersion and avoiding the delamination problem of the coating film.
Smart Images

Figure BDA0004734515620000011 
Figure BDA0004734515620000021 
Figure BDA0004734515620000022
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of waterborne coatings, and in particular to a waterborne polyol dispersion and a preparation method and application thereof. Background Art
[0002] As people's living standards improve, their requirements for the tactile feel of plastic coatings, leather coatings, and wood coatings are getting higher and higher. Coatings with a soft touch and good wear resistance have been widely loved, especially environmentally friendly, low-VOC water-based soft-touch polymers have become the focus of research.
[0003] CN107011495A discloses a soft-touch waterborne polyurethane dispersion obtained by reacting an organic polyisocyanate compound, a polycarbonate diol having a specific structure, and a compound containing a carboxyl group and / or a sulfonic group, and the coating has excellent softness. However, the resin prepared by the patent method basically does not contain hydroxyl groups, and no water-dispersible isocyanate curing agent is added during use, so the coating has a low crosslinking density and poor chemical resistance.
[0004] CN111094373A discloses a water-based two-component soft-touch coating, which includes a hydroxyl-containing polyurethane dispersion, a hydroxyl-free polyurethane dispersion, and a water-dispersible isocyanate curing agent. The coating film has good softness and excellent chemical resistance. However, the coating film prepared by the patented method is still not scratch-resistant and abrasion-resistant enough, which is still not enough for high-demand water-based plastic coatings.
[0005] All of the above water-based soft-touch resins have some defects, and a water-based resin with better wear resistance and higher softness is needed. Summary of the invention
[0006] Based on this, the purpose of the present invention is to provide an aqueous polyol dispersion and a preparation method and application thereof. By selecting components such as polycarbonate diol, nonionic emulsifier, water, etc., an aqueous polyol dispersion can be obtained. The dispersion is suitable for water-based coatings and has excellent wear resistance and softness.
[0007] An aqueous polyol dispersion comprises polycarbonate diol, a nonionic emulsifier and water;
[0008] The polycarbonate diol is at least one polycarbonate diol comprising (a), (b), and (c), wherein:
[0009] (a) is a terminal hydroxyl group;
[0010] (b) is a repeating unit represented by formula (1);
[0011]
[0012] (c) is at least one of the repeating unit represented by formula (2), the repeating unit represented by formula (3), and the repeating unit represented by formula (4);
[0013]
[0014] In formula (2), n is 4 or 5;
[0015]
[0016] In formula (3), m=4 or 5;
[0017]
[0018] In the polycarbonate diol, n1 represents the molar amount of the repeating unit represented by formula (1); n2 represents the molar amount of the repeating unit represented by formula (2); n3 represents the molar amount of the repeating unit represented by formula (3); n4 represents the molar amount of the repeating unit represented by formula (4);
[0019] The weight of the nonionic emulsifier is 2-20% of the weight of the polycarbonate diol; the nonionic emulsifier is at least one emulsifier containing alternating polyethylene oxide segments and polypropylene oxide segments; in the nonionic emulsifier, n5 represents the molar amount of the polyethylene oxide segment; n6 represents the molar amount of the polypropylene oxide segment.
[0020] The present invention can obtain an aqueous polyol dispersion by selecting the specific polycarbonate diol, the specific nonionic emulsifier, water and other components. The aqueous polyol dispersion of the present invention has excellent wear resistance and soft feel by limiting the ratio of the groups in the polycarbonate diol and the amount of the substances thereof, and limiting the structure of the nonionic emulsifier and the molar ratio of the polyoxyethylene segments in the nonionic emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments.
[0021] The common polycarbonate diol currently commercialized contains a 1,6-hexanediol structure (i.e., the structure shown in formula (1)), but this structure is very regular, which makes the polycarbonate diol very crystalline, resulting in increased cohesion and reduced softness. The polycarbonate diol described in the present invention, in addition to the repeating unit shown in formula (1), also contains at least one of the repeating units shown in formula (2), the repeating units shown in formula (3), and the repeating units shown in formula (4). The repeating units shown in formula (2), the repeating units shown in formula (3), and the repeating units shown in formula (4) destroy the regular structure of the structure of formula (1), thereby reducing the crystallinity of the polycarbonate diol and achieving a better softness. In the polycarbonate diol described in the present invention, If the molar content of the repeating unit represented by formula (1) is too high, the overall crystallinity of the polycarbonate diol is strong, the cohesion is high, and the softness becomes low; if the molar content of the repeating unit represented by formula (1) is too low, the material cost will be too high. In the polycarbonate diol, If the molar content of the repeating unit represented by formula (2) is too high, the molar content of the repeating unit represented by formula (1) is too low, which will also cause the crystallinity to increase and the material cost to be high. If the molar ratio of the repeating unit represented by formula (3) is too high, when the aqueous polyol dispersion is used to form a coating film of an aqueous coating, the wear resistance of the coating film will decrease. Since the structure of formula (4) has a certain rigidity, if the molar ratio of the repeating unit shown in formula (4) is too high, when the aqueous polyol dispersion is used to form a coating film of an aqueous coating, the coating film will have a poor softness. The structure of the polycarbonate diol has two terminal hydroxyl groups, which serve as cross-linking groups and help cross-link the coating film, so that the coating film has excellent softness and wear resistance.
[0022] In the aqueous polyol dispersion, the weight (addition amount) of the nonionic emulsifier is 2-20% of the weight (addition amount) of the polycarbonate diol. If the weight proportion of the nonionic emulsifier is too low, the emulsification effect is poor and it is difficult to form a stable aqueous polyol dispersion. If the weight proportion of the nonionic emulsifier is too high, when the aqueous polyol dispersion is used for forming a coating film with a water-based coating, the nonionic emulsifier will remain in the coating film, affecting the water resistance of the coating film.
[0023] The nonionic emulsifier of the present invention is a block emulsifier comprising alternating polyethylene oxide segments and polypropylene oxide segments, so that the aqueous polyol dispersion has good stability and is not prone to precipitation and stratification during storage. The nonionic emulsifier of the present invention has a soft structure, which makes the aqueous polyol dispersion softer. If a non-block emulsifier or other types of emulsifiers are used, the aqueous polyol dispersion is unstable and cannot be stably stored, and precipitation and stratification are prone to occur. In the nonionic emulsifier, That is, in the nonionic emulsifier, the molar ratio of the polyethylene oxide segment to the total of the polyethylene oxide segment and the polypropylene oxide segment is 35-85%. If the molar ratio of the polyethylene oxide segment to the total of the polyethylene oxide segment and the polypropylene oxide segment of the nonionic emulsifier is too low or too high, a stable aqueous polyol dispersion cannot be formed.
[0024] The aqueous polyol dispersion of the present invention has excellent softness and wear resistance and good stability through the combination of the above-mentioned specific polycarbonate diol and the specific nonionic emulsifier and the external emulsification of water.
[0025] The polycarbonate diol described in the present invention is at least one polycarbonate diol comprising (a), (b), and (c), which means that the polycarbonate diol described in the present invention is not limited to a single polycarbonate diol. The polycarbonate diol described in the present invention can also be a mixture of two or more polycarbonate diols comprising (a), (b), and (c). For example, the polycarbonate diol is a mixture of polycarbonate diol A1 and polycarbonate diol A2, and both polycarbonate diol A1 and polycarbonate diol A2 contain the structures of (a), (b), and (c). Similarly, the nonionic emulsifier described in the present invention is at least one emulsifier containing alternating polyethylene oxide segments and polypropylene oxide segments, which means that the nonionic emulsifier described in the present invention is not limited to a single emulsifier. The nonionic emulsifier described in the present invention can also be a mixture of two or more nonionic emulsifiers containing alternating polyethylene oxide segments and polypropylene oxide segments, and the molar ratio of polyethylene oxide segments to the total of polyethylene oxide segments and polypropylene oxide segments is 35-85%.
[0026] Furthermore, the number average molecular weight of the polycarbonate diol is 300-10000. The polycarbonate diol with a number average molecular weight of 300-10000 is selected to improve the dispersibility and stability of the aqueous polyol dispersion.
[0027] Furthermore, the nonionic emulsifier is a diblock emulsifier and / or a triblock emulsifier; wherein:
[0028] The diblock emulsifier contains a segment of the chemical structure shown in formula (5);
[0029]
[0030] In formula (5), x and y are integers of 1-100, and x / (x+y)=35-85%;
[0031] The triblock emulsifier contains a segment of the chemical structure shown in formula (6);
[0032]
[0033] In formula (6), x, y, and z are integers of 1-100, and (x+z) / (x+y+z)=35-85%.
[0034] The diblock emulsifier of the present invention is a diblock copolymer composed of a polyethylene oxide segment and a polypropylene oxide segment, wherein x / (x+y)=35-85% in formula (5), i.e., the molar ratio of the polyethylene oxide segment to the total of the polyethylene oxide segment and the polypropylene oxide segment in formula (5) is 35-85%. The triblock emulsifier of the present invention is a triblock copolymer composed of a polyethylene oxide segment, a polypropylene oxide segment and a polyethylene oxide segment, wherein (x+z) / (x+y+z)=35-85%, i.e., the molar ratio of the polyethylene oxide segment to the total of the polyethylene oxide segment and the polypropylene oxide segment in formula (6) is 35-85%. The above two types of emulsifiers (ie, diblock emulsifiers and triblock emulsifiers) used in the aqueous polyol dispersion of the present invention can ensure the storage stability of the aqueous polyol dispersion, and the structures of the two types of emulsifiers are relatively soft, which can improve the softness of the aqueous polyol dispersion.
[0035] Preferably, the diblock emulsifier is at least one of Maxemul 7101 and Maxemul 7102 of Croda. Croda's Maxemul 7101 and Maxemul 7102 are diblock emulsifiers of polyethylene oxide segments and polypropylene oxide segments, and the CAS number is 697765-47-2. Among them, the molar ratio of polyethylene oxide segments in Maxemul 7101 to the total of polyethylene oxide segments and polypropylene oxide segments is about 57.5%, and the molar ratio of polyethylene oxide segments in Maxemul 7102 to the total of polyethylene oxide segments and polypropylene oxide segments is about 55%.
[0036] Preferably, the triblock emulsifier is at least one of Pluronic PE 9400 and Pluronic PE 6800 of BASF. Pluronic PE 9400 and Pluronic PE 6800 of BASF are triblock emulsifiers of polyethylene oxide segments, polypropylene oxide segments and polyethylene oxide segments, and the CAS number is 9003-11-6. Among them, the molar ratio of polyethylene oxide segments in Pluronic PE 9400 to the total of polyethylene oxide segments and polypropylene oxide segments is about 40%, and the molar ratio of polyethylene oxide segments in Pluronic PE 6800 to the total of polyethylene oxide segments and polypropylene oxide segments is about 80%.
[0037] In the present invention, the molar ratio of the polyethylene oxide segment to the total of the polyethylene oxide segment and the polyethylene oxide segment in the nonionic emulsifier can be measured and calculated by nuclear magnetic hydrogen spectrum HNMR (deuterated chloroform as solvent, nuclear magnetic spectrometer 300-600MHz). For example, in the nuclear magnetic hydrogen spectrum HNMR of Pluronic PE 9400, 1.1-1.2 is the methyl peak on the polyethylene oxide group, and the integral here is 1.8; and 3.2-3.8 is the peak on the polyethylene oxide -CH2CH2- and the polyethylene oxide -CHCH2-, and the integral here is 3.4, then from 3y / [4(x+z)+3y]=1.8 / 3.4, (x+z) / y=2 / 3 is obtained, and the molar ratio of the polyethylene oxide segment to the total of the polyethylene oxide segment and the polyethylene oxide segment (x+z) / (x+y+z) is about 40%.
[0038] Further, the solid content of the aqueous polyol dispersion is 40-70wt%. In order to facilitate the design of the aqueous polyol dispersion to a suitable construction viscosity, the amount of water added makes the solid content of the aqueous polyol dispersion 40-70wt%. If the amount of water added is too little, the viscosity of the aqueous polyol dispersion will be too large, which is inconvenient to use. If the amount of water added is too much, the effective ingredient of the aqueous polyol dispersion will be too low, which will cause the coating film to dry slowly when used for water-based coatings.
[0039] Furthermore, the weight (addition amount) of the water is 40-400% of the weight (addition amount) of the polycarbonate diol. By adding an appropriate amount of water, the polycarbonate diol can be externally emulsified in combination with the nonionic emulsifier, and the aqueous polyol dispersion can be adjusted to a suitable viscosity.
[0040] Furthermore, the aqueous polyol dispersion also includes a cosolvent. The stability of the aqueous polyol dispersion can be increased by adding a cosolvent.
[0041] Furthermore, the weight (addition amount) of the co-solvent is 0-10% of the weight (addition amount) of the polycarbonate diol. If the addition amount of the co-solvent is too much, the cost will increase.
[0042] Furthermore, the cosolvent is at least one of alcohol ether, alcohol, ether, ester, and ketone cosolvents. Preferably, the cosolvent is an alcohol ether solvent. Alcohol ether cosolvents also have a good film-forming effect, which facilitates the water-based polyol dispersion to form a coating film in a water-based two-component soft-touch coating.
[0043] The present invention also provides a method for preparing any of the above-mentioned aqueous polyol dispersions, comprising the following steps: mixing the polycarbonate diol and the nonionic emulsifier, adding water for emulsification, and obtaining the aqueous polyol dispersion.
[0044] The water-based polyol dispersion is obtained by mixing the polycarbonate diol and the nonionic emulsifier and then adding the mixture into water for external emulsification.
[0045] The present invention also provides an application of an aqueous polyol dispersion in an aqueous two-component soft-touch paint. The aqueous polyol dispersion of the present invention is applied to the aqueous two-component soft-touch paint to form a coating film having excellent wear resistance and softness.
[0046] As a preferred solution, the water-based two-component matte soft-touch coating comprises a component A and a component B, wherein the component A comprises any of the above-mentioned water-based polyol dispersions; and the component B comprises a water-based isocyanate curing agent.
[0047] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0048] The aqueous polyol dispersion of the present invention can be obtained by selecting the polycarbonate diol, nonionic emulsifier, cosolvent and water. The present invention limits the ratio of the groups in the polycarbonate diol and the amount of the substances thereof, limits the structure of the nonionic emulsifier and the molar ratio of the polyethylene oxide segment in the nonionic emulsifier to the total of the polyethylene oxide segment and the polypropylene oxide segment, so that the aqueous polyol dispersion has excellent wear resistance and soft feel, and good stability. DETAILED DESCRIPTION
[0049] The present invention is further described below in conjunction with examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets. Any non-substantial changes and substitutions made by those skilled in the art on the basis of the present invention belong to the scope of protection claimed by the present invention.
[0050] In the following examples and comparative examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.
[0051] Example 1
[0052] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0053] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segment in the emulsifier to the total of the polyoxyethylene segment and the polyoxypropylene segment is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0054] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0055] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 4.0 g of Pluronic PE 9400 emulsifier (purchased from BASF, the non-ionic emulsifier is a triblock copolymer consisting of polyethylene oxide, polypropylene oxide and polyethylene oxide parts) were stirred at room temperature for 1 hour, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion for about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0056] Example 2
[0057] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0058] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, cosolvent, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0059] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0060] 46.0 g of polycarbonate diol with a molecular weight of 2000 (Ube ETERNACOLL PH-200, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50), 4.0 g of Pluronic PE 9400 emulsifier, and 5.0 g of propylene glycol butyl ether were stirred at room temperature for 1 h, and then 45.0 g of deionized water was slowly dripped into it under high-speed dispersion for about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0061] Example 3
[0062] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0063] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units represented by formula (1), and repeating units represented by formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. For details, please refer to the following preparation method and Table 1.
[0064] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0065] 46.0g of polycarbonate diol (a polycarbonate diol with 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, synthesized by a method similar to Example 2 of patent CN102317334A, only 1,4-butanediol is replaced by 1,5-pentanediol in equal moles, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 75:25), 4.0g of Pluronic PE 9400 emulsifier, stirred at room temperature for 1h, then 50.0g of deionized water was slowly added under high-speed dispersion, and the dripping was completed in about 2h, to obtain a milky white aqueous polyol dispersion with a solid content of 50.0wt%. 4.0g of Pluronic PE 9400 emulsifier, stirred at room temperature for 1h, then 50.0g of deionized water was slowly added under high-speed dispersion, and the dripping was completed in about 2h, to obtain a milky white aqueous polyol dispersion with a solid content of 50.0wt%.
[0066] Example 4
[0067] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0068] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segment in the emulsifier to the total of the polyoxyethylene segment and the polyoxypropylene segment is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0069] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0070] 46.0 g of polycarbonate diol (synthesized according to the method of Example 2 of patent CN102317334A, with a hydroxyl value of 57.3 mg KOH / g, wherein the molar ratio of 1,4-butanediol to 1,6-hexanediol is about 75:25) and 4.0 g of Pluronic PE9400 emulsifier were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion for about 2 h to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0071] Example 5
[0072] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0073] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, cosolvent, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (4); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segment in the emulsifier to the total of the polyoxyethylene segment and the polyoxypropylene segment is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0074] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0075] 46.0 g of polycarbonate diol with a molecular weight of 900 (Ube ETERNACOLL UM-90 (1 / 3), using 1,4-cyclohexanedimethanol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,4-cyclohexanedimethanol to 1,6-hexanediol is about 25:75), 4.0 g of Pluronic PE 9400 emulsifier, and 5.0 g of propylene glycol butyl ether were stirred at room temperature for 1 h, and then 45.0 g of deionized water was slowly dripped into it under high-speed dispersion for about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0076] Example 6
[0077] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0078] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (3); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segment in the emulsifier to the total of the polyoxyethylene segment and the polyoxypropylene segment is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0079] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0080] The following method was used to synthesize polycaprolactone-modified polycarbonate diol: 75.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL UH-100, using 1,6-hexanediol as a polymerization monomer), 25.0 g of ε-caprolactone, and 0.05 g of stannous octoate were heated to 200° C. and reacted for 8 hours to obtain polycaprolactone-modified polycarbonate diol with a molecular weight of 1330, wherein the molar ratio of ε-caprolactone to 1,6-hexanediol was approximately 30:70.
[0081] 46.0 g of the above-synthesized polycaprolactone-modified polycarbonate diol and 4.0 g of Pluronic PE 9400 emulsifier were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dropped into it under high-speed dispersion for about 2 h to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0082] Example 7
[0083] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0084] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (3); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segment in the emulsifier to the total of the polyoxyethylene segment and the polyoxypropylene segment is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0085] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0086] The polyvalerolactone-modified polycarbonate diol was synthesized by the following method: 75.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL UH-100, using 1,6-hexanediol as a polymerization monomer), 25.0 g of δ-valerolactone, and 0.05 g of stannous octoate were heated to 200° C. and reacted for 8 hours to obtain a polyvalerolactone-modified polycarbonate diol with a molecular weight of 1330, wherein the molar ratio of δ-valerolactone to 1,6-hexanediol was approximately 32:68.
[0087] 46.0 g of the above-synthesized polyvalerolactone-modified polycarbonate diol and 4.0 g of Pluronic PE 9400 emulsifier were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dropped into it under high-speed dispersion for about 2 h to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0088] Example 8
[0089] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0090] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), repeating units shown in formula (2), and repeating units shown in formula (3); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0091] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0092] The polycaprolactone-modified polycarbonate diol was synthesized by the following method: 75.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol was approximately 50:50), 25.0 g of ε-caprolactone, and 0.05 g of stannous octoate were heated to 200° C. and reacted for 8 hours to obtain a polycaprolactone-modified polycarbonate diol with a molecular weight of 1330, wherein the molar ratio of ε-caprolactone to 1,5-pentanediol to 1,6-hexanediol was approximately 28:36:36.
[0093] 46.0 g of the above-synthesized polycaprolactone-modified polycarbonate diol and 4.0 g of Pluronic PE 9400 emulsifier were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dropped into it under high-speed dispersion for about 2 h to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0094] Example 9
[0095] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0096] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 80%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0097] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0098] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 4.0 g of Pluronic PE 6800 emulsifier (purchased from BASF, the non-ionic emulsifier is a triblock copolymer consisting of polyethylene oxide, polypropylene oxide and polyethylene oxide parts) were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion. The dripping lasted for about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0099] Example 10
[0100] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0101] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (2); the nonionic emulsifier is a diblock emulsifier, the molar ratio of the polyoxyethylene segment in the emulsifier to the total of the polyoxyethylene segment and the polyoxypropylene segment is 55%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0102] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0103] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 4.0 g of Maxemul 7102 emulsifier (purchased from Croda, the emulsifier is a diblock copolymer composed of polyethylene oxide and polypropylene oxide parts) were stirred at room temperature for 1 hour, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion. The dripping lasted for about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0104] Embodiment 11
[0105] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0106] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), repeating units shown in formula (2), repeating units shown in formula (3), and repeating units shown in formula (4); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segment in the emulsifier to the total of the polyoxyethylene segment and the polyoxypropylene segment is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. Please refer to the following preparation method and Table 1 for details.
[0107] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0108] The following method was used to synthesize polycaprolactone-modified polycarbonate diol: 90.0 g of polycarbonate diol with a molecular weight of 1000 (polycarbonate diol with 1,5-pentanediol, 1,4-cyclohexanedimethanol and 1,6-hexanediol as polymerization monomers, synthesized according to a method similar to Example 2 of Patent CN102317334A, and the molar ratio of 1,5-pentanediol to 1,6-hexanediol was changed from 75:25 to 1,5 -pentanediol and 1,4-cyclohexanedimethanol and 1,6-hexanediol in a molar ratio of 25:25:50), 10.0g ε-caprolactone, 0.05g stannous octoate, heated to 200°C for reaction for 8h to obtain a polycaprolactone-modified polycarbonate diol, wherein the molar ratio of ε-caprolactone to 1,5-pentanediol to 1,4-cyclohexanedimethanol to 1,6-hexanediol is approximately 11:22:22:45.
[0109] 46.0 g of the above-synthesized polycaprolactone-modified polycarbonate diol and 4.0 g of Pluronic PE 9400 emulsifier were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dropped into it under high-speed dispersion for about 2 h to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0110] Example 12
[0111] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0112] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 2.2%. Please refer to the following preparation method and Table 1 for details.
[0113] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0114] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 1.0 g of Pluronic PE 9400 emulsifier were stirred at room temperature for 1 h, and then 47.0 g of deionized water was slowly dripped into it under high-speed dispersion for about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0115] Embodiment 13
[0116] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0117] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 19.1%. Please refer to the following preparation method and Table 1 for details.
[0118] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0119] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 8.8 g of Pluronic PE 9400 emulsifier were stirred at room temperature for 1 hour, and then 54.8 g of deionized water was slowly dripped into it under high-speed dispersion for about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0120] Comparative Example 1
[0121] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0122] The aqueous polyol dispersion of this comparative example comprises polycarbonate diol, nonionic emulsifier and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising terminal hydroxyl groups and repeating units represented by formula (1); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. For details, please refer to the following preparation method and Table 1.
[0123] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0124] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL UH-100, using 1,6-hexanediol as a polymerization monomer) and 4.0 g of Pluronic PE 9400 emulsifier were stirred at room temperature for 1 hour, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion for about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0125] Comparative Example 2
[0126] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0127] The aqueous polyol dispersion of this comparative example comprises polycarbonate diol, nonionic emulsifier, cosolvent and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising terminal hydroxyl groups, repeating units represented by formula (1) and repeating units represented by formula (4); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. For details, please refer to the following preparation method and Table 1.
[0128] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0129] 46.0 g of polycarbonate diol with a molecular weight of 900 (Ube ETERNACOLL UM-90 (3 / 1), using 1,4-cyclohexanedimethanol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,4-cyclohexanedimethanol to 1,6-hexanediol is about 75:25), 4.0 g of Pluronic PE 9400 emulsifier, and 5.0 g of propylene glycol butyl ether were stirred at room temperature for 1 h, and then 45.0 g of deionized water was slowly dripped into it under high-speed dispersion. The dripping took about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0130] Comparative Example 3
[0131] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0132] The aqueous polyol dispersion of this comparative example comprises polycarbonate diol, nonionic emulsifier, cosolvent and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising terminal hydroxyl groups, repeating units represented by formula (1) and repeating units represented by formula (4); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. For details, please refer to the following preparation method and Table 1.
[0133] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0134] 46.0 g of polycarbonate diol with a molecular weight of 900 (Ube ETERNACOLL UM-90 (1 / 1), using 1,4-cyclohexanedimethanol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,4-cyclohexanedimethanol to 1,6-hexanediol is about 50:50), 4.0 g of Pluronic PE 9400 emulsifier, and 5.0 g of propylene glycol butyl ether were stirred at room temperature for 1 h, and then 45.0 g of deionized water was slowly dripped into it under high-speed dispersion for about 2 hours to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0135] Comparative Example 4
[0136] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0137] The aqueous polyol dispersion of this comparative example comprises polycarbonate diol, nonionic emulsifier and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising terminal hydroxyl groups, repeating units represented by formula (1) and repeating units represented by formula (3); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. For details, please refer to the following preparation method and Table 1.
[0138] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0139] The following method was used to synthesize polycaprolactone-modified polycarbonate diol: 60.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL UH-100, using 1,6-hexanediol as a polymerization monomer), 40.0 g of ε-caprolactone, and 0.05 g of stannous octoate were heated to 200° C. and reacted for 8 hours to obtain polycaprolactone-modified polycarbonate diol, wherein the molar ratio of ε-caprolactone to 1,6-hexanediol was approximately 46:54.
[0140] 46.0 g of the above-synthesized polycaprolactone-modified polycarbonate diol and 4.0 g of Pluronic PE 9400 emulsifier were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dropped into it under high-speed dispersion for about 2 h to obtain a milky white aqueous polyol dispersion with a solid content of 50.0 wt%.
[0141] Comparative Example 5
[0142] This embodiment provides an aqueous polyol dispersion and a preparation method thereof.
[0143] The aqueous polyol dispersion of this embodiment includes polycarbonate diol, nonionic emulsifier, and water. The polycarbonate diol of this embodiment is a polycarbonate diol containing terminal hydroxyl groups, repeating units shown in formula (1), and repeating units shown in formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 40%, and the weight ratio of the emulsifier to the polycarbonate diol is 0.9%. Please refer to the following preparation method and Table 1 for details.
[0144] The preparation method of the aqueous polyol dispersion of the present embodiment comprises the following steps:
[0145] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 0.4 g of Pluronic PE 9400 emulsifier were stirred at room temperature for 1 hour, and then 46.4 g of deionized water was slowly dripped into it under high-speed dispersion. After about 2 hours of dripping, a stable emulsion could not be obtained, and the mixture was allowed to stand overnight before stratification.
[0146] Comparative Example 6
[0147] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0148] The aqueous polyol dispersion of this comparative example comprises polycarbonate diol, nonionic emulsifier and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising terminal hydroxyl groups, repeating units represented by formula (1) and repeating units represented by formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the polyoxyethylene segments in the emulsifier to the total of the polyoxyethylene segments and the polyoxypropylene segments is 20%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. For details, please refer to the following preparation method and Table 1.
[0149] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0150] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50), 4.0 g of Pluronic PE 9200 emulsifier (purchased from BASF, the nonionic emulsifier is a triblock copolymer consisting of polyethylene oxide, polypropylene oxide and polyethylene oxide parts) were stirred at room temperature for 1 hour, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion. The dripping was completed in about 2 hours, but a stable emulsion could not be obtained. After standing overnight, stratification was achieved.
[0151] Comparative Example 7
[0152] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0153] The aqueous polyol dispersion of this comparative example comprises polycarbonate diol, nonionic emulsifier and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising terminal hydroxyl groups, repeating units represented by formula (1) and repeating units represented by formula (2); the nonionic emulsifier is a triblock emulsifier, the molar ratio of the emulsifier polyoxyethylene segments to the total of the polyoxyethylene segments and the polyoxypropylene segments is 90%, and the weight ratio of the emulsifier to the polycarbonate diol is 8.7%. For details, please refer to the following preparation method and Table 1.
[0154] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0155] A triblock copolymer consisting of polyethylene oxide, polyethylene oxide and polyethylene oxide was synthesized by the following method, wherein the polyethylene oxide segment accounted for 90% of the total polyethylene oxide segment and polyethylene oxide segment in molar proportion: 20.0 g of polypropylene glycol with a molecular weight of 200 and 0.63 g of sodium methoxide were introduced into a pressure reactor, and nitrogen was filled at room temperature and then evacuated. The mixture was then heated to 115° C. 180.0 g of ethylene oxide was added at 115° C. for about 4 h. After continuing the reaction for 2 h, the mixture was cooled to <90° C. to obtain a triblock copolymer with a hydroxyl value of 56 mgKOH / g.
[0156] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 4.0 g of the above-synthesized triblock emulsifier were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion. After about 2 hours of dripping, a stable emulsion could not be obtained, and it was separated after standing overnight.
[0157] Comparative Example 8
[0158] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0159] The aqueous polyol dispersion of this comparative example comprises polycarbonate diol, emulsifier and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising terminal hydroxyl groups, repeating units represented by formula (1) and repeating units represented by formula (2); the emulsifier is a non-blocking emulsifier, and the specific preparation method is as follows.
[0160] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0161] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50), 4.0 g of mixed polyether (containing 40 wt% of polyethylene glycol 4000 and 60 wt% of polypropylene glycol 4000, non-blocked, only physically blended) were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion. The dripping was completed in about 2 h, and a stable emulsion could not be obtained. After standing overnight, stratification was achieved.
[0162] Comparative Example 9
[0163] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0164] The aqueous polyol dispersion of this comparative example comprises a polycarbonate diol, an emulsifier, and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising a terminal hydroxyl group, a repeating unit represented by formula (1), and a repeating unit represented by formula (2); the emulsifier is an emulsifier containing only polyethylene oxide, and the specific preparation method is described below.
[0165] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0166] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 4.0 g of polyethylene glycol 4000 were stirred at room temperature for 1 hour, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion. After about 2 hours of dripping, a stable emulsion could not be obtained, and the emulsion was separated after standing overnight.
[0167] Comparative Example 10
[0168] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0169] The aqueous polyol dispersion of this comparative example comprises polycarbonate diol, emulsifier and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising terminal hydroxyl groups, repeating units represented by formula (1) and repeating units represented by formula (2); the emulsifier is a fatty alcohol polyoxyethylene ether emulsifier containing only polyoxyethylene. For details, please refer to the following preparation method.
[0170] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0171] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 4.0 g of fatty alcohol polyoxyethylene ether AEO-9 (without polyoxypropylene segment) were stirred at room temperature for 1 h, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion. The dripping was completed in about 2 hours, but a stable emulsion could not be obtained. After standing overnight, stratification occurred.
[0172] Comparative Example 11
[0173] This comparative example provides an aqueous polyol dispersion and a preparation method thereof.
[0174] The aqueous polyol dispersion of this comparative example comprises polycarbonate diol, emulsifier and water. The polycarbonate diol of this comparative example is a polycarbonate diol comprising terminal hydroxyl groups, repeating units represented by formula (1) and repeating units represented by formula (2); the emulsifier is an anionic emulsifier, and the specific preparation method is as follows.
[0175] The preparation method of the aqueous polyol dispersion of this comparative example comprises the following steps:
[0176] 46.0 g of polycarbonate diol with a molecular weight of 1000 (Ube ETERNACOLL PH-100, using 1,5-pentanediol and 1,6-hexanediol as polymerization monomers, wherein the molar ratio of 1,5-pentanediol to 1,6-hexanediol is about 50:50) and 4.0 g of sodium dodecylbenzene sulfonate emulsifier were stirred at room temperature for 1 hour, and then 50.0 g of deionized water was slowly dripped into it under high-speed dispersion. After about 2 hours of dripping, a stable aqueous dispersion could not be obtained and obvious stratification occurred.
[0177] Embodiment 14
[0178] This comparative example provides an application of an aqueous polyol dispersion in an aqueous two-component soft-touch coating.
[0179] The water-based two-component soft-touch paint of this embodiment includes component A and component B. Among them:
[0180] Component A includes the following components calculated by weight: 64 parts of any aqueous polyol dispersion of Examples 1-13, 21 parts of water, 0.7 parts of defoaming agent, 0.5 parts of dispersant, 6.5 parts of matting powder, 0.5 parts of wetting agent, 5.4 parts of film-forming aid, 1 part of aqueous organotin catalyst, and 0.4 parts of thickener.
[0181] Component B is a water-based isocyanate curing agent.
[0182] The ratio of the molar amount of -OH (hydroxyl group) in the aqueous polyol dispersion in component A to the molar amount of -NCO (isocyanate group) in the aqueous isocyanate curing agent is 1.5.
[0183] Table 1 Parameters of polycarbonate diol and nonionic emulsifier of Examples 1-13 and Comparative Examples 1-7
[0184]
[0185]
[0186] In Table 1, n1, n2, n3, and n4 respectively represent the molar amount of the repeating unit represented by formula (1), the molar amount of the repeating unit represented by formula (2), the molar amount of the repeating unit represented by formula (3), and the molar amount of the repeating unit represented by formula (4) in the polycarbonate diol; n5 and n6 respectively represent the molar amount of the polyoxyethylene segment and the molar amount of the polyoxypropylene segment in the nonionic emulsifier; is the weight ratio of the nonionic emulsifier to the polycarbonate diol in the aqueous polyol dispersion (m2 is the weight of the nonionic emulsifier, m1 is the weight of the polycarbonate diol).
[0187] Performance Testing
[0188] Since Comparative Examples 5-11 cannot form a stable aqueous polyol dispersion, this specification only tests the performance of the aqueous polyol dispersions provided by Examples 1-13 and Comparative Examples 1-4. The process is as follows:
[0189] The waterborne polyol dispersions and waterborne isocyanate curing agents provided in Examples 1-13 and Comparative Examples 1-4 were respectively formulated into AB two-component waterborne two-component matte soft-touch coatings 1-13 (corresponding to Examples 1-13) and waterborne two-component matte soft-touch coatings 14-17 (corresponding to Comparative Examples 1-4), and the relevant properties of coatings 1-17 were tested. The formula of component A in each coating is shown in Table 2, and component B is a commercial waterborne anionic isocyanate curing agent: OS-9016 (Guanzhi New Materials, NCO content 16.3wt%, solid content 80wt%). The molar ratio of the waterborne polyol dispersion and the waterborne isocyanate curing agent component is calculated according to NCO / OH=1.5 to obtain the amount of each component.
[0190] Table 2 Formula of component A in coating 1-17 (parts)
[0191]
[0192]
[0193] After mixing the A component and B component of coating 1-17, add water to adjust to the appropriate viscosity (apply 4 cups of viscosity for 20-30 seconds) and spray them. The construction substrate is a black PC substrate plastic plate, the dry film thickness is 20±3um, and the drying condition is 70℃ for 4h and then placed at room temperature overnight. Then the coating film is tested for the following properties:
[0194] Gloss test: The test was carried out in accordance with GB 1743-1979 (1989), and the 60° gloss was recorded.
[0195] Matt powder distribution effect test: observe whether the coating surface is uneven.
[0196] Soft touch test: Score the soft touch of the coating film on a scale of 1-10, with 10 being the best and 1 being the worst.
[0197] RCA wear test: Tested in accordance with standard ASTM F2357-04, load 175g.
[0198] The test results are shown in Table 3:
[0199] Table 3 Performance test results of coatings 1-17
[0200]
[0201] From the above results, it can be seen that the coatings formed by the water-based two-component soft-touch coatings 1-13 prepared by the water-based polyol dispersions of Examples 1-13 of the present invention have good matte powder arrangement effect, good softness, and excellent RCA wear resistance. However, coating 14 uses the water-based polyol dispersion of Comparative Example 1, and its polycarbonate diol contains only terminal hydroxyl groups and repeating units represented by formula (1), that is, the content of 1,6-hexanediol units is too high, making the structure of the polycarbonate diol too regular, with strong crystallinity, and improving cohesion, resulting in the coating formed by the water-based two-component soft-touch coating 12 prepared by the water-based polyol dispersion of Comparative Example 1 having a lower softness. Coating 15 uses the aqueous polyol dispersion of Comparative Example 2, and coating 16 uses the aqueous polyol dispersion of Comparative Example 3. However, since the content of the repeating unit represented by formula (4) in the polycarbonate diol of the aqueous polyol dispersions of Comparative Example 2 and Comparative Example 3 is too high, that is, the content of 1,4-cyclohexanedimethanol units is too high, the softness of the coating film formed by the aqueous two-component soft-touch coating 13 and coating 16 prepared by the aqueous polyol dispersions of Comparative Example 2 and Comparative Example 3 with excessive rigid repeating units represented by formula (4) is deteriorated. Coating 17 uses the aqueous polyol dispersion of Comparative Example 4, and the content of the repeating unit represented by formula (3) in the polycarbonate diol is too high, that is, the content of the polycaprolactone segment is too high, resulting in the RCA wear resistance of the coating film formed by the aqueous two-component soft-touch coating 17 prepared by the aqueous polyol dispersion of Comparative Example 4 being deteriorated.
[0202] The embodiments 1-13 of the present invention use a nonionic emulsifier with a specific structure and a specific molar ratio of polyethylene oxide segments to the total of polyethylene oxide segments and polypropylene oxide segments, and the nonionic emulsifier has a specific weight ratio with the polycarbonate diol, so that the water-based polyol dispersions of the embodiments 1-13 have good stability, while the emulsifier with the specific structure and the specific molar ratio of polyethylene oxide segments to the total of polyethylene oxide segments and polypropylene oxide segments, and the water-based polyol dispersions without the specific weight ratio of the nonionic emulsifier to the polycarbonate diol are prone to stratification. For example, the water-based polyol dispersion of Comparative Example 5, although using a nonionic emulsifier, the weight ratio of the emulsifier to the polycarbonate diol is 0.9%, which is less than the limited range of the present invention, and a stable water-based polyol dispersion cannot be obtained, and stratification is prone to occur after standing. For example, although the aqueous polyol dispersion of Comparative Example 6 uses a nonionic emulsifier, the molar ratio of the polyethylene oxide segment of the nonionic emulsifier used is 20% of the total of the polyethylene oxide segment and the polypropylene oxide segment, which is less than the limited range of the present invention, and a stable aqueous polyol dispersion cannot be obtained, and stratification is easy to occur after standing. The aqueous polyol dispersion of Comparative Example 7 uses a nonionic emulsifier in which the molar ratio of the polyethylene oxide segment of the nonionic emulsifier used is 90% of the total of the polyethylene oxide segment and the polypropylene oxide segment, which is greater than the limited range of the present invention, and a stable aqueous polyol dispersion cannot be obtained, and stratification is easy to occur after standing. The aqueous polyol dispersion of Comparative Example 8 uses physically blended polyethylene glycol and polypropylene glycol as emulsifiers instead of block emulsifiers, and a stable aqueous polyol dispersion cannot be obtained, and stratification is easy to occur after standing. The aqueous polyol dispersion of Comparative Example 9 uses polyethylene glycol 4000 containing only polyoxyethylene as an emulsifier; the aqueous polyol dispersion of Comparative Example 10 uses fatty alcohol polyoxyethylene ether AEO-9 containing only polyoxyethylene as an emulsifier. Both emulsifiers are diblock emulsifiers or triblock emulsifiers not of the present invention. Comparative Examples 9 and 10 also cannot obtain stable aqueous polyol dispersions, and are prone to stratification after standing. The aqueous polyol dispersion of Comparative Example 11 uses an anionic emulsifier such as sodium dodecylbenzene sulfonate, and cannot obtain a stable aqueous dispersion.
[0203] Compared with the prior art, the water-based polyol dispersion of the present invention can obtain a water-based soft-touch polyol by selecting the polycarbonate diol, nonionic emulsifier, cosolvent and water. Among them, the present invention limits the ratio of the groups in the polycarbonate diol and the amount of the substance thereof, and limits the structure of the nonionic emulsifier and the molar ratio of the polyoxyethylene segment in the nonionic emulsifier to the total of the polyoxyethylene segment and the polyoxypropylene segment, so that the water-based soft-touch polyol has excellent wear resistance and soft feel, and good stability. The water-based polyol dispersion of the present invention is applied to a water-based two-component soft-touch coating to form a coating film having excellent wear resistance and soft feel.
[0204] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.
Claims
1. An aqueous polyol dispersion, characterized in that: Including polycarbonate diol, nonionic emulsifier, water; The polycarbonate diol is at least one polycarbonate diol comprising (a), (b), and (c), wherein: (a) is a terminal hydroxyl group; (b) is a repeating unit represented by formula (1); (c) is at least one of the repeating unit represented by formula (2), the repeating unit represented by formula (3), and the repeating unit represented by formula (4); In formula (2), n is 4 or 5; In formula (3), m=4 or 5; In the polycarbonate diol, n1 represents the molar amount of the repeating unit represented by formula (1); n2 represents the molar amount of the repeating unit represented by formula (2); n3 represents the molar amount of the repeating unit represented by formula (3); n4 represents the molar amount of the repeating unit represented by formula (4); The weight of the nonionic emulsifier is 2-20% of the weight of the polycarbonate diol; the nonionic emulsifier is a diblock emulsifier and / or a triblock emulsifier; wherein: The diblock emulsifier contains a segment represented by formula (5); In formula (5), x and y are integers of 1-100, and x / (x+y)=35-85%; The triblock emulsifier contains a segment represented by formula (6); In formula (6), x, y, and z are integers of 1-100, and (x+z) / (x+y+z)=35-85%.
2. The aqueous polyol dispersion according to claim 1, characterized in that: The number average molecular weight of the polycarbonate diol is 300-10000.
3. The aqueous polyol dispersion according to claim 1, characterized in that: The solid content of the aqueous polyol dispersion is 40-70 wt %.
4. The aqueous polyol dispersion according to claim 1, characterized in that: The weight of the water is 40-400% of the weight of the polycarbonate diol.
5. The aqueous polyol dispersion according to claim 1, characterized in that: Cosolvents are also included.
6. The aqueous polyol dispersion according to claim 5, characterized in that: The weight of the co-solvent is 0-10% of the weight of the polycarbonate diol.
7. The aqueous polyol dispersion according to claim 5, characterized in that: The co-solvent is at least one of alcohol ether, alcohol, ether, ester and ketone co-solvents.
8. A method for preparing the aqueous polyol dispersion according to any one of claims 1 to 7, comprising the following steps: The polycarbonate diol and the nonionic emulsifier are mixed, and water is added for emulsification to obtain the aqueous polyol dispersion.
9. Use of the aqueous polyol dispersion according to any one of claims 1 to 7 in an aqueous two-component soft-touch coating.
Citation Information
Patent Citations
Two-pack polyurethane paint for backing film
CN102317334A
Water-based polyurethane dispersion
CN107011495A
Two-component system for elastic coatings
CN111094373A
Hydroxylated polyurethane water dispersoid for waterborne soft-feel coating and preparation method thereof
CN102002166A
Active energy ray curable aqueous emulsions
CN104284948A