Preparation and application of an intumescent flame retardant powder coating
By modifying the combination of aluminum hydroxide and POSS-based epoxy curing agent, the thickness and economic problems of ultra-thin steel structure expansion fire-retardant coating are solved, and high-performance ultra-thin coating is achieved, with excellent flame retardant, mechanical properties and Low temperature curing characteristics.
Patent Information
- Application Number
- CN202410246943.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-03-05
AI Technical Summary
The existing ultra-thin steel structure expansion fire-retardant coating has thick coating thickness, poor economy, poor adhesion and chemical resistance, and it is difficult to obtain excellent flame retardant and mechanical properties in thin coatings.
Modified aluminum hydroxide with cage-shaped polysilsesquioxane containing silanol groups as composite flame retardant, combining POSS-based epoxy curing agent and epoxy resin to form high compatibility and dispersion Coating, the cross-linking density and POSS structural content of the coating are enhanced by medium and low temperature curing agents.
A ultra-thin coating with a thickness of 0.3-0.7mm is obtained, with excellent fire and flame retardant properties, mechanical impact resistance, chemical resistance and adhesion. The coating can achieve low temperature curing, save energy, and be suitable for thermal sensitivity Substrate.
Smart Images

Figure BDA0004726285970000121 
Figure BDA0004726285970000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of intumescent flame-retardant powder coatings, and in particular to an ultra-thin epoxy resin-based intumescent flame-retardant powder coating. Background Art
[0002] Flame retardant coating is a special functional coating. When applied to the surface of an object, it can prevent fire, stop the spread of fire, isolate the source of fire, prolong the ignition time of the substrate, or increase the insulation performance to delay the structural damage.
[0003] Intumescent flame retardant coatings are the most widely used type of flame retardant coatings in actual production. Intumescent flame retardant coatings are mainly composed of base materials, dehydration catalysts, carbonizing agents, foaming agents, flame retardants, pigments, fillers, additives and dispersion media. Steel structure fire retardant coatings are the main application of intumescent fire retardant coatings. Fire retardant coatings with a coating thickness of less than 3mm and a fire resistance limit of 0.5-1h are called ultra-thin steel structure intumescent fire retardant coatings.
[0004] Since powder coatings have no solvent volatilization, reduce air pollution, and do not have the fire hazard caused by organic solvents, intumescent flame retardant powder coatings have been rapidly developed. At present, the fire resistance of ultra-thin fire-retardant powder coatings for steel structures is basically 2mm in coating thickness and about 60min in fire resistance time. The coating thickness is still too thick, which is poor in economic efficiency, and the fire retardant performance needs to be further improved.
[0005] The Chinese invention patent with application number 200510126070.2 discloses an intumescent flame-retardant epoxy resin powder coating suitable for steel structure and a preparation method thereof, which obtains an intumescent flame-retardant coating with diisooctyl phosphate modified epoxy resin as film-forming resin and dicyandiamide as curing agent system. However, the spraying thickness of the coating is 2.5-3 cm, the economic efficiency is poor, and the construction is relatively complicated. Moreover, the adhesion of the coating obtained by the coating is level 1, and the chemical resistance test result of the coating is not ideal, and still cannot meet certain specific application requirements.
[0006] The Chinese invention patent with application number 200710017706.9 discloses a fire-retardant powder coating for ultra-thin steel structures and a preparation method thereof, wherein tetrabromobisphenol A epoxy resin is first prepared, and then the fire-retardant powder coating is prepared with raw materials such as an intumescent flame retardant. However, the patent document does not record the fire-retardant properties of the obtained coating.
[0007] Cage-type polysilsesquioxane (POSS) is a high-performance organic-inorganic hybrid material, which uses POSS as an inorganic component, and the organic substituents connected to the silicon atoms of POSS are organic components. Therefore, the inorganic phase and the organic phase are combined by strong chemical bonds to overcome the problems of agglomeration of inorganic particles and weak bonding force between the organic and inorganic phase interfaces. Therefore, POSS is a hybrid material with excellent performance, which is easy to be compounded with a polymer matrix by copolymerization, grafting or blending to improve the heat resistance, flame retardancy, toughening and other properties of the polymer matrix.
[0008] Application number is that the Chinese invention patent of 200910054551.5 discloses a kind of preparation method based on silsesquioxane modified ultra-thin fireproof coating polymer matrix, it is that POSS is introduced in the coating matrix resin with physical or chemical method, and the addition of POSS is 0.1-20wt%.But any performance of the obtained coating is not recorded in this patent document, such as heat resistance or flame retardant property.But in fact, the compatibility of POSS and coating matrix resin is poor, and the amount of adding POSS is too much, and the obtained coating storage stability is poor, and the obtained coating forms defect easily.And the amount of adding POSS is few, then the application performance of coating is improved comparatively limited.
[0009] The Chinese invention patent with application number 201010179346.4 discloses a POSS / epoxy nano hybrid material and its preparation method and application, which discloses that the obtained nano hybrid material has excellent heat resistance, aging resistance, transparency and other properties, but does not disclose the specific application of the nano hybrid material, and does not pay attention to the flame retardant property of the material. In addition, a high-content of POSS with multiple epoxy groups is added in the specific embodiment of the application, and the POSS with multiple epoxy groups can form a large amount of cross-linked structures during the curing process, resulting in poor adhesion and construction performance of the coating, and is not suitable for the application of coating.
[0010] Aluminum hydroxide is a common flame retardant. Its flame retardant principle is that aluminum hydroxide releases crystal water when it is decomposed by heat. This process is a strong endothermic reaction, absorbing a large amount of heat, which can cool the polymer. At the same time, the water vapor produced by the reaction can dilute the combustible gas and inhibit the spread of combustion. The newly formed refractory metal oxide aluminum oxide has high activity. It will catalyze the thermal oxygen cross-linking reaction of the polymer and form a carbonized film on the surface of the polymer. The carbonized film will weaken the heat and mass transfer effects during combustion, thereby playing a flame retardant role. At the same time, aluminum oxide can also absorb smoke particles and play a smoke suppression role.
[0011] The Chinese invention patent with application number 201910442743.7 discloses a fire-retardant powder coating, which uses aluminum hydroxide as the main flame-retardant filler of polyester resin-based powder coating. The addition of aluminum hydroxide to the powder coating improves the fire-retardant performance of the coating. However, the particle size of the flame-retardant filler aluminum hydroxide must be controlled below 3000 mesh, otherwise it will seriously affect the leveling effect of the powder coating.
[0012] The Chinese invention patent with application number 201510232259.3 discloses a composite flame retardant material of POSS and aluminum hydroxide, and discloses that the flame retardant effect of the composite flame retardant material as a flame retardant for plastics is better than the same amount of POSS or aluminum hydroxide. However, the invention patent document does not involve the use of flame retardants as flame retardants for coatings, and does not consider the application of composite flame retardants in coating construction, coating curing and film formation, and other issues.
[0013] Although the prior art discloses the use of POSS and epoxy resin to prepare flame retardant coatings, or discloses the use of aluminum hydroxide as a flame retardant for polymer materials or coatings, when a high content of POSS is directly added to epoxy resin-based coatings, the resulting coatings are prone to poor adhesion and poor impact resistance of the coatings due to excessive crosslinking, and it is difficult to obtain an ultra-thin coating without defects. If the amount of aluminum hydroxide added is too high, its dispersibility in the polymer matrix deteriorates, making it difficult to further improve the flame retardant properties of the coating, and other application properties of the coating may deteriorate. Summary of the invention
[0014] In order to solve the above problems, the present invention provides an intumescent flame retardant powder coating and a preparation method thereof. The powder coating obtained by the present invention can obtain an ultra-thin coating with a coating thickness of 0.3-0.7 mm. The obtained coating has the characteristics of fire retardant performance, mechanical impact resistance, good chemical resistance and excellent adhesion. The obtained coating can be used as an ultra-thin intumescent fire retardant coating for steel structures. In addition, the coating obtained by the present invention can achieve low-temperature curing, save energy, and can expand the application of the coating to the surface coating of heat-sensitive substrates.
[0015] The technical solution of the present invention to solve the above technical problems is as follows:
[0016] An intumescent flame retardant powder coating, wherein the raw materials of the powder coating include the following components by mass percentage: 30-50% of film-forming resin, 25-40% of composite flame retardant, 8-15% of POSS-based epoxy curing agent, 5-15% of epoxy-based POSS-modified aluminum hydroxide, 2-5% of pigment and filler, and 0.1-3% of auxiliary agent;
[0017] The composite flame retardant is composed of 20-35% of a carbonizing agent, 30-50% of a carbonizing catalyst, and 20-35% of a foaming agent in terms of mass percentage;
[0018] The epoxy POSS modified aluminum hydroxide is a reaction product of a caged polysilsesquioxane containing a silanol group, a silane coupling agent KH-560, and nano aluminum hydroxide;
[0019] The POSS-based epoxy curing agent is a reaction product of a caged polysilsesquioxane containing a primary amino group and carbonyldiimidazole, aniline or an aniline derivative.
[0020] Furthermore, the film-forming resin includes one or more of epoxy resin and polyester resin, and the epoxy resin includes one or more of bisphenol A epoxy resin, o-cresol epoxy resin, bisphenol F epoxy resin, and bisphenol S epoxy resin.
[0021] Furthermore, the polyester resin is a saturated carboxyl polyester resin with an acid value between 50-80 mgKOH / g.
[0022] Furthermore, the bisphenol A epoxy resin is one or more of E-20, E-12, and E-06.
[0023] Further, the preparation method of the POSS-based epoxy curing agent comprises the following steps:
[0024] S1: Add carbonyldiimidazole to a mixture of octaaminopropyl POSS, triethylamine and tetrahydrofuran at room temperature, react for 0.5-4 hours, then add an N,N-dimethylformamide solution containing aniline or an aniline derivative, and stir to react for 6-12 hours to obtain a reaction mixture;
[0025] S2: pouring the reaction mixture into water, extracting, washing, drying and separating to obtain a POSS-based epoxy curing agent.
[0026] Furthermore, the preparation method of the epoxy POSS modified aluminum hydroxide comprises the following steps:
[0027] SS1: Add nano aluminum hydroxide to 40-95% by mass ethanol aqueous solution, and ultrasonically disperse for 0.5-2h to obtain nano aluminum hydroxide dispersion;
[0028] SS2: Add caged polysilsesquioxane containing silanol groups and anhydrous ethanol into a constant temperature magnetic stirring water bath with a reflux device container, stir to obtain a uniform mixed solution, then add distilled water dropwise into the mixed solution while stirring, and raise the temperature to maintain reflux;
[0029] The caged polysilsesquioxane containing silanol groups is one or more of tetrasilanol phenylated caged polysilsesquioxane, trisilanol phenylated caged polysilsesquioxane, trisilanol isooctyl caged polysilsesquioxane, trisilanol isobutyl esterified caged polysilsesquioxane, and trisilanol ethyl esterified caged polysilsesquioxane;
[0030] SS3: Slowly add the nano aluminum hydroxide dispersion and the silane coupling agent KH-560 to the reflux liquid of step SS2 at the same time. After the addition is complete, continue the reaction for 5-12 hours, then filter, vacuum dry and sieve the solid to obtain epoxy POSS modified aluminum hydroxide.
[0031] Furthermore, the carbon-forming agent includes one or more of pentaerythritol, sorbitol, starch, dipentaerythritol, and glucose.
[0032] Furthermore, the carbon-forming catalyst includes one or more of ammonium bicarbonate, diammonium hydrogen phosphate, ammonium polyphosphate, and ammonium phosphate.
[0033] Furthermore, the foaming agent includes one or more of dicyandiamide, melamine, glycine, urea, and chlorinated paraffin.
[0034] Furthermore, the pigments and fillers include one or more of titanium dioxide, carbon black, barium sulfate, silica powder, talcum powder, mica powder, and calcium carbonate, and the additives include one or more of leveling agents, degassing agents, brighteners, charge enhancers, and texturing agents.
[0035] The present invention provides a method for preparing an intumescent flame retardant powder coating, the preparation method comprising the following steps:
[0036] (1) Weighing the raw material components of the powder coating in proportion, adding them into a mixer, mixing them evenly and crushing them to obtain a mixture;
[0037] (2) feeding the mixed material into an extruder for extrusion at a temperature of 80-100° C.;
[0038] (3) The extruded material is tableted, cooled, crushed, and sieved to select D 50 The powder with a particle size of 20-50 microns is the finished powder coating product.
[0039] The invention provides an application of an intumescent flame retardant powder coating, which is coated on a metal substrate or a heat-sensitive substrate by a high-voltage electrostatic method or a fluidized bed method, with a curing temperature of 130-160° C. and a curing time of 5-30 minutes.
[0040] Furthermore, the metal substrate is a steel structure, and the heat-sensitive substrate is a medium-density fiberboard, a sandwich panel, or a bakelite board.
[0041] The beneficial effects of the present invention are as follows:
[0042] The present invention adopts caged polysilsesquioxane containing silanol groups and silane coupling agent KH-560 to modify aluminum hydroxide sol, obtains POSS modified aluminum hydroxide containing epoxy groups, and uses it as the flame retardant of expansion flame retardant coating.Compared with conventional aluminum hydroxide flame retardant, the POSS modified aluminum hydroxide containing epoxy groups has better compatibility with matrix resin, its dispersibility in coating is better, and POSS structure is introduced, effectively improving the application performances such as flame retardant performance and mechanical properties of coating.And the POSS modified aluminum hydroxide containing epoxy groups contains epoxy reactive functional groups, can participate in curing reaction, reacts with the curing agent containing POSS structure equally, and forms stable POSS linking structure by covalent bond, under the premise of not affecting the dispersibility of POSS in coating matrix, effectively improves the content of POSS structure in coating, thereby can also obtain the technical effect that fire resistance is greater than 60min and adhesion is 0 grade in the case of thin coating.
[0043] The curing agent of the present invention is a medium and low temperature curing agent of the urea containing POSS, which can form a bonded structure with the POSS modified aluminum hydroxide containing epoxy groups through curing reaction, effectively improve the crosslinking density of the coating, and improve the POSS structure content in the coating. Make the coating film have excellent flame retardant properties, corrosion resistance and resistance to cold and heat shock and other properties. And the curing agent is a medium and low temperature curing agent, can crosslink with epoxy resin at a relatively low temperature without adding a curing accelerator to solidify the film, and save energy. DETAILED DESCRIPTION
[0044] The present invention will be further described below in conjunction with specific embodiments:
[0045] It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are merely used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0046] For the purpose of simplicity and illustration, the principles of the embodiments are described mainly by reference to examples. In the following description, many specific details are proposed to provide a thorough understanding of the embodiments. However, it is obvious. For those of ordinary skill in the art, these embodiments may not be limited to these specific details in practice. In some instances, known methods and structures are not described in detail to avoid making these embodiments unnecessarily difficult to understand. In addition, all embodiments may be used in combination with each other.
[0047] The selection of raw materials in the following examples and comparative examples is as follows:
[0048] The film-forming resin is epoxy resin E-12, produced by Kunshan Nan Ya; the carbonizing agent is pentaerythritol, produced by Henan Yongan Chemical; the carbonizing agent catalyst is ammonium polyphosphate, produced by Shandong Shian Chemical; and the foaming agent is melamine, produced by Jiangsu Sanmu Group.
[0049] In the composite flame retardant, the mass proportion of the carbon-forming agent pentaerythritol is 28%, the mass proportion of the carbon-forming catalyst ammonium polyphosphate is 50%, and the mass proportion of the foaming agent melamine is 22%.
[0050] The pigment and filler are a combination of titanium dioxide, calcium carbonate and precipitated barium sulfate, and the mass ratio of the three is 1:2:2. The sources of titanium dioxide, calcium carbonate and precipitated barium sulfate are commercially available powder coating raw materials.
[0051] The additives are a combination of leveling agent, charge enhancer and deaerator, with a mass ratio of 4:1:1. The leveling agent is Resiflow PL-200A, the charge enhancer is Lubrizol Lanco 308, and the deaerator is Clariant Ceridust 6050M.
[0052] The preparation method of POSS-based epoxy curing agent comprises the following steps:
[0053] S1: At room temperature, carbonyldiimidazole was added to a mixture of octaaminopropyl POSS, triethylamine and tetrahydrofuran, and the mixture was reacted for 2 h. Then, an N,N-dimethylformamide solution containing aniline was added, and the mixture was stirred and reacted for 12 h to obtain a reaction mixture; the molar ratio of octaaminopropyl POSS, triethylamine, carbonyldiimidazole and aniline was 1:8:8:8.
[0054] S2: pouring the reaction mixture into water, extracting, washing, drying and separating to obtain a POSS-based epoxy curing agent.
[0055] In the preparation step of the POSS-based epoxy curing agent, octaaminopropyl POSS (i.e., octaaminopropyl caged polysilsesquioxane) was obtained from Qiyue Biotechnology, and the remaining raw materials were obtained from commercially available reagents.
[0056] The preparation method of epoxy POSS modified aluminum hydroxide comprises the following steps:
[0057] SS1: Add 5 parts by weight of nano aluminum hydroxide to 100 parts by weight of 75% ethanol aqueous solution, and disperse by ultrasonic for 1 hour to obtain a nano aluminum hydroxide dispersion;
[0058] SS2: Add 3 parts by weight of trisilanol ethyl esterified cage-shaped silsesquioxane and 300 parts by weight of anhydrous ethanol into a constant temperature magnetic stirring water bath with a reflux device container, stir to obtain a uniform mixed solution, then add 50 parts by weight of distilled water dropwise into the mixed solution while stirring, and increase the temperature to maintain reflux.
[0059] SS3: 50 parts by weight of nano-aluminum hydroxide dispersion and 1 part by weight of silane coupling agent KH-560 are slowly added to the reflux liquid of step SS2 at the same time. After the addition is complete, the reaction is continued at 50° C. for 8 hours, and then filtered. The solid is vacuum dried and passed through a 400-mesh sieve to obtain epoxy POSS-modified aluminum hydroxide.
[0060] In the preparation steps of epoxy POSS modified aluminum hydroxide, nano aluminum hydroxide is VK-LA20 from Jingrui New Materials, trisilanol ethyl esterified cage-shaped silsesquioxane comes from Delta Biotechnology, and the remaining raw materials are commercially available chemical reagents.
[0061] Example 1
[0062] Film-forming resin 35%, composite flame retardant 40%, POSS-based epoxy curing agent 12%, epoxy POSS-modified aluminum hydroxide 7%, pigments and fillers 4%, and additives 2%.
[0063] Example 2
[0064] Film-forming resin 50%, composite flame retardant 20%, POSS-based epoxy curing agent 15%, epoxy-based POSS-modified aluminum hydroxide 10%, pigments and fillers 3%, and additives 2%.
[0065] Example 3
[0066] Film-forming resin 42%, composite flame retardant 28%, POSS-based epoxy curing agent 13%, epoxy POSS-modified aluminum hydroxide 10%, pigments and fillers 5%, and additives 2%.
[0067] Comparative Example 1
[0068] Film-forming resin 42%, composite flame retardant 28%, dicyandiamide 5%, VK-LA20 nano aluminum hydroxide 10%, pigment filler 13%, auxiliary agent 2%. That is, on the basis of Example 3, conventional dicyandiamide is used as a curing agent, and unmodified nano aluminum hydroxide is used as a flame retardant filler.
[0069] Comparative Example 2
[0070] Film-forming resin 42%, composite flame retardant 28%, octaaminopropyl POSS 13%, epoxy POSS modified aluminum hydroxide 10%, pigment 5%, additive 2%. That is, on the basis of Example 3, the homemade POSS-based epoxy curing agent is replaced by octaaminopropyl POSS of the same mass percentage.
[0071] Comparative Example 3
[0072] Film-forming resin 42%, composite flame retardant 28%, POSS-based epoxy curing agent 13%, VK-LA20 nano aluminum hydroxide 10%, pigment filler 5%, auxiliary agent 2%. That is, on the basis of Example 3, unmodified nano aluminum hydroxide is used as the flame retardant filler.
[0073] Comparative Example 4
[0074] Film-forming resin 42%, composite flame retardant 28%, POSS-based epoxy curing agent 13%, amino POSS-modified aluminum hydroxide 10%, pigments and fillers 5%, and auxiliary agents 2%. That is, on the basis of Example 3, amino POSS-modified aluminum hydroxide is used to replace epoxy POSS-modified aluminum hydroxide, wherein amino POSS-modified aluminum hydroxide is based on the preparation method of epoxy POSS-modified aluminum hydroxide, and KH-550 is used to replace KH-560.
[0075] The preparation method of the intumescent flame retardant powder coating of the above embodiment and comparative example comprises the following steps:
[0076] Step 1, preparing raw materials of corresponding weight percentage according to the formula, including preparing POSS-based epoxy curing agent, epoxy POSS-modified aluminum hydroxide, and amino POSS-modified aluminum hydroxide.
[0077] Step 2: adding each raw material component into a mixer, mixing them evenly, and crushing them to obtain a mixed material.
[0078] Step 3, feeding the crushed mixed material into an extruder and extruding at 95°C.
[0079] Step 4, tabletting, cooling, crushing and screening the extruded material, selecting powder of 20-40 μm, and obtaining an intumescent flame retardant powder coating.
[0080] Performance Testing:
[0081] The coatings obtained in the examples and comparative examples were applied to the steel structure by electrostatic spraying and then cured at 150° C. for 30 min. The thickness of the obtained coating was about 0.6 mm.
[0082] According to GB / T 14907-2018 steel structure fire retardant coating test standard, the salt spray corrosion resistance, bonding strength, high temperature and humidity, acid resistance, alkali resistance and fire resistance of the obtained coating are tested. The flame retardant grade refers to the vertical burning test. Mechanical impact test method: GB / T1732-1993; Adhesion test method: GB / T9286-2021; Hardness test method: GB / T5739-2006.
[0083] The test results are as follows:
[0084]
[0085]
[0086] From the above test results, it can be seen that the coating obtained from the powder coating obtained in Examples 1-3 has an adhesion of level 0, a hardness of up to 2H, a bonding strength ≥7MPa, a double 85 high temperature and high humidity test of greater than 1000h, a high and low temperature impact of greater than 1000 cycles, a flame retardant grade of V-0, a fire resistance limit of greater than 60min, and has good resistance to salt spray corrosion, acid and alkali resistance.
[0087] Comparative Example 1 uses conventional dicyandiamide as a curing agent on the basis of Example 3, and uses unmodified nano aluminum hydroxide as a flame retardant filler. The resulting coating has a high curing temperature, low hardness of the coating film, and poor flame retardancy, corrosion resistance and chemical resistance.
[0088] Comparative Example 2 uses octaaminopropyl POSS to replace the homemade POSS-based epoxy curing agent as the curing agent of the powder coating on the basis of Example 3, and the curing effect of the coating film of the obtained coating is deteriorated. In addition, the flexibility of the obtained coating film is deteriorated, resulting in poor adhesion and impact resistance.
[0089] Comparative Example 3 uses unmodified nano aluminum hydroxide to replace the epoxy POSS modified aluminum hydroxide on the basis of Example 3. Since the content of POSS in the coating film becomes lower and the cross-linking density of the cured coating film becomes lower, the hardness, fire retardant properties, chemical resistance, salt spray resistance, high temperature and humidity resistance, and aging resistance of the coating film deteriorate.
[0090] Comparative Example 4, based on Example 3, uses homemade amino POSS-modified aluminum hydroxide to replace the homemade epoxy POSS-modified aluminum hydroxide. The compatibility of the modified aluminum hydroxide with the coating deteriorates, and no covalent bond can be formed between the modified aluminum hydroxide and the POSS-based epoxy curing agent, resulting in the compatibility of the POSS in the coating with the polymer matrix deteriorating, thereby causing the application performance of the coating to deteriorate.
[0091] It can be seen that the coating of the intumescent flame retardant powder coating obtained by the present invention is an ultra-thin coating with excellent comprehensive application performance, and can be used as an ultra-thin intumescent flame retardant powder coating for fire retardancy of steel structures. On the other hand, the curing temperature of the intumescent flame retardant coating obtained by the present invention is low, which saves energy, and the coating can be applied to heat-sensitive substrates.
[0092] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. An intumescent flame retardant powder coating, Features: The raw materials of the coating include the following components in percentage by mass: 30-50% film-forming resin, 25-40% composite flame retardant, 8-15% POSS-based epoxy curing agent, 5-15% epoxy-based POSS-modified aluminum hydroxide, 2-5% pigment and filler, and 0.1-3% additive; The film-forming resin includes one or more of epoxy resin and polyester resin; The composite flame retardant is composed of 20-35% of carbon forming agent, 30-50% of carbon forming catalyst and 20-35% of foaming agent in terms of mass percentage; The epoxy POSS modified aluminum hydroxide is a reaction product of a caged polysilsesquioxane containing a silanol group, a silane coupling agent KH-560, and nano aluminum hydroxide; The caged polysilsesquioxane containing silanol groups is one or more of tetrasilanol phenylated caged polysilsesquioxane, trisilanol phenylated caged polysilsesquioxane, trisilanol isooctyl caged polysilsesquioxane, trisilanol isobutyl esterified caged polysilsesquioxane, and trisilanol ethyl esterified caged polysilsesquioxane; The POSS-based epoxy curing agent is a reaction product of a caged polysilsesquioxane containing a primary amino group and carbonyldiimidazole, aniline or an aniline derivative; The preparation method of the POSS-based epoxy curing agent comprises the steps: S1: Add carbonyldiimidazole to a mixture of octaaminopropyl POSS, triethylamine and tetrahydrofuran at room temperature, react for 0.5-4 hours, then add an N,N-dimethylformamide solution containing aniline or an aniline derivative, and stir to react for 6-12 hours to obtain a reaction mixture; S2: pouring the reaction mixture into water, extracting, washing, drying and separating to obtain a POSS-based epoxy curing agent.
2. The intumescent flame retardant powder coating according to claim 1, Features: The epoxy resin includes one or more of bisphenol A epoxy resin, o-cresol epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin or modified epoxy resin; the polyester resin is a saturated carboxyl polyester resin with an acid value between 50-80 mgKOH / g.
3. The intumescent flame retardant powder coating according to claim 2, Features: The bisphenol A type epoxy resin is one or more of E-20, E-12 and E-06.
4. The intumescent flame retardant powder coating according to claim 1, Features: The preparation method of the epoxy POSS modified aluminum hydroxide comprises the following steps: SS1: Add nano aluminum hydroxide to 40-95% by mass ethanol aqueous solution, and ultrasonically disperse for 0.5-2h to obtain nano aluminum hydroxide dispersion; SS2: Add caged polysilsesquioxane containing silanol groups and anhydrous ethanol into a constant temperature magnetic stirring water bath with a reflux device container, stir to obtain a uniform mixed solution, then add deionized water dropwise into the mixed solution while stirring, and increase the temperature to maintain reflux; The caged polysilsesquioxane containing silanol groups is one or more of tetrasilanol phenylated caged polysilsesquioxane, trisilanol phenylated caged polysilsesquioxane, trisilanol isooctyl caged polysilsesquioxane, trisilanol isobutyl esterified caged polysilsesquioxane, and trisilanol ethyl esterified caged polysilsesquioxane; SS3: Slowly add the nano aluminum hydroxide dispersion and the silane coupling agent KH-560 to the reflux liquid of step SS2 at the same time. After the addition is complete, continue the reaction for 5-12 hours, then filter, vacuum dry and sieve the solid to obtain epoxy POSS modified aluminum hydroxide.
5. The intumescent flame retardant powder coating according to claim 1, Features: The carbon-forming agent includes one or more of pentaerythritol, sorbitol, starch, dipentaerythritol, and glucose; the carbon-forming catalyst includes one or more of ammonium bicarbonate, diammonium hydrogen phosphate, ammonium polyphosphate, and ammonium phosphate; and the foaming agent includes one or more of dicyandiamide, melamine, glycine, urea, and chlorinated paraffin.
6. The intumescent flame retardant powder coating according to claim 1, Features: The pigments and fillers include one or more of titanium dioxide, carbon black, barium sulfate, silica powder, talcum powder, mica powder, and calcium carbonate; the additives include one or more of leveling agents, degassing agents, brighteners, charge enhancers, and texture agents.
7. A method for preparing an intumescent flame retardant powder coating according to any one of claims 1 to 6, Features The preparation method comprises the following steps: (1) Weigh the raw material components of the powder coating in proportion, add them into a mixer, mix them evenly and crush them to obtain a mixture; (2) feeding the mixed material into an extruder for extrusion at a temperature of 80-100°C; (3) The extruded material is tableted, cooled, crushed, and sieved to select powder with a D50 particle size of 20-50 microns to obtain a finished powder coating.
8. Use of the intumescent flame retardant powder coating according to any one of claims 1 to 6, Features: It is applied on metal substrates or heat-sensitive substrates by high-voltage electrostatic method or fluidized bed method, with a curing temperature of 130-160°C and a curing time of 5-30 minutes.
9. Use of the intumescent flame retardant powder coating according to claim 8, Features: The metal substrate is a steel structure, and the heat-sensitive substrate is a medium-density fiberboard, a sandwich panel, or a bakelite board.
Citation Information
Patent Citations
Fireproof powder paint for super-thin steel structure and preparation method thereof
CN101058694A
Preparation method of modified ultra-thin fire-resistant coating polymer matrix based on silsesquioxane
CN101597385A
POSS / epoxy nanometer hybrid material and preparation method and application thereof
CN101985513A
Preparation method of polyhedral oligomeric silsesquioxane-aluminum hydroxide composite flame-resistant material
CN104829864A