Photovoltaic bracket prepared by extruding and reshaping waste wind turbine blades and preparation method thereof
By combining waste wind power blade powder and waste thermoplastic resin particles with chemical additives, photovoltaic brackets are prepared, which solves the problem of waste wind power blade and waste thermoplastic resin disposal, realizes cascade utilization and harmless disposal, and reduces environmental pollution and Disposal cost and improves the mechanical properties and combustion resistance of the photovoltaic bracket.
Patent Information
- Application Number
- CN202410194311.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-21
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-02-21
AI Technical Summary
The prior art cannot effectively realize the cascade utilization and harmless disposal of waste wind power blades and waste thermoplastic resins, resulting in high environmental pollution and disposal costs.
Photovoltaic brackets are prepared by waste wind power blade powder and waste thermoplastic resin particles combined with chemical additives. Through mixing and refining and extrusion molding, photovoltaic brackets with good mechanical properties are prepared to realize the cascade utilization and harmlessness of waste materials. Disposal.
It reduces the risk of environmental pollution and disposal costs, improves economic benefits, and improves the mechanical properties and combustion resistance of the photovoltaic stent through the synergistic effects of silane coupling agent, lubricant and flame retardant.
Smart Images

Figure CN118146647B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of solid waste treatment, and in particular, to a photovoltaic bracket prepared from waste wind turbine blade extrusion and reshaping materials and a preparation method thereof. Background Art
[0002] As resources become increasingly scarce, the recycling of waste resources will be of great significance. Wind power has been developed on a large scale in my country, and a large number of wind turbines will be retired year by year in the near future. Most of the current wind turbine blades are made of fiber-reinforced thermosetting resin-based composite materials (glass fiber reinforced plastics). At this stage, they are treated by stacking and burying, which not only occupies land, but also causes environmental pollution. Therefore, how to dispose of waste wind turbine blades will become a major problem in the field of solid waste treatment. In addition, waste plastics are regarded as white garbage, which is difficult to degrade in the environment and will also cause long-term and deep-seated environmental problems. In addition, the existing technology cannot achieve the cascade utilization and harmless disposal of waste wind turbine blades and waste thermoplastic resins, resulting in high disposal costs for waste wind turbine blades and waste thermoplastic resins. Summary of the invention
[0003] The purpose of the present invention is to provide a photovoltaic bracket made of waste wind turbine blade extrusion reshaped material and a preparation method thereof, so as to solve the problem that the prior art cannot achieve the cascade utilization and harmless disposal of waste wind turbine blades and waste thermoplastic resins.
[0004] In order to achieve the above-mentioned purpose, the first aspect of the present disclosure provides a photovoltaic bracket prepared by extruding and reshaping materials of waste wind turbine blades, wherein the raw materials for preparing the photovoltaic bracket include waste wind turbine blade powder, waste thermoplastic resin particles and chemical additives; the particle size of the waste wind turbine blade powder is 5 to 20 meshes; the chemical additives include silane coupling agents, lubricants, colorants, flame retardants and plasticizers; relative to 100 parts by weight of the waste wind turbine blade powder and the waste thermoplastic resin particles, the waste wind turbine blade powder The content of the waste thermoplastic resin particles is 20-80 parts by weight, the content of the silane coupling agent is 1-5 parts by weight, the content of the lubricant is 1-2 parts by weight, the content of the colorant is 0.1-2 parts by weight, the content of the flame retardant is 1-5 parts by weight, and the content of the plasticizer is 1-5 parts by weight; the weight ratio of the plasticizer, the silane coupling agent and the lubricant is (1-5): (1-2): 1.
[0005] Optionally, the particle size of the waste wind turbine blade powder is 6-15 mesh.
[0006] Optionally, the waste thermoplastic resin particles are crushed materials with a particle size of 0.5-2 cm; the waste thermoplastic resin particles include one or more of polyethylene, polypropylene, polyvinyl chloride and polystyrene.
[0007] Optionally, the silane coupling agent includes a vinyl silane coupling agent, a methacryloxy silane coupling agent and an epoxy silane coupling agent; the lubricant includes one or more of stearic acid, methyl stearate and capric amide; the colorant includes one or more of chrome yellow, cadmium red and phthalocyanine blue; the flame retardant includes one or more of antimony trioxide, ammonium polyphosphate and antimony oxide; and the plasticizer is dibutyl phthalate.
[0008] Optionally, the weight ratio of the total weight of the vinyl silane coupling agent and the methacryloyloxy silane coupling agent to the epoxy silane coupling agent is (4-7):1; the lubricant is a composition of stearic acid, methyl stearate and capric amide; the weight ratio of stearic acid, methyl stearate and capric amide is (1.5-2):(5-6):(2.5-3).
[0009] Optionally, relative to 100 parts by weight of the waste wind turbine blade powder and waste thermoplastic resin particles, the content of the waste wind turbine blade powder is 30 to 70 parts by weight, the content of the waste thermoplastic resin particles is 30 to 70 parts by weight, the content of the silane coupling agent is 1.5 to 4 parts by weight, the content of the lubricant is 1 to 1.5 parts by weight, the content of the colorant is 0.5 to 1 part by weight, the content of the flame retardant is 2 to 4 parts by weight, and the content of the plasticizer is 2 to 4 parts by weight.
[0010] Optionally, the weight ratio of the plasticizer, the silane coupling agent and the lubricant is (2-4):(1.5-2):1.
[0011] A second aspect of the present disclosure provides a method for preparing a photovoltaic support by extruding and reshaping waste wind turbine blades, the method comprising:
[0012] S1, putting waste wind turbine blade powder, waste thermoplastic resin particles and chemical additives into a mixing device for mixing and refining to obtain a mixed material;
[0013] The chemical additives include silane coupling agents, lubricants, colorants, flame retardants and plasticizers;
[0014] The particle size of the waste wind turbine blade powder is 5-20 mesh;
[0015] Relative to 100 parts by weight of the waste wind turbine blade powder and the waste thermoplastic resin particles, the added amount of the waste wind turbine blade powder is 20 to 80 parts by weight, the added amount of the waste thermoplastic resin particles is 20 to 80 parts by weight, the added amount of the silane coupling agent is 1 to 5 parts by weight, the added amount of the lubricant is 1 to 2 parts by weight, the added amount of the colorant is 0.1 to 2 parts by weight, the added amount of the flame retardant is 1 to 5 parts by weight, and the added amount of the plasticizer is 1 to 5 parts by weight; the weight ratio of the plasticizer, the silane coupling agent and the lubricant is (1 to 5): (1 to 2): 1;
[0016] S2, allowing the mixed material to enter an extrusion molding device for melt extrusion and molding to obtain a photovoltaic support component;
[0017] S3, assembling the photovoltaic support components to obtain a photovoltaic support.
[0018] Optionally, step S1 also includes: allowing the waste wind turbine blade powder, the waste thermoplastic resin particles, the silane coupling agent, the lubricant and part of the plasticizer to enter a mixing device for a first mixing and refining treatment to obtain a first mixed material; allowing another part of the plasticizer, the colorant and the flame retardant to enter the mixing device and mix with the first mixed material for a second mixing and refining treatment to obtain the mixed material; the weight ratio of the plasticizer added in the first mixing and refining treatment and the second mixing and refining treatment is (1~4):1.
[0019] Optionally, the temperature of the mixing and refining treatment is 80~115℃, and the time is 0.1~0.3h; the temperature of the first mixing and refining treatment is 80~95℃, and the time is 0.1~0.2h; the temperature of the second mixing and refining treatment is 100~115℃, and the time is 0.1~0.2h; the temperature of the melt extrusion treatment is 160~220℃, the pressure of the molding treatment is 2~50MPa, and the time is 1.5~5min.
[0020] Through the above technical scheme, the raw materials of the photovoltaic bracket prepared by the present invention contain waste wind turbine blade powder with a smaller particle size, which can realize the cascade utilization and harmless disposal of waste wind turbine blades and waste thermoplastic resins, reduce the risk of environmental pollution and disposal costs, and thus improve economic benefits. In addition, under the synergistic effect of silane coupling agents, lubricants and plasticizers in chemical additives, not only can the coupling effect of the resin components of the waste wind turbine blade powder and the waste thermoplastic resin particles be improved, but also the bonding effect between the glass fiber and the resin in the waste wind turbine blade powder can be improved, thereby obtaining a photovoltaic bracket with mechanical properties that meet the requirements of photovoltaic equipment. In addition, under the action of flame retardants, the obtained photovoltaic bracket can have better flame resistance.
[0021] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0023] Figure 1 The present invention discloses a process flow chart of a method for preparing a photovoltaic support by extruding and reshaping waste wind turbine blades.
[0024] Description of Reference Numerals
[0025] 1 blade cutting device; 2 shredding device; 3 grinding device; 4 mixing device; 5 cleaning device; 6 crushing device; 8 extrusion molding device; 9 performance testing unit; 10 assembly unit; A waste wind turbine blades; B chemical additives; C waste thermoplastic resin. DETAILED DESCRIPTION
[0026] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0027] The first aspect of the present disclosure provides a photovoltaic bracket prepared by extruding and reshaping materials of waste wind turbine blades. The raw materials for preparing the photovoltaic bracket include waste wind turbine blade powder, waste thermoplastic resin particles and chemical additives B; the particle size of the waste wind turbine blade powder is 5-20 mesh; the chemical additives B include silane coupling agents, lubricants, colorants, flame retardants and plasticizers; relative to 100 parts by weight of the waste wind turbine blade powder and the waste thermoplastic resin particles, the content of the waste wind turbine blade powder is 20-80 parts by weight, the content of the waste thermoplastic resin particles is 20-80 parts by weight, the content of the silane coupling agent is 1-5 parts by weight, the content of the lubricant is 1-2 parts by weight, the content of the colorant is 0.1-2 parts by weight, the content of the flame retardant is 1-5 parts by weight, and the content of the plasticizer is 1-5 parts by weight; the weight ratio of the plasticizer, the silane coupling agent and the lubricant is (1-5): (1-2): 1.
[0028] Through the above technical scheme, the raw materials of the photovoltaic bracket prepared by the present invention contain waste wind turbine blade powder with smaller particle size, which can realize the cascade utilization and harmless disposal of waste wind turbine blades A and waste thermoplastic resin C, reduce the risk of environmental pollution and disposal costs, and thus improve economic benefits. In addition, under the synergistic effect of the silane coupling agent, lubricant and plasticizer in the chemical auxiliary agent B, not only can the coupling effect of the resin component of the waste wind turbine blade powder and the waste thermoplastic resin particles be improved, but also the bonding effect between the glass fiber and the resin in the waste wind turbine blade powder can be improved, so that a photovoltaic bracket with mechanical properties that meet the requirements of photovoltaic equipment can be obtained. In addition, under the action of the flame retardant, the obtained photovoltaic bracket can have better flame resistance.
[0029] In a preferred embodiment, relative to 100 parts by weight of the waste wind turbine blade powder and waste thermoplastic resin particles, the content of the waste wind turbine blade powder is 30 to 70 parts by weight, the content of the waste thermoplastic resin particles is 30 to 70 parts by weight, the content of the silane coupling agent is 1.5 to 4 parts by weight, the content of the lubricant is 1 to 1.5 parts by weight, the content of the colorant is 0.5 to 1 part by weight, the content of the flame retardant is 2 to 4 parts by weight, and the content of the plasticizer is 2 to 4 parts by weight.
[0030] In a further preferred embodiment, relative to 100 parts by weight of the waste wind turbine blade powder and waste thermoplastic resin particles, the content of the waste wind turbine blade powder is 40 to 60 parts by weight, the content of the waste thermoplastic resin particles is 40 to 60 parts by weight, the content of the silane coupling agent is 1.5 to 3 parts by weight, the content of the lubricant is 1 to 1.25 parts by weight, the content of the colorant is 0.5 to 0.8 parts by weight, the content of the flame retardant is 2 to 3 parts by weight, and the content of the plasticizer is 2 to 3 parts by weight.
[0031] In a specific implementation, relative to 100 parts by weight of the waste wind turbine blade powder and waste thermoplastic resin particles, the content of the waste wind turbine blade powder is 50 parts by weight, the content of the waste thermoplastic resin particles is 50 parts by weight, the content of the silane coupling agent is 2 parts by weight, the content of the lubricant is 1 part by weight, the content of the colorant is 0.5 parts by weight, the content of the flame retardant is 2 parts by weight, and the content of the plasticizer is 3 parts by weight.
[0032] In the above embodiment, by reasonably proportioning the components in the raw materials of the photovoltaic bracket, the mechanical properties of the profile of the photovoltaic bracket can be further enhanced. Specifically, the density of the profile of the photovoltaic bracket can be increased to 1300 kg / m 3 The tensile strength is above 15 MPa, the compressive strength is above 35 MPa, the flexural strength is above 35 MPa, the elastic modulus is above 3 GPa, and the compressive elastic modulus is above 3 GPa.
[0033] In a preferred embodiment, the particle size of the waste wind turbine blade powder is 6-15 mesh.
[0034] In a specific implementation, the particle size of the waste wind turbine blade powder is 8-11 meshes.
[0035] In the above-mentioned embodiment, the waste wind turbine blade powder used in the present disclosure is obtained by cutting, shredding, grinding and screening the waste wind turbine blades A in sequence. Since the waste wind turbine blades A are composed of glass fibers and thermosetting resins, after the waste wind turbine blades A are ground, the glass fibers in the thermosetting resin will be cut into glass fibers of suitable lengths, and the extension direction of the glass fibers is irregular in the photovoltaic bracket. Specifically, on the one hand, it contains more glass fibers whose extension direction is consistent with the extension direction of the photovoltaic bracket and / or has an angle distribution. This type of glass fiber will improve the mechanical properties of the photovoltaic bracket; on the other hand, it contains smaller glass fibers whose extension direction is perpendicular to the extension direction of the photovoltaic bracket. This type of glass fiber will affect the mechanical properties of the photovoltaic bracket. ; When the particle size of the waste wind turbine blade powder is small, the length of the glass fiber in the profile of the prepared photovoltaic bracket is small. Although the vertically distributed glass fiber has little effect on the mechanical strength of the photovoltaic bracket, the glass fiber distributed in the same direction and / or with an angle has little improvement on the mechanical strength of the photovoltaic bracket, which will reduce the mechanical properties of the prepared photovoltaic bracket; When the particle size of the waste wind turbine blade powder is large, the length of the glass fiber in the profile of the prepared photovoltaic bracket is large, and the vertically distributed glass fiber has a greater effect on the mechanical strength of the photovoltaic bracket, which will reduce the mechanical properties of the prepared photovoltaic bracket. Therefore, in order to further improve the mechanical properties of the prepared photovoltaic bracket, the particle size of the waste wind turbine blade powder can be optimized.
[0036] In one embodiment, the waste thermoplastic resin particles used in the present disclosure are conventionally selected in the art and are not specifically required in this application. For example, the waste thermoplastic resin particles include one or more of polyethylene, polypropylene, polyvinyl chloride and polystyrene, preferably mixed resin particles of polyethylene and polypropylene.
[0037] In one embodiment, the waste thermoplastic resin particles are crushed materials with a particle size of 0.5-2 cm. Preferably, the waste thermoplastic resin particles are crushed materials with a particle size of 1-1.8 cm.
[0038] In this embodiment, before mixing and refining the waste wind turbine blade powder with the waste thermoplastic resin particles, the waste thermoplastic resin C is washed and crushed to obtain crushed waste thermoplastic resin particles, which can improve the effect of mixing and refining. In order to further improve the effect of mixing and refining, the particle size of the crushed waste thermoplastic resin particles can be optimized.
[0039] In one embodiment, in order to further improve the mechanical properties of the photovoltaic bracket, the raw materials of the photovoltaic bracket also include a chemical additive B, and the chemical additive B includes a silane coupling agent, a lubricant, a colorant, a flame retardant and a plasticizer.
[0040] In one embodiment, the silane coupling agent includes a vinyl silane coupling agent, a methacryloxy silane coupling agent and an epoxy silane coupling agent; wherein the vinyl silane coupling agent includes one or more of vinyl triethoxy silane (A151), vinyl trimethoxy silane (A171) and vinyl tri(β-methoxyethoxy) silane (A172); the methacryloxy silane coupling agent may be γ-(methacryloyloxy)propyl trimethoxy silane (KH-570); the epoxy silane coupling agent may be γ-glycidyloxypropyl trimethoxy silane (KH-560).
[0041] In a preferred embodiment, the silane coupling agent is a combination of a vinyl silane coupling agent, a methacryloxy silane coupling agent and an epoxy silane coupling agent.
[0042] In the above embodiment, by adding a silane coupling agent to the raw materials of the photovoltaic support, the non-hydrolyzable organic functional group at one end of the silane coupling agent can be combined with the thermoplastic resin, and the hydrolyzable group at the other end of the silane coupling agent can be combined with the glass fiber exposed on the surface of the waste wind turbine blade powder, thereby improving the graft coupling effect between the waste wind turbine blade powder and the waste thermoplastic resin particles, thereby improving the mechanical properties of the photovoltaic support assembly. Vinyl silane coupling agents and methacryloxy silane coupling agents can further improve the bonding strength between such silane coupling agents and polyester resins or acrylic resins; epoxy silane coupling agents can improve the bonding strength between such silane coupling agents and epoxy resins.
[0043] In one embodiment, the weight ratio of the total weight of the vinyl silane coupling agent and the methacryloxy silane coupling agent to the epoxy silane coupling agent is (4-7):1, preferably (4-6):1.
[0044] In this embodiment, in order to further improve the bonding strength between the waste wind turbine blade powder and the thermoplastic resin, the content of each component in the silane coupling agent can be optimized according to the specific composition of the thermoplastic material. For example, when the polyester resin or acrylic resin in the thermoplastic material is relatively large, the total weight of the vinyl silane coupling agent and the methacryloxy silane coupling agent can be increased accordingly. According to the specific composition of the thermoplastic resin described in the present disclosure, it is necessary to optimize the weight ratio of the total weight of the vinyl silane coupling agent and the methacryloxy silane coupling agent to the epoxy silane coupling agent.
[0045] In one embodiment, the lubricant includes one or more of stearic acid, methyl stearate and capric amide.
[0046] In a preferred embodiment, the lubricant is a composition of stearic acid, methyl stearate and capric amide, wherein the weight ratio of stearic acid, methyl stearate and capric amide is (1-2):(5-7):(2-3), preferably (1.5-2):(5-6):(2.5-3), and more preferably 2:5:3.
[0047] In this embodiment, by adding lubricants to the raw materials of the photovoltaic bracket, not only can the materials obtained after mixing and refining have better softness and tensile properties, but also the mechanical properties of the photovoltaic bracket can be improved; the effect of melt extrusion treatment can also be improved to make the surface of the prepared photovoltaic bracket smooth. Among them, stearic acid acts as an external lubricant, which can reduce the friction between the thermoplastic resin and the thermosetting resin, reduce the difficulty of mixing between the thermosetting resin and the thermoplastic resin, and thus improve the mixing uniformity of the waste wind turbine blade powder inside the thermoplastic resin; decylamide acts as an internal lubricant, which can reduce the friction of the thermoplastic resin during stirring, reduce the friction of the thermoplastic resin during stirring, and improve the mixing uniformity of the waste wind turbine blade powder inside the thermoplastic resin; methyl stearate can have the functions of both external lubricant and internal lubricant.
[0048] In one embodiment, the plasticizer is dibutyl phthalate. In this embodiment, by adding the plasticizer to the raw materials of the photovoltaic bracket, on the one hand, the solubility of the thermoplastic resin particles can be improved, thereby improving the mixing effect of the thermoplastic resin particles and the waste wind turbine blade powder; on the other hand, the material obtained after the mixing and refining can have better softness, so that the waste wind turbine blade powder can be evenly dispersed in the entire photovoltaic bracket, thereby improving the mechanical properties of the entire photovoltaic bracket.
[0049] In one embodiment, the colorant includes one or more of chrome yellow, cadmium red and phthalocyanine blue.
[0050] In one embodiment, the flame retardant includes one or more of antimony trioxide, ammonium polyphosphate and antimony oxide. In this embodiment, by adding the flame retardant to the raw materials of the photovoltaic bracket, the photovoltaic bracket can have flame retardant properties.
[0051] In one embodiment, in order to further enhance the synergistic effect of the silane coupling agent, the plasticizer and the lubricant, the weight ratio of the plasticizer, the silane coupling agent and the lubricant can be optimized. Specifically, the weight ratio of the plasticizer, the silane coupling agent and the lubricant is (1-5): (1-2): 1, preferably (2-4): (1.5-2): 1, and more preferably (2.5-3.5): (1.8-2): 1.
[0052] In a specific implementation manner, the weight ratio of the plasticizer, the silane coupling agent and the lubricant is 3:2:1.
[0053] In this embodiment, adding corresponding silane coupling agents, plasticizers and lubricants to the raw materials of the photovoltaic bracket can further enhance the synergistic effect of the silane coupling agents, plasticizers and lubricants, thereby further enhancing the coupling effect of the resin components of the waste wind turbine blade powder and the waste thermoplastic resin particles, and further enhancing the bonding effect between the glass fiber in the waste wind turbine blade powder and the resin, thereby improving the mechanical properties of the photovoltaic bracket.
[0054] like Figure 1 As shown, the second aspect of the present disclosure provides a method for preparing a photovoltaic bracket by extruding and reshaping waste wind turbine blades, the method comprising:
[0055] S1, putting waste wind turbine blade powder, waste thermoplastic resin particles and chemical additive B into a mixing device 4 for mixing and refining to obtain a mixed material;
[0056] The chemical auxiliary agent B includes a silane coupling agent, stearic acid, a colorant, a flame retardant and an epoxy resin;
[0057] The particle size of the waste wind turbine blade powder is 5-20 mesh;
[0058] Relative to 100 parts by weight of the waste wind turbine blade powder and the waste thermoplastic resin particles, the added amount of the waste wind turbine blade powder is 20 to 80 parts by weight, the added amount of the waste thermoplastic resin particles is 20 to 80 parts by weight, the added amount of the silane coupling agent is 1 to 5 parts by weight, the added amount of the lubricant is 1 to 2 parts by weight, the added amount of the colorant is 0.1 to 2 parts by weight, the added amount of the flame retardant is 1 to 5 parts by weight, and the added amount of the plasticizer is 1 to 5 parts by weight; the weight ratio of the plasticizer, the silane coupling agent and the lubricant is (1 to 5): (1 to 2): 1;
[0059] S2, allowing the mixed material to enter the extrusion molding device 8 for melt extrusion and molding to obtain a photovoltaic support component;
[0060] S3, assembling the photovoltaic support components to obtain a photovoltaic support.
[0061] Through the above-mentioned implementation mode, waste wind turbine blades A and waste thermoplastic resin C are processed to obtain waste wind turbine blade powder and waste thermoplastic resin particles with smaller particle size, and the waste wind turbine blade powder, waste thermoplastic resin particles and chemical additive B are mixed and refined, and then subjected to hot pressing treatment to obtain a photovoltaic bracket with mechanical properties that meet the requirements of photovoltaic equipment; and the photovoltaic bracket prepared in the present invention can achieve the cascade utilization and harmless disposal of waste wind turbine blades A and waste thermoplastic resin C, reduce the risk of environmental pollution and disposal costs, and thus improve economic benefits.
[0062] In one implementation, step S1 further includes:
[0063] S11. The waste wind turbine blades A are fed into a blade cutting device 1 for cutting to obtain waste wind turbine blade blocks; the wind turbine blade blocks are fed into a shredding device 2 for shredding to obtain waste wind turbine blade particles; the waste wind turbine blade particles are fed into a grinding device 3 for grinding to obtain waste wind turbine blade powder; the waste wind turbine blade blocks have a length of 0.5 to 1.5 m and a width of 0.3 to 0.6 m; the particle size of the waste wind turbine blade particles is 1 to 3 cm.
[0064] The blade cutting device 1, the shredding device 2 and the grinding device 3 used in the present disclosure are respectively conventionally selected in the art, and this application does not make any special requirements.
[0065] In one embodiment, step S11 further includes, before the cutting process, subjecting the waste wind turbine blades A to dust removal by a dust removal device to avoid the introduction of impurities during the mixing and refining process, thereby reducing the mechanical properties of the photovoltaic support.
[0066] In one embodiment, a belt conveyor device is provided between the blade cutting device 1, the shredding device 2 and the grinding device 3, so that the materials generated at the outlet of each device can enter the subsequent device through the belt conveyor device.
[0067] In one embodiment, a screening device is provided at the outlet of the powder device so that the waste wind turbine blade powder with a particle size of 5-20 mesh can enter the mixing device 4 for mixing and refining. The screening device used in the present disclosure is a conventional choice in the art, for example, the screening device can be a plurality of screens of different specifications.
[0068] In a specific embodiment, the screening device of the present disclosure is two screens, namely a first screen and a second screen, wherein the mesh number of the first screen is 5-8 meshes, and the mesh number of the second screen is 11-20 meshes. In this embodiment, after the waste wind turbine blade particles obtained in step S11 are screened by the first screen, the remaining material on the first screen is placed on the second screen, and under the action of the screen, the waste wind turbine blade powder meeting 5-20 meshes, preferably 6-15 meshes, and more preferably 8-11 meshes enters the mixing device 4 through the gaps of the screen.
[0069] In one embodiment, step S1 further comprises: S12, subjecting the waste thermoplastic resin C to crushing treatment by a crushing device 6 to obtain the waste thermoplastic resin particles; the waste thermoplastic resin particles are crushed materials with a size of 0.5 to 2 cm.
[0070] In a preferred embodiment, before the crushing process, the waste thermoplastic resin C is first cleaned in a cleaning device 5 to remove impurities in the waste thermoplastic resin C.
[0071] Step S1 also includes: S13, making the waste wind turbine blade powder, waste thermoplastic resin particles and chemical additives B enter the mixing device 4 for mixing and refining treatment to obtain a mixed material; wherein the addition amount of each material includes: relative to 100 parts by weight of the waste wind turbine blade powder and the waste thermoplastic resin particles, the addition amount of the waste wind turbine blade powder is 20 to 80 parts by weight, preferably 30 to 70 parts by weight, and more preferably 40 to 60 parts by weight; the addition amount of the waste thermoplastic resin particles is 20 to 80 parts by weight, preferably 30 to 70 parts by weight, and more preferably 40 to 60 parts by weight; the addition amount of the silane coupling agent is The addition amount is 1 to 5 parts by weight, preferably 1.5 to 4 parts by weight, and more preferably 1.5 to 3 parts by weight; the addition amount of the lubricant is 1 to 2 parts by weight, preferably 1 to 1.5 parts by weight, and more preferably 1 to 1.25 parts by weight; the addition amount of the colorant is 0.1 to 2 parts by weight, preferably 0.5 to 1 parts by weight, and more preferably 0.5 to 0.8 parts by weight; the addition amount of the flame retardant is 1 to 5 parts by weight, preferably 2 to 4 parts by weight, and more preferably 2 to 3 parts by weight; the addition amount of the plasticizer is 1 to 5 parts by weight, preferably 2 to 4 parts by weight, and more preferably 2 to 3 parts by weight.
[0072] In a specific implementation, relative to 100 parts by weight of the waste wind turbine blade powder and waste thermoplastic resin particles, the added amount of the waste wind turbine blade powder is 50 parts by weight, the added amount of the waste thermoplastic resin particles is 50 parts by weight, the added amount of the silane coupling agent is 2 parts by weight, the added amount of the stearic acid is 1 part by weight, the added amount of the colorant is 0.5 parts by weight, the added amount of the flame retardant is 2 parts by weight, and the added amount of the epoxy resin is 3 parts by weight.
[0073] In one embodiment, the mixing device 4 described in the present disclosure is a conventional choice in the art, and this application does not make any special requirements. For example, the mixing device 4 is a high-speed mixer.
[0074] In one embodiment, the mixing and refining treatment is carried out by a one-pot method, specifically comprising: allowing waste wind turbine blade powder, waste thermoplastic resin particles, silane coupling agent, lubricant, colorant, flame retardant and plasticizer to enter the mixing device 4 for the mixing and refining treatment to obtain the mixed material. Wherein, under the conditions of the mixing and refining treatment, the temperature of the mixing and refining treatment is 80~115°C, preferably 85~110°C; the time is 0.1~0.3h, preferably 0.15~0.25h; the mixing frequency is 20~45Hz, preferably 25~40Hz.
[0075] In this embodiment, waste wind turbine blade powder, waste thermoplastic resin particles and chemical additive B are added to the mixing device 4 for heating, so that the thermoplastic material can be changed from solid to liquid. Under the action of the silane coupling agent, lubricant and plasticizer in the chemical additive B, on the one hand, the use of lubricants and plasticizers can not only improve the softness of the mixed material, thereby improving the convenience of extrusion molding of the mixed material, but also reduce the temperature of solid-liquid conversion of waste wind turbine blade powder and waste thermoplastic resin particles, and improve the difficulty of mixed refining; on the other hand, the silane coupling agent can improve the bonding ability of the glass fiber exposed on the surface of the waste wind turbine blade powder and the thermoplastic resin in the reaction, thereby improving the mechanical properties of the final product. In addition, reacting under the reaction conditions set in the present disclosure can optimize the effect of the mixed refining process, thereby improving the mechanical properties of the final product.
[0076] In another embodiment, the mixing and refining treatment is carried out by a step-by-step method, specifically comprising: allowing the waste wind turbine blade powder, waste thermoplastic resin particles, silane coupling agent, lubricant and part of the plasticizer to enter the mixing device 4 for a first mixing and refining treatment to obtain a first mixed material; allowing another part of the plasticizer, colorant and flame retardant to enter the mixing device 4 and mix with the first mixed material for a second mixing and refining treatment to obtain the mixed material.
[0077] The plasticizers added in the first mixing and refining process and the second mixing and refining process may be the same or different. Preferably, the plasticizers added in the first mixing and refining process and the second mixing and refining process are both dibutyl phthalate.
[0078] In one embodiment, the weight ratio of the plasticizer added in the first mixing and refining process to the plasticizer added in the second mixing and refining process is (1-4):1.
[0079] In one embodiment, under the conditions of the mixing and refining treatment, the temperature of the first mixing and refining treatment is 80-95°C, preferably 85-95°C; the time is 0.1-0.2h, preferably 0.15-0.2h; the mixing frequency is 20-45Hz, preferably 25-40Hz. The temperature of the second mixing and refining treatment is 100-115°C, preferably 105-115°C; the time is 0.1-0.2h, preferably 0.1-0.15h; the mixing frequency is 20-45Hz, preferably 25-40Hz.
[0080] In this embodiment, waste wind turbine blade powder, waste thermoplastic resin particles, silane coupling agent, lubricant and part of plasticizer are first mixed at a relatively low temperature, which can not only reduce the deterioration of lubrication performance caused by volatilization of components in the lubricant at high temperature, but also further enhance the synergistic effect of silane coupling agent, lubricant and plasticizer. Then, another part of plasticizer, colorant and flame retardant are mixed at a relatively high temperature. By adding another part of plasticizer, the mixing effect can be further enhanced, and the mechanical properties of the prepared photovoltaic bracket can be further enhanced.
[0081] In one embodiment, the ratio of the added amounts of the plasticizer, the silane coupling agent and the lubricant is (1-5):(1-2):1, preferably (2-4):(1.5-2):1, and more preferably (2.5-3.5):(1.8-2):1.
[0082] In a specific implementation manner, the ratio of the added amounts of the plasticizer, the silane coupling agent and the lubricant is 3:2:1.
[0083] In one embodiment, the extrusion molding device 8 used in the present disclosure includes an extrusion device and a molding device, wherein the extrusion device and the molding device are conventionally selected in the art, and this application does not make special requirements. For example, the extrusion device is a parallel twin-screw extruder.
[0084] In one embodiment, the temperature used in the melt extrusion process is 160-220°C. Specifically, the temperature of the melt extrusion process includes the extruder barrel temperature and the extruder head temperature, wherein the extruder barrel temperature is 160-205°C, and the extruder head temperature is 200-220°C.
[0085] In one embodiment, the molding method used in the present disclosure is a conventional choice in the art, and this application does not make any special requirements. In this embodiment, the mixed material is squeezed into different molds, and the mixed material is made to fill the entire mold at a hot pressing temperature, and then the molding process is performed in a molding device to obtain different photovoltaic bracket components.
[0086] In one embodiment, the pressure of the molding treatment is 2-50 MPa, preferably 5-40 MPa; the time is 1.5-5 min, preferably 1.8-4 min.
[0087] In one embodiment, the photovoltaic support components obtained through step S2 include photovoltaic support columns, first support diagonal braces, second support diagonal braces, photovoltaic support diagonal beams, and photovoltaic support purlins. The size of the photovoltaic support components is related to the size of the photovoltaic panels installed on the photovoltaic support. For example, the photovoltaic support column disclosed in the present invention has a length of 1.8m, a width of 0.15m, and a thickness of 0.02m; the first support diagonal brace has a length of 2.08m, a width of 0.06m, and a thickness of 0.04m; the second support diagonal brace has a length of 1.554m, a width of 0.05m, and a thickness of 0.04m; the photovoltaic support diagonal beam has a length of 2.3m, a width of 0.09m, and a thickness of 0.03m; the photovoltaic support purlin has a length of 3.3m, a width of 0.09m, and a thickness of 0.03m.
[0088] In one embodiment, step S3 further includes, before assembling the photovoltaic support components, making each photovoltaic support component enter the performance test unit 9 for performance testing, and if the test result shows that the performance of the component is unqualified, the component is scrapped. The standard for the qualified performance test result is to meet all the following conditions: density is 1300kg / m 3 The tensile strength is above 15 MPa, the compressive strength is above 35 MPa, the flexural strength is above 35 MPa, the elastic modulus is above 3 GPa, and the compressive elastic modulus is above 3 GPa.
[0089] In one embodiment, step S3 further includes assembling the photovoltaic support column, the first support diagonal brace, the second support diagonal brace, the photovoltaic support diagonal beam and the photovoltaic support purlin by the assembly unit 10 to obtain the photovoltaic support.
[0090] In one embodiment, if Figure 1 As shown, the method for preparing a photovoltaic support by extruding and reshaping waste wind turbine blades comprises:
[0091] S11, the waste wind turbine blades A are subjected to dust removal treatment by a dust removal device and then enter a blade cutting device 1 for cutting treatment to obtain waste wind turbine blade blocks with a length of 0.5-1.5 m and a width of 0.3-0.6 m; the wind turbine blade blocks are subjected to shredding treatment by a shredding device 2 to obtain waste wind turbine blade particles with a particle size of 1-3 cm; the waste wind turbine blade particles are subjected to pulverizing treatment by a grinding device 3 to obtain waste wind turbine blade powder with a particle size of 5-20 mesh;
[0092] S12, cleaning the waste thermoplastic resin C in the cleaning device 5 and then entering the crushing device 6 for crushing to obtain crushed waste thermoplastic resin particles with a particle size of 0.5-2 cm;
[0093] S13, the waste wind turbine blade powder, waste thermoplastic resin particles and chemical additives B are put into the mixing device 4 for mixing and refining treatment to obtain a mixed material; wherein the chemical additives B include silane coupling agent, lubricant, colorant, flame retardant and plasticizer; the addition amount of each material includes: relative to 100 parts by weight of the waste wind turbine blade powder and waste thermoplastic resin particles, the addition amount of the waste wind turbine blade powder is 20 to 80 parts by weight, and the addition amount of the waste thermoplastic resin particles is 10 to 15 parts by weight. The addition amount is 20-80 parts by weight, the addition amount of the silane coupling agent is 1-5 parts by weight, the addition amount of the lubricant is 1-2 parts by weight, the addition amount of the colorant is 0.1-2 parts by weight, the addition amount of the flame retardant is 1-5 parts by weight, and the addition amount of the plasticizer is 1-5 parts by weight; the temperature of the mixing and refining treatment is 80-115° C.; the weight ratio of the plasticizer, the silane coupling agent and the lubricant is (1-5): (1-2): 1;
[0094] S2, the mixed material is allowed to enter the extrusion molding device 8, and the mixed material is allowed to fill the entire mold at 160-220° C., and then pressed and molded at a pressure of 2-50 MPa for 1.5-5 min, and the mold is cooled to room temperature, and then demolded to obtain photovoltaic support columns, first support diagonal braces, second support diagonal braces, photovoltaic support diagonal beams and photovoltaic support purlins respectively;
[0095] S3. Send the photovoltaic support column, the first support diagonal brace, the second support diagonal brace, the photovoltaic support diagonal beam and the photovoltaic support purlin to the performance testing unit 9 for performance testing. If the test result is qualified, the above-mentioned photovoltaic support components are sent to the assembly unit 10 for assembly to obtain the photovoltaic support. If the test result is unqualified, the component is re-prepared.
[0096] The present disclosure is further described below by way of examples, but the present disclosure is not limited thereby. Unless otherwise specified, the compounds used in the following examples and comparative examples are all purchased pharmaceutical reagents.
[0097] Example 1
[0098] like Figure 1 As shown, the method for preparing a photovoltaic support by extruding and reshaping waste wind turbine blades comprises:
[0099] S11, the waste wind turbine blade A is subjected to dust removal treatment by a dust removal device and then enters a blade cutting device 1 for cutting treatment to obtain waste wind turbine blade blocks with a length of 1 m and a width of 0.5 m; the wind turbine blade blocks are subjected to shredding treatment by a shredding device 2 to obtain waste wind turbine blade particles with a particle size of 2 cm; the waste wind turbine blade particles are subjected to pulverizing treatment by a grinding device 3 to obtain waste wind turbine blade powder with a particle size of 10 mesh;
[0100] S12, cleaning the waste thermoplastic resin C in the cleaning device 5 and then entering the crushing device 6 for crushing to obtain crushed waste thermoplastic resin particles with a particle size of 1 cm;
[0101] S13, using a one-pot method, 50 parts by weight of waste wind turbine blade powder, 50 parts by weight of waste thermoplastic resin particles (a composition of polyethylene and polypropylene), 2 parts by weight of silane coupling agent (70wt% of A171, 10wt% of KH-570 and 20wt% of KH-560), 1 part by weight of lubricant (a composition of 20wt% of stearic acid, 50wt% of methyl stearate and 30wt% of capric amide), 0.5 parts by weight of colorant (phthalocyanine blue), 2 parts by weight of flame retardant (antimony trioxide) and 3 parts by weight of plasticizer (dibutyl phthalate) are introduced into a mixing device 4 for mixing and refining treatment to obtain a mixed material; the mixing and refining treatment temperature is 105°C, the time is 0.3h, and the mixing frequency is 30Hz;
[0102] S2, sending the mixed material into the extrusion molding device 8 for melt extrusion treatment, sending it into different molds of the molding device for molding treatment, and making the mixed material fill the entire mold at 200°C, and then pressing and molding it at a pressure of 10MPa for 3min, and cooling the above mold to room temperature to obtain photovoltaic support columns, first support diagonal braces, second support diagonal braces, photovoltaic support diagonal beams and photovoltaic support purlins; wherein, the length of the photovoltaic support column is 1.8m, the width is 0.15m, and the thickness is 0.02m; the length of the first support diagonal brace is 2.08m, the width is 0.06m, and the thickness is 0.04m; the length of the second support diagonal brace is 1.554m, the width is 0.05m, and the thickness is 0.04m; the length of the photovoltaic support diagonal beam is 2.3m, the width is 0.09m, and the thickness is 0.03m; the length of the photovoltaic support purlin is 3.3m, the width is 0.09m, and the thickness is 0.03m;
[0103] S3. Send the photovoltaic support column, the first support diagonal brace, the second support diagonal brace, the photovoltaic support diagonal beam and the photovoltaic support purlin to the performance testing unit 9 for performance testing. If the test result is qualified, assemble the above-mentioned photovoltaic support components through the assembly unit 10 to obtain a photovoltaic support. If the test result is unqualified, re-prepare the assembly.
[0104] Example 2
[0105] The method for preparing a photovoltaic bracket by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that 30 parts by weight of waste wind turbine blade powder, 70 parts by weight of waste thermoplastic resin particles, 2 parts by weight of silane coupling agent, 1 part by weight of lubricant, 0.5 parts by weight of colorant, 2 parts by weight of flame retardant and 3 parts by weight of plasticizer (dibutyl phthalate) are introduced into a mixing device 4 for mixing and refining treatment to obtain a mixed material.
[0106] Example 3
[0107] The method for preparing a photovoltaic support by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that the particle size of the waste wind turbine blade powder is 20 mesh.
[0108] Example 4
[0109] The method for preparing a photovoltaic bracket by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that 60 parts by weight of waste wind turbine blade powder, 40 parts by weight of waste thermoplastic resin particles, 4 parts by weight of silane coupling agent, 2 parts by weight of lubricant, 2 parts by weight of colorant, 4 parts by weight of flame retardant and 5 parts by weight of plasticizer (dibutyl phthalate) are introduced into a mixing device 4 for mixing and refining treatment to obtain a mixed material.
[0110] Example 5
[0111] The method for preparing a photovoltaic support by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that the silane coupling agent is composed of a combination of 65wt% A171, 10wt% KH-570 and 25wt% KH-560.
[0112] Example 6
[0113] The method for preparing a photovoltaic support by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that the lubricant is composed of a composition of 30 wt % of stearic acid, 20 wt % of methyl stearate and 50 wt % of capric amide.
[0114] Example 7
[0115] The method for preparing a photovoltaic bracket by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that step S13 comprises: 50 parts by weight of waste wind turbine blade powder, 50 parts by weight of waste thermoplastic resin particles (a composition of polyethylene and polypropylene), 2 parts by weight of silane coupling agent, 1 part by weight of lubricant and 2 parts by weight of first plasticizer (dibutyl phthalate) are introduced into a mixing device 4 for a first mixing and refining treatment to obtain a first mixed material; the temperature of the first mixing and refining treatment is 90° C., the time is 0.15, and the mixing frequency is 30 Hz;
[0116] 1 part by weight of the second plasticizer (dibutyl phthalate), 0.5 parts by weight of the colorant and 2 parts by weight of the flame retardant are introduced into the mixing device 4 and mixed with the first mixed material for a second mixing and refining treatment to obtain the mixed material; the temperature of the second mixing and refining treatment is 105°C, the time is 0.15, and the mixing frequency is 30Hz.
[0117] Comparative Example 1
[0118] The method for preparing a photovoltaic bracket by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that 10 parts by weight of waste wind turbine blade powder, 90 parts by weight of waste thermoplastic resin particles (polyethylene), 6 parts by weight of silane coupling agent, 0.5 parts by weight of lubricant, 3 parts by weight of colorant, 6 parts by weight of flame retardant and 6 parts by weight of plasticizer (dibutyl phthalate) are introduced into a mixing device 4 for mixing and refining treatment to obtain a mixed material.
[0119] Comparative Example 2
[0120] The method for preparing a photovoltaic support by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that the chemical auxiliary agent B does not contain a plasticizer (dibutyl phthalate).
[0121] Comparative Example 3
[0122] The method for preparing a photovoltaic support by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that the particle size of the waste wind turbine blade powder is 2 mesh.
[0123] Comparative Example 4
[0124] The method for preparing a photovoltaic bracket by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that 50 parts by weight of waste wind turbine blade powder, 50 parts by weight of waste thermoplastic resin particles, 0.5 parts by weight of a silane coupling agent, 2 parts by weight of a lubricant, 0.5 parts by weight of a colorant, 2 parts by weight of a flame retardant and 5 parts by weight of a plasticizer (dibutyl phthalate) are introduced into a mixing device 4 for mixing and refining treatment to obtain a mixed material.
[0125] Comparative Example 5
[0126] The method for preparing a photovoltaic bracket by extruding and reshaping waste wind turbine blades is the same as that in Example 1, except that 50 parts by weight of waste wind turbine blade powder, 50 parts by weight of waste thermoplastic resin particles, 1.5 parts by weight of silane coupling agent, 1 part by weight of lubricant, 0.5 parts by weight of colorant, 2 parts by weight of flame retardant and 6 parts by weight of plasticizer (dibutyl phthalate) are introduced into a mixing device 4 for mixing and refining treatment to obtain a mixed material.
[0127] Test Case
[0128] The photovoltaic bracket components prepared in Examples 1 to 7 and Comparative Examples 1 to 5 were subjected to performance tests. The indicators of qualified products included density of 1300 kg / m 3 The test methods include:
[0129] 1. The tensile strength of the photovoltaic bracket components prepared in the embodiments and comparative examples was tested according to the provisions of the national standard GB / T 1040-2018 "Determination of tensile properties of plastics". The test results are shown in Table 1;
[0130] 2. The compressive strength of the photovoltaic bracket components prepared in the embodiment and the comparative example was tested according to the provisions of the national standard GB / T 1040-2008 "Determination of the compressive properties of plastics". The test results are shown in Table 1.
[0131] 3. The bending strength of the photovoltaic bracket components prepared in the embodiment and the comparative example was evaluated by using the provisions of the national standard GB / T 9341-2008 "Determination of Bending Properties of Plastics". The test results are shown in Table 1;
[0132] 4. The elastic modulus of the photovoltaic bracket components prepared in the embodiment and the comparative example was tested according to the provisions of the national standard GB / T 1040-2018 "Determination of tensile properties of plastics". The test results are shown in Table 1;
[0133] 5. The compressive elastic modulus of the photovoltaic support components prepared in the examples and comparative examples was tested according to the national standard GB / T 1040-2008 "Determination of compression properties of plastics". The test results are shown in Table 1.
[0134] Table 1 Performance of photovoltaic bracket components
[0135]
[0136] As shown in Table 1, based on the comparison of the data in Examples 1 to 7 and Comparative Examples 1 to 5, it can be seen that the raw materials of the photovoltaic bracket prepared by the present disclosure contain waste wind turbine blade powder with a smaller particle size, which can achieve the cascade utilization and harmless disposal of waste wind turbine blades and waste thermoplastic resins, reduce the risk of environmental pollution and disposal costs, and thus improve economic benefits. Moreover, under the action of silane coupling agent and epoxy resin, the coupling effect of waste wind turbine blade powder and waste thermoplastic resin particles is good, and a photovoltaic bracket with mechanical properties that meet the requirements of photovoltaic equipment can be obtained. In addition, under the action of stearic acid and flame retardant, the obtained photovoltaic bracket can have good cold resistance and flame resistance.
[0137] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0138] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0139] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A photovoltaic support made of extruded and reshaped materials from waste wind turbine blades, characterized in that: The raw materials for preparing the photovoltaic bracket include waste wind turbine blade powder, waste thermoplastic resin particles and chemical additives; the particle size of the waste wind turbine blade powder is 5-20 mesh; The chemical additives include silane coupling agents, lubricants, colorants, flame retardants and plasticizers; Relative to 100 parts by weight of the waste wind turbine blade powder and the waste thermoplastic resin particles, the content of the waste wind turbine blade powder is 20 to 80 parts by weight, the content of the waste thermoplastic resin particles is 20 to 80 parts by weight, the content of the silane coupling agent is 1 to 5 parts by weight, the content of the lubricant is 1 to 2 parts by weight, the content of the colorant is 0.1 to 2 parts by weight, the content of the flame retardant is 1 to 5 parts by weight, and the content of the plasticizer is 1 to 5 parts by weight; The weight ratio of the plasticizer, the silane coupling agent and the lubricant is (1-5):(1-2):
1.
2. The photovoltaic bracket according to claim 1, characterized in that: The particle size of the waste wind turbine blade powder is 6-15 mesh.
3. The photovoltaic bracket according to claim 1, characterized in that: The waste thermoplastic resin particles are crushed materials with a particle size of 0.5-2 cm; The waste thermoplastic resin particles include one or more of polyethylene, polypropylene, polyvinyl chloride and polystyrene.
4. The photovoltaic bracket according to claim 1, characterized in that: The silane coupling agent includes vinyl silane coupling agent, methacryloxy silane coupling agent and epoxy silane coupling agent; The lubricant includes one or more of stearic acid, methyl stearate and capric amide; The colorant includes one or more of chrome yellow, cadmium red and phthalocyanine blue; The flame retardant includes antimony trioxide and / or ammonium polyphosphate; The plasticizer is dibutyl phthalate.
5. The photovoltaic support according to claim 4, characterized in that: The weight ratio of the total weight of the vinyl silane coupling agent and the methacryloxy silane coupling agent to the epoxy silane coupling agent is (4-7):1; The lubricant is a composition of stearic acid, methyl stearate and capric amide; the weight ratio of stearic acid, methyl stearate and capric amide is (1.5-2): (5-6): (2.5-3).
6. The photovoltaic support according to claim 1, characterized in that: Relative to 100 parts by weight of the waste wind turbine blade powder and the waste thermoplastic resin particles, the content of the waste wind turbine blade powder is 30 to 70 parts by weight, the content of the waste thermoplastic resin particles is 30 to 70 parts by weight, the content of the silane coupling agent is 1.5 to 4 parts by weight, the content of the lubricant is 1 to 1.5 parts by weight, the content of the colorant is 0.5 to 1 part by weight, the content of the flame retardant is 2 to 4 parts by weight, and the content of the plasticizer is 2 to 4 parts by weight.
7. The photovoltaic support according to claim 1, characterized in that: The weight ratio of the plasticizer, the silane coupling agent and the lubricant is (2-4):(1.5-2):
1.
8. A method for preparing photovoltaic brackets by extruding and reshaping waste wind turbine blades, characterized in that: The method includes: S1, putting waste wind turbine blade powder, waste thermoplastic resin particles and chemical additives into a mixing device for mixing and refining to obtain a mixed material; The chemical additives include silane coupling agents, lubricants, colorants, flame retardants and plasticizers; The particle size of the waste wind turbine blade powder is 5-20 mesh; Relative to 100 parts by weight of the waste wind turbine blade powder and the waste thermoplastic resin particles, the added amount of the waste wind turbine blade powder is 20 to 80 parts by weight, the added amount of the waste thermoplastic resin particles is 20 to 80 parts by weight, the added amount of the silane coupling agent is 1 to 5 parts by weight, the added amount of the lubricant is 1 to 2 parts by weight, the added amount of the colorant is 0.1 to 2 parts by weight, the added amount of the flame retardant is 1 to 5 parts by weight, and the added amount of the plasticizer is 1 to 5 parts by weight; The weight ratio of the plasticizer, the silane coupling agent and the lubricant is (1-5): (1-2): 1; S2, allowing the mixed material to enter an extrusion molding device for melt extrusion and molding to obtain a photovoltaic support component; S3, assembling the photovoltaic support components to obtain a photovoltaic support.
9. The method according to claim 8, characterized in that Step S1 also includes: The waste wind turbine blade powder, the waste thermoplastic resin particles, the silane coupling agent, the lubricant and part of the plasticizer are put into a mixing device for a first mixing and refining treatment to obtain a first mixed material; another part of the plasticizer, the colorant and the flame retardant are put into the mixing device for mixing with the first mixed material for a second mixing and refining treatment to obtain the mixed material; The weight ratio of the plasticizer added in the first mixing and refining process to the plasticizer added in the second mixing and refining process is (1-4):
1.
10. The method according to claim 9, characterized in that The mixing and refining process is carried out at a temperature of 80-115°C and a time of 0.1-0.3h; The temperature of the first mixing and refining treatment is 80-95°C and the time is 0.1-0.2h; The temperature of the second mixing and refining treatment is 100-115°C and the time is 0.1-0.2h; The temperature used in the melt extrusion process is 160-220° C., the pressure used in the molding process is 2-50 MPa, and the time is 1.5-5 min.
Citation Information
Patent Citations
Reinforced resin-plastic compound plate prepared from waste printed circuit board (PCB) powder and preparation method thereof
CN103834100A
Wood-imitating profile prepared through glass fiber reinforced plastic waste regeneration and preparation process thereof
CN106220956A