Degradable plastic particles for making ground film and production method thereof

By coating UV absorbers and branched polysilanol additives with zein, a three-dimensional network structure is formed, which solves the mechanical properties and water resistance problems of the degradable mulch film, and achieves the long-term stability and anti-UV aging effect of the mulch film.

CN118165476BActive Publication Date: 2024-10-08SHANDONG BLUE OCEAN CRYSTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410348680.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-10-08
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

When existing degradable mulch films are compounded with aliphatic polyester and starch, they have poor mechanical properties, poor water resistance and are prone to UV aging.

Method used

Zein is used to coat UV absorbers and branched polysilanol additives to form coated UV absorbers and three-dimensional network structures to improve the mechanical properties and water resistance of plastic particles.

Benefits of technology

It achieves long-term stability of plastic particles, avoids UV aging and performance degradation, and improves the service life and water resistance of the mulch film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118165476B_ABST
    Figure CN118165476B_ABST
Patent Text Reader

Abstract

The invention relates to the field of plastic technology, and discloses a degradable plastic particle for making a ground film and a production method thereof. The degradable plastic particle is made of starch and aliphatic polyester as main raw materials, and auxiliary materials such as a coated ultraviolet absorber and a branched polysilicone additive are blended and melt-extruded to form a three-dimensional network with the aliphatic polyester and starch by adding the branched polysilicone additive, thereby improving the mechanical properties of the plastic. At the same time, the coated ultraviolet absorber can be fixed in the plastic particle through the confinement effect, thereby effectively avoiding the problem that the coated ultraviolet absorber cannot be used due to shedding, and then utilizing the sustained-release effect of the coated ultraviolet absorber on the ultraviolet absorber, so that the ground film can maintain its own performance under long-term outdoor use conditions, thereby maintaining a good service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastics, and in particular to degradable plastic particles for making ground films and a production method thereof. Background Art

[0002] As global environmental problems become increasingly serious, environmental protection concepts have gradually gained popularity, and all walks of life are striving to explore the path of sustainable development. As the foundation of the national economy, agriculture has attracted much attention for its environmental protection issues. In agricultural production, mulch films, as an important agricultural production material, are widely used to increase soil temperature, maintain soil moisture, and inhibit weed growth. However, traditional mulch films are mostly made of non-degradable materials such as polyethylene, which are difficult to degrade after use, causing serious pollution to the soil and ecological environment. Therefore, the research, development and promotion of degradable mulch films are of great significance to promoting green agricultural development and protecting the ecological environment.

[0003] At present, degradable mulch films are mainly made of aliphatic polyesters as the main raw materials, such as polybutylene succinate, etc. Since its structure contains both rigid links and flexible links, it can show good mechanical properties. However, the price of aliphatic polyesters is relatively high, so other ingredients are often added to reduce the amount of polyester to achieve the purpose of controlling costs. Starch is a biomass material. Mixing it with aliphatic polyesters can reduce costs without changing its degradability. However, the chemical structure of aliphatic polyesters makes it difficult to merge with starch. They may age after being exposed to sunlight for a long time and separate from each other, causing the water resistance and mechanical properties of the mulch to decrease sharply. Therefore, the use of starch and aliphatic polyesters to make mulch films still has defects in practical applications.

[0004] Based on this, the present invention provides a degradable plastic particle that can solve the above technical problems. Summary of the invention

[0005] The purpose of the present invention is to provide a degradable plastic particle for making ground film and a production method thereof, which solves the problems that the ground film made by compounding aliphatic polyester and starch has poor mechanical properties, poor water resistance and is prone to ultraviolet aging.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A degradable plastic particle for making ground film, comprising the following components by weight:

[0008]

[0009] Furthermore, the aliphatic polyester is at least one of polybutylene succinate, polybutylene terephthalate or polybutylene succinate / adipate; and the filler is at least one of calcium carbonate, talc or silica powder.

[0010] Furthermore, the preparation method of the coated ultraviolet absorber is as follows:

[0011] Step A, mixing zein with an ethanol aqueous solution, and mechanically stirring at a stirring rate of 300-500 r / min until the mixture is uniformly dissolved to obtain a protein solution with a mass fraction of 20-30%;

[0012] Specifically, the applicant discovered during a large number of experiments that zein is insoluble in water or ethanol, but has excellent solubility in 60-80% ethanol aqueous solution. Therefore, ethanol aqueous solution was used as a good solvent to prepare a zein solution.

[0013] Step B, controlling the stirring rate to 100-200 r / min, adding the ultraviolet absorber to the protein solution under stirring, and continuing to stir after the addition. After a uniform solution is formed, controlling the stirring rate to 500-1000 r / min, adding the uniform solution to deionized water under continuous stirring, controlling the dropping rate to 5-15 mL / min, and placing it for 1-2 hours, and then performing reduced pressure concentration and freeze drying to obtain a coated ultraviolet absorber.

[0014] Specifically, the ultraviolet absorber cannot be dissolved in water, but can be dissolved in ethanol. When the uniform solution is added to deionized water, the water content in the solution increases rapidly, causing the zein and the ultraviolet absorber to precipitate rapidly. Since zein is amphiphilic, under such conditions, the hydrophilic groups of the zein will be outward and the hydrophobic groups will be inward, resulting in a chamber-like structure with internal hydrophobicity and external hydrophilicity. The hydrophobic ultraviolet absorber that is also precipitated will enter the chamber, prompting the zein to complete the encapsulation of the ultraviolet absorber, and finally forming a coated ultraviolet absorber.

[0015] Furthermore, in step A, the volume fraction of the ethanol aqueous solution is 60-80%.

[0016] Furthermore, in step B, the ultraviolet absorber is any one of a salicylate ultraviolet absorber or a benzophenone ultraviolet absorber.

[0017] Furthermore, in step B, the volume ratio of the homogeneous solution to deionized water is 1:3-4.

[0018] Furthermore, the preparation method of the branched polysilanol additive is as follows:

[0019] Add polycaprolactone triol, 3-glycidyloxypropyl-terminated dimethylpolysiloxane mixture and toluene into a reaction kettle, start stirring, mix the materials evenly, fill with nitrogen to exclude oxygen, then add a phase transfer catalyst into the reaction kettle, heat, and when the temperature reaches 70-80°C, keep warm and stir for 8-12 hours, remove the solvent under reduced pressure, separate the materials, and obtain a branched polysilanol additive.

[0020] Specifically, under the action of a phase transfer catalyst, the terminal hydroxyl group of polycaprolactone triol will undergo ring opening with the epoxy substituent in the 3-glycidyloxypropyl-terminated dimethylpolysiloxane structure, and gradually branch and polymerize to ultimately form a branched polysilanol additive with polysiloxane as a bridging agent.

[0021] Furthermore, the number average molecular weight of the polycaprolactone triol is 550; and the number average molecular weight of the 3-glycidyloxypropyl terminated dimethylpolysiloxane is 1000.

[0022] Furthermore, the phase transfer catalyst is any one of tetramethylammonium bromide, tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate or boron trifluoride ether complex.

[0023] A method for producing degradable plastic particles for making ground film comprises the following steps:

[0024] Step 1: Weigh each raw material according to weight and set aside;

[0025] Step 2: Put all raw materials into a stirring kettle, and mechanically stir and mix them at a stirring speed of 1000-2000 r / min for 5-10 minutes to form a pre-feed;

[0026] Step 3: Pass the pre-material through the feeder into the twin-screw extruder, set the extrusion temperature to 150-200°C and the screw speed to 100-200rpm, perform melt extrusion, and after natural cooling, use a pelletizer to pelletize to obtain biodegradable plastic particles.

[0027] Beneficial effects of the present invention:

[0028] (1) The present invention uses zein to coat the UV absorber to form a coated UV absorber. After the small molecule UV absorber is coated, it can effectively avoid volatilization, so that the UV absorber can exist in the plastic particles for a long time. Moreover, this coating structure can achieve the sustained release of the small molecule UV absorber. Therefore, during the use of the mulch film, the UV absorber can be continuously released, so that the mulch film can maintain its own performance under long-term outdoor use conditions, thereby maintaining a good service life.

[0029] (2) The branched polysilanol additive prepared by the present invention has a hyperbranched structure, and the branch chain contains a large number of substituted hydroxyl groups generated by ring opening. From a microscopic perspective, this structure can simultaneously form hydrogen bonds with aliphatic polyesters and starch, so that the branch chains of the branched polysilanol additive are highly entangled with the molecular chains of aliphatic polyesters and starch to form a tightly connected three-dimensional network structure. In other words, the addition of the branched polysilanol additive can play a transitional effect, realize the mutual fusion of materials, and form a homogeneous mixture, thereby avoiding phase separation and causing a sharp decrease in the mechanical properties of the plastic. In addition, a higher cross-linking density will make the plastic more compact, and the hydrophobic siloxy bonds in the branched polysilanol additive will make the plastic exhibit stronger water resistance.

[0030] (3) The present invention forms a three-dimensional network with aliphatic polyester and starch by adding a branched polysilicone additive, and can fix the coated ultraviolet absorber in the plastic particles through the confinement effect, thereby effectively avoiding the problem of the coated ultraviolet absorber falling off and failing to exert its effect.

[0031] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0033] Figure 1 This is an infrared analysis test chart of the branched polysilanol additive of the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] A degradable plastic particle for making ground film, comprising the following components by weight:

[0037]

[0038] The method for preparing the plastic particles comprises the following steps:

[0039] Step 1: weigh each raw material according to weight and set aside;

[0040] Step 2: Put all raw materials into a stirring kettle, and mechanically stir and mix them at a stirring speed of 1000 r / min for 10 minutes to form a pre-mixed material;

[0041] Step 3: Pass the pre-material through the feeder into the twin-screw extruder, set the extrusion temperature to 150°C and the screw speed to 100rpm, perform melt extrusion, and after natural cooling, use a pelletizer to pelletize to obtain biodegradable plastic particles.

[0042] Example 2

[0043] A degradable plastic particle for making ground film, comprising the following components by weight:

[0044]

[0045] The method for preparing the plastic particles comprises the following steps:

[0046] Step 1: Weigh each raw material according to weight and set aside;

[0047] Step 2: Put all the raw materials into a stirring kettle, and mechanically stir and mix them at a stirring speed of 1500r / min for 6 minutes to form a pre-mixed material;

[0048] Step 3: Pass the pre-material through the feeder into the twin-screw extruder, set the extrusion temperature to 160°C and the screw speed to 150rpm, perform melt extrusion, and after natural cooling, use a pelletizer to pelletize to obtain biodegradable plastic particles.

[0049] Example 3

[0050] A degradable plastic particle for making ground film, comprising the following components by weight:

[0051]

[0052] The method for preparing the plastic particles comprises the following steps:

[0053] Step 1: Weigh each raw material according to weight and set aside;

[0054] Step 2: Put all raw materials into a stirring kettle, and mechanically stir and mix them at a stirring speed of 2000 r / min for 5 minutes to form a pre-mixed material;

[0055] Step 3: Pass the pre-material through the feeder into the twin-screw extruder, set the extrusion temperature to 180°C and the screw speed to 200rpm, perform melt extrusion, and after natural cooling, use a pelletizer to pelletize to obtain biodegradable plastic particles.

[0056] Comparative Example 1

[0057] A degradable plastic particle for making ground film, comprising the following components by weight:

[0058]

[0059]

[0060] The method for preparing the plastic particles comprises the following steps:

[0061] Step 1: Weigh each raw material according to weight and set aside;

[0062] Step 2: Put all the raw materials into a stirring kettle, and mechanically stir and mix them at a stirring speed of 1500r / min for 6 minutes to form a pre-mixed material;

[0063] Step 3: Pass the pre-material through the feeder into the twin-screw extruder, set the extrusion temperature to 160°C and the screw speed to 150rpm, perform melt extrusion, and after natural cooling, use a pelletizer to pelletize to obtain biodegradable plastic particles.

[0064] Comparative Example 2

[0065] A degradable plastic particle for making ground film, comprising the following components by weight:

[0066]

[0067] The method for preparing the plastic particles comprises the following steps:

[0068] Step 1: Weigh each raw material according to weight and set aside;

[0069] Step 2: Put all the raw materials into a stirring kettle, and mechanically stir and mix them at a stirring speed of 1500r / min for 6 minutes to form a pre-mixed material;

[0070] Step 3: Pass the pre-material through the feeder into the twin-screw extruder, set the extrusion temperature to 160°C and the screw speed to 150rpm, perform melt extrusion, and after natural cooling, use a pelletizer to pelletize to obtain biodegradable plastic particles.

[0071] The preparation method of the coated ultraviolet absorber used in the above examples and comparative examples is as follows:

[0072] Step A, mixing 2.5 g of zein with an ethanol aqueous solution having a volume fraction of 80%, and mechanically stirring until the solution is uniformly dissolved to obtain a protein solution having a mass fraction of 25%;

[0073] Step B, controlling the stirring rate to 15 r / min, adding 1.8 g of phenyl o-hydroxybenzoate to the protein solution under stirring, and continuing to stir after the addition. After a uniform solution is formed, the stirring rate is controlled to 1000 r / min, and 30 mL of the uniform solution is added to 100 mL of deionized water under continuous stirring. The dropping rate is controlled to 6 mL / min. After standing for 2 hours, the solution is concentrated under reduced pressure and freeze-dried to obtain a coated ultraviolet absorber.

[0074] The preparation method of the branched polysilanol additive used in the above examples and comparative examples is as follows:

[0075] Add 1.6 g of polycaprolactone triol with a number average molecular weight of 550, 4.5 g of 3-glycidyloxypropyl-terminated dimethylpolysiloxane with a number average molecular weight of 1000 and toluene into the reactor, start stirring, mix the materials evenly, fill with nitrogen to exclude oxygen, and then add 0.3 g of boron trifluoride ether complex to the reactor, heat, and when the temperature reaches 75°C, stir and keep warm for 9 hours, remove the solvent under reduced pressure, separate the materials, and obtain a branched polysilanol additive.

[0076] Figure 1 This is the infrared test image of the branched polysilanol additive, where 3342 cm -1 The OH stretching vibration peak of the hydroxyl group appears at 1739 cm -1 The C=O stretching vibration peak of the ester group appears at 1103 cm -1 and 1032cm -1 Overlapping characteristic absorption peaks of ether bonds and siloxy bonds appeared at the positions respectively. Since polycaprolactone triol and 3-glycidyloxypropyl-terminated dimethylpolysiloxane do not contain ether bonds, it can be inferred that the hydroxyl groups in polycaprolactone triol and the epoxy substituents in 3-glycidyloxypropyl-terminated dimethylpolysiloxane underwent ring opening to produce a large number of substituted hydroxyl groups and ether bonds.

[0077] Test Case

[0078] The plastic particles in Examples 1 to 3 of the present invention and Comparative Example 2 were injection molded into standard tensile specimens and the following tests were performed:

[0079] a. According to the standard GB / T 1040.3-2006, the tensile properties were tested. After the test was completed, the test specimens were collected and placed for 60 days. Then, 300 mJ / cm 2The specimens were irradiated with a mercury lamp for 12 hours, and the tensile properties of the specimens were tested again;

[0080] b. According to the standard GB / T 1034-2008, the water absorption rate of the test specimens after immersion in water for 24 hours;

[0081] The test results are shown in Table 1:

[0082] Table 1 - Test results

[0083]

[0084] The analysis results show that the plastic particles prepared using coated UV absorbers and branched polysilicone additives as modifiers have excellent mechanical properties, good resistance to UV aging, can be used outdoors for a long time, and have good water resistance.

[0085] In Comparative Example 1, a small molecule UV absorber is directly used to modify the aliphatic polyester. Due to the continuous volatilization during the storage process, the tensile strength decreases significantly after 60 days, so the anti-ultraviolet aging effect is poor.

[0086] The plastic particles in Comparative Example 2 do not contain branched polysilicone additives, so a three-dimensional network structure cannot be formed. The bonding force between starch and aliphatic polyester is weak, resulting in poor mechanical properties. In addition, the confinement effect of the three-dimensional network cannot be utilized to effectively load the coated UV absorber, resulting in the shedding of the coated UV absorber, resulting in poor anti-UV aging performance.

[0087] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

[0088] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A degradable plastic particle for making ground film, It is characterized in that By weight, it includes the following components: 30-45 parts of starch; Aliphatic polyester 40-50 parts; 0.5-1.5 parts of coated UV absorber; 2-4.5 parts of branched polysilanol additive; 1-5 parts of filler; The preparation method of the coated ultraviolet absorber is as follows: Step A, mixing zein with an ethanol aqueous solution, and mechanically stirring until the zein is uniformly dissolved to obtain a protein solution with a mass fraction of 20-30%; Step B, controlling the stirring rate to 100-200 r / min, adding the ultraviolet absorber to the protein solution under stirring, and continuing to stir after the addition. After a uniform solution is formed, controlling the stirring rate to 500-1000 r / min, adding the uniform solution to deionized water under continuous stirring, controlling the drop rate to 5-15 mL / min, leaving it for 1-2 hours, and then performing reduced pressure concentration and freeze drying to obtain a coated ultraviolet absorber; The preparation method of the branched polysilanol additive is as follows: The polycaprolactone triol and 3-glycidyloxypropyl-terminated dimethylpolysiloxane are mixed, chain extension and branching are carried out in the presence of toluene solvent and phase transfer catalyst, the solvent is removed under reduced pressure after 8-12 hours, and the material is separated to obtain a branched polysilanol additive.

2. The degradable plastic particles for making ground film according to claim 1, It is characterized in that The aliphatic polyester is polybutylene succinate or polybutylene succinate / adipate; the filler is at least one of calcium carbonate, talc or silica powder.

3. The degradable plastic particles for making ground film according to claim 1, It is characterized in that In step A, the volume fraction of the ethanol aqueous solution is 60-80%.

4. The degradable plastic particles for making ground film according to claim 1, It is characterized in that In step B, the ultraviolet absorber is any one of a salicylate ultraviolet absorber or a benzophenone ultraviolet absorber.

5. The degradable plastic particles for making ground film according to claim 1, It is characterized in that In step B, the volume ratio of the homogeneous solution to deionized water is 1:3-4.

6. The degradable plastic particles for making ground film according to claim 1, It is characterized in that The number average molecular weight of the polycaprolactone triol is 550; the number average molecular weight of the 3-glycidyloxypropyl-terminated dimethylpolysiloxane is 1000.

7. The degradable plastic particles for making ground film according to claim 1, It is characterized in that The phase transfer catalyst is any one of tetramethylammonium bromide, tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate or boron trifluoride ether complex.

8. A method for producing degradable plastic particles for making ground film as claimed in claim 1, It is characterized in that The following steps are involved: Step 1: Weigh each raw material according to weight and set aside; Step 2: Put all raw materials into a stirring kettle, and mechanically stir and mix them at a stirring speed of 1000-2000 r / min for 5-10 minutes to form a pre-feed; Step 3: Pass the pre-material through the feeder into the twin-screw extruder, set the extrusion temperature to 150-200°C and the screw speed to 100-200rpm, perform melt extrusion, and after natural cooling, use a pelletizer to pelletize to obtain biodegradable plastic particles.