12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod and its manufacturing method
Through the chemical composition of C-Si-Mn-Cr and molten salt ultra-fast cold quenching technology, a multi-phase structure is formed, which solves the problem of annealing-free cold heading steel wire rods in the manufacturing of grade 12.9 fasteners, and achieves high efficiency and low cost. High-strength fasteners are manufactured to improve cold working performance and avoid the risk of breakage.
Patent Information
- Application Number
- CN202410607547.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-16
AI Technical Summary
In the current manufacturing process of grade 12.9 ultra-high strength fasteners, it is difficult to achieve anneal-free cold heading steel wire rods, resulting in long production cycles, high costs, high energy consumption, poor cold working performance, and prone to work hardening and cold heading cracking problems. .
The low-hardenability chemical composition design of C-Si-Mn-Cr is used, combined with molten salt ultra-fast cold quenching and isothermal technology to promote the transformation of austenite structure into bainite and martensite, and return to normal temperature through online molten salt heating. The slow cooling of the fire and roller forms a complex phase structure dominated by tempered bainite and supplemented by quasi-spheroidized carbides, which improves the hardenability and plasticity of the steel.
It achieves efficient green manufacturing of 12.9-level anneal-free high-strength fasteners, reduces material costs, improves cold working performance, and avoids fracture problems caused by hard and brittle phases. It is suitable for manufacturing high-strength fastener bolts and other application fields.
Smart Images

Figure CN118166189B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cold heading steel hot rolled wire rods, and in particular relates to a 12.9 grade annealing-free hot rolled complex phase cold heading steel wire rod and a manufacturing method thereof. Background Art
[0002] Ultra-high strength fasteners of grade 12.9 and above are usually made of medium carbon, high hardenability such as Mn, Cr and precious metal alloy component systems such as Mo, V, Nb. Due to the high alloy content, the raw material hot-rolled wire rod needs to be processed and manufactured in the fastener factory in sequence through spheroidizing annealing, drawing, spheroidizing annealing, drawing, cold heading and other processes. The purpose of the spheroidizing annealing process is to soften the structure to improve the drawing and cold heading performance, and reduce the risk of wire breakage and cold heading cracking of the wire rod. Since spheroidizing annealing often undergoes 10 to 24 hours of high-temperature heat treatment at 750 to 780°C, not only the production cycle is long, but also the manufacturing cost is increased and the energy consumption is high. Therefore, it is necessary to develop a 12.9 grade annealing-free hot-rolled cold heading steel wire rod to achieve efficient and green manufacturing of ultra-high strength fastener bolts. The technical difficulties and causes of the hot-rolled cold heading steel wire rod in the existing technology that are difficult to meet the manufacturing and application requirements of 12.9 grade annealing-free fasteners are:
[0003] (1) The addition of alloying elements can improve the hardenability of steel and improve the mechanical properties of fasteners through overall strengthening. For example, Cr helps to improve the strength grade of bolts, but it will reduce the cold working performance of wire rods, which is prone to work hardening and cold heading cracking. At the same time, the addition of high alloying elements increases the material cost of cold heading steel wire rods. On this basis, cold heading steel wire rods are mainly manufactured by Stelmore air cooling wire after spinning. Due to the limited cooling capacity of the Stelmore air cooling wire, the high hardenability components aggravate the production of martensite and bainite hard and brittle phases under strong air cooling conditions, which in turn causes the wire rod to have an increased range, plastic deterioration and the risk of cold heading cracking. Therefore, the process of reducing the spinning temperature as much as possible and slow cooling after rolling is usually adopted to improve the cold heading performance of wire rods by increasing the ferrite content in the structure. For example: Patent CN117265408A discloses an annealing-free cold heading steel and its manufacturing method and the fasteners obtained therefrom, using C-SI-Mn-Al-Cr-Mo-B -Mg composition design, combined with low-temperature rolling and spinning and Stelmor insulation cooling process, obtains 60%~70% ferrite structure and 30%~40% degraded pearlite by volume, reaching Rm≤650MPa and surface reduction Z≥53%. However, on the one hand, low-temperature rolling increases the wear load of the rolling mill, and low-temperature spinning easily leads to spinning difficulties. Increasing the rolling and spinning temperatures for the purpose of improving rolling efficiency will increase the risk of hard and brittle phase precipitation. At the same time, the extended insulation online time will seriously damage the production efficiency. On the other hand, only a soft phase structure dominated by ferrite and pearlite can be obtained. The increase in the proportion of ferrite structure damages the strength of the wire rod. When manufacturing fasteners, it is necessary to strengthen the strength through large drawing processing to achieve the strength grade after quenching and tempering. The plasticity loss is large in the process, which is easy to produce work hardening and then cause cold heading cracking. The application range is too narrow. At the same time, the addition of micro-alloy elements not only has high material costs but also has limited improvement on the strength of cold heading steel wire rods.
[0004] (2) Since the original structure is ferrite + pearlite, the cementite dissolution is slow and the spheroidization time is long. In order to shorten the spheroidizing annealing cycle, the design idea of manufacturing cold heading steel wire rod is all bainite or bainite and martensite composite structure, mainly using the combination of fast cooling and slow cooling after rolling. For example, the production method of bainite cold heading steel wire rod disclosed in patent CN109023103B adopts C-Si-Mn-Cr-Mo composition design, combined with the post-rolling water tank fast cooling, low-temperature wire drawing, air cooling fast cooling and insulation slow cooling process design, forming a large amount of bainite + a small amount of ferrite + a small amount of martensite structure. However, on the one hand, the hard and brittle phases of martensite and bainite will seriously damage the plasticity of the wire rod, which is easy to cause breakage during the unwinding process of downstream processing coiling, during transportation from the steel plant to the downstream, and even during the coiling process of the steel plant, affecting the yield; on the other hand, although the difficulty of spheroidizing annealing is reduced and the production cycle is shortened, in order to achieve 12 .9 performance level, its organization still needs to undergo at least one spheroidization degradation, the production cycle is still long, the manufacturing cost is high, and the energy consumption is high. Summary of the invention
[0005] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a 12.9-grade annealing-free hot-rolled complex phase cold heading steel wire rod and a manufacturing method thereof, which can reduce material costs, improve the cold processing performance of the cold heading steel wire rod, and be used for annealing-free, efficient and green manufacturing of 12.9-grade high-strength cold heading steel fasteners.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] A method for manufacturing a 12.9-grade annealing-free hot-rolled complex phase cold heading steel wire rod, wherein the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.37% to 0.43%, Si: 0.20% to 0.35%, Mn: 0.50% to 0.75%, Cr: 0.32% to 0.47%, P≤0.015%, S≤0.008%, and the rest is Fe and unavoidable impurities; the manufacturing method comprises:
[0008] The wire rod produced by spinning in a controlled rolling process is first subjected to ultra-fast cold quenching in molten salt, so that the wire rod is cooled at a cooling rate of ≥30°C / s to a temperature range dominated by the bainite phase region, so that the austenite structure is transformed into a mixed structure of quenched bainite and quenched martensite, and then subjected to online molten salt heating and tempering, isothermal tempering to transform the quenched bainite into tempered bainite, and the quenched martensite into tempered martensite, while promoting the transformation of carbides into spheroidized structures, and finally subjected to roller slow cooling to obtain a cold heading steel wire rod having a microstructure consisting of a complex phase structure dominated by tempered bainite, a small amount of tempered martensite, and the rest being quasi-spheroidized carbides.
[0009] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:
[0010] (1) Carbon: The carbon element is the most basic and cheap strengthening element in steel. As the carbon content increases, it can improve the tensile strength and hardenability of steel, and is conducive to promoting the transformation of austenite to quenched bainite. However, too high a carbon content will lead to reduced ductility and cold heading performance of steel, and increase the risk of decarburization. Therefore, in order to enable the cold heading steel wire rod to reach the final strength grade through quenching and tempering under the annealing-free process, while taking into account the plasticity and cold heading performance of the steel, the mass percentage of C is controlled to be 0.37%~0.43%.
[0011] (2) Silicon: Si is the main deoxidizing element in steel and can also be dissolved in austenite to increase the strength and hardness of steel. However, excessive silicon will promote the growth of columnar crystals in continuous casting steel, reduce the plasticity of wire rod, and make cold heading more difficult. Therefore, the mass percentage of Si is controlled to be 0.20%~0.35%.
[0012] (3) Manganese: Mn is a strong hardenability element that can promote the transformation of quenched bainite and quenched martensite. Too low Mn content will lead to poor deoxidation and increase the difficulty of smelting. However, too high Mn content will easily aggravate the segregation during the solidification process of the steel billet, resulting in poor uniformity of the steel. Therefore, the Mn content is appropriately reduced, and the mass percentage of Mn is controlled to be 0.50%~0.75%.
[0013] (4) Chromium: The Cr element can significantly improve the hardenability of steel and strongly delay the transformation of pearlite and bainite, so that the steel has good comprehensive mechanical properties after quenching and tempering. Reducing the Cr content is beneficial to controlling the bainite content of the matrix. At the same time, the Cr element is a medium-strong carbide-forming element. If the content is too high, it will deteriorate the drawing and cold heading properties of the wire rod. Therefore, the Cr content is appropriately reduced, and the mass percentage of Cr is controlled to be 0.32%~0.47%.
[0014] (5) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.008%.
[0015] Mo element is a ferrite-forming element and can strongly improve hardenability, but its cost is extremely high. Based on the medium carbon component design of the present invention, the present invention uses a component design that does not contain Mo element to reduce the hardenability of the material and effectively control the matrix complex phase structure; on the basis of the low hardenability and low-cost chemical composition design of the above-mentioned C-Si-Mn-Cr, combined with molten salt ultra-fast cold quenching and isothermal technology, the wire rod after spinning is subjected to molten salt ultra-fast cold quenching in online molten salt, and the high heat exchange capacity of molten salt is utilized. Compared with the Stelmore insulation and slow cooling process, the phase transition temperature range of ferrite and pearlite can be quickly skipped to avoid the formation of soft phase ferrite and pearlite in the organization. At the same time, compared with the Stelmore Air cooling can reduce the wire rod from the high-temperature spinning temperature to the molten salt temperature more quickly, control the high-temperature austenite in the wire rod to undergo quenching transformation in a temperature range dominated by the bainite phase region, use ultra-fast cooling to make up for the loss of hardenability in the composition, improve the hardenability of the steel grade, and promote the high-temperature austenite structure of the wire rod after spinning to transform into a mixed structure of mostly quenched bainite and a small part of quenched martensite after ultra-fast quenching, provide matrix strength, and avoid excessive formation of quenched martensite, which will cause excessive tempered martensite content in subsequent structures and cause plasticity to decrease; because the wire rod can evenly exchange heat with the molten salt when passing through the molten salt, the temperature difference of the wire rod is smaller than that of the uneven air volume during air cooling, so the performance extremes of the wire rod are also smaller.
[0016] Compared with the Stelmor air-cooling rapid cooling followed by insulation and slow cooling to obtain a mixture of all bainite or martensite and bainite, the present invention further performs online molten salt heating and tempering on the wire rod that has been quenched by ultra-fast molten salt cooling, so that the quenched bainite and quenched martensite structures are subjected to high-temperature isothermal treatment, and are transformed into tempered bainite and tempered martensite for toughening, which can retain the strength characteristics of the quenched bainite and quenched martensite, and is used to make up for the strength loss caused by the low-cost components that reduce the alloy content, and the plasticity of the quenched structure can be significantly improved by the tempered structure; at the same time, compared with continuous slow cooling, the wire rod can be kept consistent with the molten salt temperature for high-temperature isothermal treatment, the wire rod has a higher temperature state for a longer time, and after being converted into the tempered structure, the matrix structure can be further softened at high temperature for a long time, thereby promoting the The carbides are transformed into spheroidized structures to ensure the strength and plasticity match of the wire rod, effectively avoiding the breakage caused by hard and brittle phases during the unwinding process of the downstream processing coil, the transportation process from the steel plant to the downstream, and even the coiling process of the wire rod in the steel plant; similarly, further slow cooling on the roller can utilize the high temperature state of the wire rod out of the molten salt to continue the softening effect in the later stage of the online heating and tempering stage, and slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides, thereby improving the softening effect of the wire rod. Compared with extending the high-temperature isothermal time, slow cooling on the roller consumes less energy and is more economical. Therefore, by adjusting the structure of the hot-rolled cold heading steel wire rod to the tempered state, the strength and plasticity match of the cold heading steel wire rod can be adjusted, which can be used in the manufacture of 12.9 grade annealing-free high-strength fasteners and bolts and other application fields.
[0017] Preferably, the steel billet before controlled rolling is produced by converter smelting, refining and continuous casting. The basicity of the protective slag in the converter smelting is controlled to be 1.5-5, which is used to improve the cleanliness of the molten steel and reduce the S content in the smelting process. At the same time, it is avoided that the basicity of the protective slag is too high to affect the fluidity of the slag, and the segregation or solidification precipitation caused by excessive S content to cause brittleness, thereby reducing the risk of cold working cracking due to sulfides.
[0018] Preferably, the controlled rolling process controls the initial rolling temperature to 1000~1050℃ and the initial rolling reduction to 35%~45%; since the wire rod has a high cooling rate after ultra-fast cold quenching in molten salt, there is no need to consider the low-temperature wire drawing and rolling requirements caused by the limited Stelmor cooling capacity and process requirements. Therefore, a higher initial rolling temperature can be used to reduce rolling mill wear and improve rolling efficiency, and a larger initial rolling reduction can be used to break up columnar crystals as much as possible to prepare for grain refinement.
[0019] Preferably, the controlled rolling process controls the final rolling temperature to 850-900°C and the final rolling reduction to 26%-36%; a higher final rolling temperature is used to reduce rolling mill wear and improve rolling efficiency, and a larger final rolling reduction is used to refine the austenite grains as much as possible, with a large dispersion, making austenite easier to homogenize, which is beneficial to improving the hardenability of cold heading steel wire rods, and can increase the nucleation rate, which is beneficial to promoting the transformation of carbides to spheroidized structures.
[0020] Preferably, in the controlled rolling process, the soaking time of the steel billet is controlled to be ≤2 hours and the oxygen content in the furnace is ≤1.5% before rolling; on the basis of increasing the initial rolling temperature, a higher soaking temperature can be used to promote the homogenization of the steel billet composition, and the soaking time and the low oxygen content in the furnace can be further controlled to reduce the risk of decarburization.
[0021] Preferably, the molten salt ultra-fast cold quenching controls the quenching temperature to be 375-415°C, and the quenching treatment time is 8-20s; within the quenching temperature range of the molten salt ultra-fast cold quenching, the lower the quenching temperature and the longer the quenching treatment time, the greater the proportion of quenched martensite in the mixed structure, resulting in an increase in the content of tempered martensite in the complex phase structure, causing the strength of the cold heading steel wire rod to increase and the plasticity to decrease; conversely, the higher the quenching temperature and the shorter the quenching treatment time, the greater the proportion of quenched bainite in the mixed structure, resulting in an increase in the content of tempered bainite in the complex phase structure, The strength of the cold heading steel wire rod decreases and the plasticity increases; however, if the quenching temperature is too high, it will be close to the phase transformation temperature range of ferrite and pearlite, which is not conducive to the transformation of austenite structure to quenched bainite and quenched martensite. If the quenching temperature is too low, it will be close to the phase transformation temperature range of quenched martensite, which is not conducive to the transformation of austenite structure to mixed structure. Therefore, the quenching temperature can be controlled to be in the temperature range dominated by the bainite phase region, and the quenching treatment time can be further adjusted to adjust the proportion of quenched bainite and quenched martensite in the mixed structure, so as to make organizational preparations for the subsequent online molten salt heating and tempering.
[0022] Preferably, the molten salt ultra-fast cold quenching controls the molten salt temperature rise to ≤8°C; since the temperature difference of the wire rod from the spinning temperature to the quenching temperature is large, the molten salt circulation amount can be controlled to further control the molten salt temperature rise and improve the quenching control accuracy.
[0023] Preferably, the online molten salt heating and tempering controls the isothermal temperature to be 550-615°C, and the molten salt isothermal time to be 380-580s; within the online molten salt heating and tempering temperature range, the higher the isothermal temperature and the longer the molten salt isothermal time, the more obvious the softening effect, the higher the proportion of quasi-spheroidized carbides, the higher the plasticity of the cold heading steel wire rod, the greater the strength loss, and the higher the energy consumption and production cost; conversely, the lower the isothermal temperature and the shorter the molten salt isothermal time, the weaker the softening effect, and even when the isothermal temperature is too low and the molten salt isothermal time is too short, the quenched martensite and the quenched bainite fail to complete the tempering transformation and significantly reduce the plasticity of the cold heading steel wire rod.
[0024] Preferably, the online molten salt temperature rise tempering controls the molten salt temperature rise to ≤5°C; since the temperature difference of the wire rod from the quenching temperature to the isothermal temperature is relatively small, it is easier to control the temperature difference, and the molten salt circulation amount can be controlled to further control the molten salt temperature rise, thereby improving the isothermal tempering accuracy.
[0025] Preferably, the roller slow cooling adopts a roller to transport the wire rod into the heat preservation cover, so that the wire rod is slowly cooled to below 350°C at a cooling rate of 0.5~1.2°C / s for coiling; the higher the cooling rate, the weaker the softening effect of the roller slow cooling on promoting the toughening and spheroidization of the wire rod structure, the slower the cooling rate, the better the softening effect, but the longer the online time, the lower the production efficiency, so the cooling rate of the wire rod can be further controlled to promote the strength and plasticity matching of the wire rod on the basis of economical production.
[0026] A 12.9-grade annealing-free hot-rolled complex phase cold heading steel wire rod is obtained according to the manufacturing method of the 12.9-grade annealing-free hot-rolled complex phase cold heading steel wire rod described in any one of the above items.
[0027] Preferably, the volume percentage of the tempered bainite is 55%~60%, and the volume percentage of the tempered martensite is 35%~40%; tempered bainite has significantly improved plasticity compared with quenched bainite, and has better plasticity than tempered martensite, and tempered martensite has significantly improved plasticity compared with quenched martensite, and has better strength than tempered bainite. Therefore, on the basis of having both quasi-spheroidized carbides in the complex phase group organization, controlling the proportion of tempered bainite and tempered martensite, and regulating the cold heading steel wire rod organization can further regulate the strength-plasticity matching of the wire rod.
[0028] Preferably, the diameter of the cold heading steel wire rod is 6.0~12.0mm, the tensile strength is 1012~1063MPa, and the cross-sectional shrinkage rate is 55%~59%. Compared with the existing air-cooled cold heading steel wire rod, it maintains a higher tensile strength, and thus does not need to be strengthened by a large drawing amount. It can reach the strength grade of 12.9 fasteners through tempering without annealing, reducing the risk of drawing fracture and cold heading cracking caused by excessive plastic loss during the manufacturing process. On this basis, it has significantly improved plasticity, that is, a higher cross-sectional shrinkage rate, and thus has a lower deformation resistance, can withstand a large degree of deformation without cracking, and is suitable for annealing-free production.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) In view of the fact that the existing cold heading steel wire rod needs to be annealed at least once when used in the manufacture of 12.9 grade fasteners, which not only has a long production cycle, but also brings about the problems of increased manufacturing costs and high energy consumption, the present invention adopts a low-cost, low-hardenability chemical composition design with reduced Cr and Mn content and no micro-alloy components such as Mo, combined with molten salt ultra-fast cold quenching and isothermal technology directly after wire spinning, firstly promotes the high-temperature austenite structure to transform into a mixed structure of bainite and martensite after ultra-fast cold quenching, provides matrix strength, and uses ultra-fast cooling to compensate for the hardenability loss of the composition, thereby improving the strength of the steel. The hardenability of high steel grades is improved, and the cold heading steel wire rod structure is adjusted to the tempered state, and the wire rod structure is further toughened and the carbide is spheroidized to obtain a microstructure including a complex phase structure composed of mainly tempered bainite, a small amount of tempered martensite, and the rest is quasi-spheroidized carbides. The strength and plasticity of the cold heading steel wire rod are matched, and the fracture problem caused by hard and brittle phases in the downstream processing coil unwinding process, in the transportation process from the steel plant to the downstream, and even in the coiling process of the steel plant wire rod is avoided. It has good industrial adaptability.
[0031] (2) In view of the problems of mill wear and wire drawing difficulty caused by the low-temperature wire drawing and low-temperature rolling processes used in the existing cold heading steel wire rods for grade 12.9 fasteners, the present invention combines controlled rolling control with molten salt ultra-fast cold quenching and isothermal technology to increase the initial rolling and final rolling temperatures to reduce mill wear and improve rolling efficiency. Austenite grains are refined as much as possible with a large reduction, the hardenability of the steel grade is improved, and the transformation of carbides to spheroidized structures is promoted.
[0032] (3) In view of the current situation that the application scope of existing cold heading steel wire rods for 12.9 grade fasteners without annealing is relatively narrow, the present invention has successfully developed a 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod, which can reduce material costs and improve the cold processing performance of cold heading steel wire rods. It can achieve a tensile strength of 1012~1063MPa and a cross-sectional shrinkage rate of 55%~59%. It can effectively improve the work hardening and cold heading cracking problems caused by large drawing, and can be used in the manufacture of 12.9 grade annealing-free high-strength fasteners, bolts and other application fields, and has good industrial adaptability and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0034] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;
[0035] Figure 2 is the metallographic structure diagram of Comparative Example 2 of the present invention;
[0036] Figure 3 is the metallographic structure diagram of Example 2 of the present invention;
[0037] Figure 4 It is the metallographic structure diagram of Example 4 of the present invention. DETAILED DESCRIPTION
[0038] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:
[0039] A preferred embodiment of the manufacturing method of the 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.42%, Si: 0.2%, Mn: 0.5%, Cr: 0.41%, P: 0.013%, S: 0.008%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of converter smelting → refining → continuous casting → controlled rolling → wire laying → molten salt ultra-fast cold quenching and isothermal → roller slow cooling → coiling, specifically:
[0040] The converter smelting is used to smelt the molten iron raw material into primary molten steel through a blast furnace, control the basicity of the protective slag to 1.5, reduce the S content in the smelting process, and reduce the risk of cold working cracking caused by sulfides; the refining is used to further adjust the composition, deoxidize and desulfurize, and remove inclusions in the primary molten steel at the refining station; the continuous casting is used to pour the refined molten steel into a continuous casting machine, and the continuous casting production specification is 220mm×220mm steel billets; the controlled rolling is used to heat the steel billet through a heating furnace to achieve a high-temperature steel billet that can be rolled through a rolling line. The steel billet is rolled into a wire with a specification of 10 mm, and the columnar crystals are broken as much as possible by high temperature and large reduction to prepare for grain refinement. Specifically: the steel billet soaking time is controlled to be 1.8 hours, the oxygen content in the furnace is 1.4%, the initial rolling temperature is 1020°C, the initial rolling reduction is 38%, the final rolling temperature is 860°C, and the final rolling reduction is 29%; the wire-spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a wire-spinning mechanism, and the wire-spinning temperature is controlled to be 844°C. Austenitization is performed to prepare for subsequent organization, and the wire rod is spread on the roller and transported along the roller.
[0041] The molten salt ultra-fast cold quenching and isothermal treatment adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, and is rapidly cooled to the molten salt temperature for molten salt ultra-fast cold quenching, so that the wire rod is cooled at a cooling rate of 33°C / s to a temperature range dominated by the bainite phase region, so that the austenite structure is transformed into a mixed structure of quenched bainite and quenched martensite, providing matrix strength; the wire rod is then conveyed by a roller to pass through the second salt bath tank, and is rapidly heated to the molten salt temperature for online molten salt heating and tempering, and isothermal tempering The quenching process transforms the quenched bainite into tempered bainite and the quenched martensite into tempered martensite for toughening, and at the same time promotes the transformation of carbides into spheroidized structures, and softens the matrix structure at high temperature for a long time to ensure the strength and plasticity matching of the wire rod. Specifically: the molten salt ultra-fast cold quenching controls the quenching temperature to 388°C, the quenching treatment time to 18s, and the molten salt temperature rise to ≤8°C; the online molten salt heating and tempering controls the isothermal temperature to 615°C, the molten salt isothermal time to 580s, and the molten salt temperature rise to ≤5°C.
[0042] The roller slow cooling process is to convey the wire rod coming out of the second salt bath tank into the heat preservation cover by rollers for slow cooling treatment. The slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides, and improves the softening effect of the wire rod. Specifically, the wire rod is slowly cooled to 325°C at a cooling rate of 1.2°C / s until it is coiled; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 1 shown.
[0043] Comparative Example 1:
[0044] A method for manufacturing cold heading steel wire rod, which differs from Example 1 in that: the manufacturing method is manufactured according to the process flow of low-temperature hot rolling → wire laying → Stelmor insulation slow cooling → coiling, specifically: the initial rolling temperature of the low-temperature hot rolling process is controlled to be 925°C, and the final rolling temperature is 800°C; the wire laying process controls the wire laying temperature to be 780°C; the Stelmor insulation slow cooling is to pass the wire rod after wire laying through a Stelmor air cooling line, turn off all fans and insulation covers, so that the wire rod completes phase change at a cooling rate of 1.5°C / s in the cover, and obtain the cold heading steel wire rod finished product after coiling off the line.
[0045] Comparative Example 2:
[0046] A method for manufacturing a cold heading steel wire rod, which differs from Example 1 in that: the manufacturing method is manufactured according to the process flow of low temperature hot rolling → wire spinning → molten salt ultra-fast cold quenching, specifically: the molten salt ultra-fast cold quenching adopts a two-stage salt bath tank with molten salt inside, the quenching temperature is 250°C, the quenching treatment time is 30s, and the cold heading steel wire rod product is obtained after the production line is off, and its metallographic structure diagram is as follows Figure 2 shown. Embodiment 2:
[0047] A preferred embodiment of the manufacturing method of the 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.43%, Si: 0.35%, Mn: 0.58%, Cr: 0.47%, P: 0.015%, S: 0.007%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of converter smelting → refining → continuous casting → controlled rolling → wire laying → molten salt ultra-fast cold quenching and isothermal → roller slow cooling → coiling, specifically:
[0048] The converter smelting is used to smelt the molten iron raw material into primary molten steel through a blast furnace, control the basicity of the protective slag to 3.5, reduce the S content in the smelting process, and reduce the risk of cold working cracking caused by sulfides; the refining is used to further adjust the composition, deoxidize and desulfurize the primary molten steel, and remove inclusions in the refining station; the continuous casting is used to pour the refined molten steel into a continuous casting machine, and the continuous casting production specification is 220mm×220mm steel billets; the controlled rolling is used to heat the steel billet through a heating furnace to achieve a high-temperature steel billet that can be rolled through a rolling line. The steel billet coming out of the furnace is rolled into wire with a specification of 12mm, and the columnar crystals are broken as much as possible by high temperature and large reduction to prepare for grain refinement. Specifically: the steel billet soaking time is controlled to be 2 hours, the oxygen content in the furnace is 1.5%, the initial rolling temperature is 1000℃, the initial rolling reduction is 35%, the final rolling temperature is 850℃, and the final rolling reduction is 26%; the wire-spinning process is used to convert the wire coming out of the rolling line into wire rods through a wire-spinning mechanism, and the wire-spinning temperature is controlled to be 830℃. Austenitization is performed to prepare for subsequent organization, and the wire rods are spread on the rollers and transported along the rollers.
[0049] The molten salt ultra-fast cold quenching and isothermal treatment adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, and is rapidly cooled to the molten salt temperature for molten salt ultra-fast cold quenching, so that the wire rod is cooled at a cooling rate of 33°C / s to a temperature range dominated by the bainite phase region, so that the austenite structure is transformed into a mixed structure of quenched bainite and quenched martensite, providing matrix strength; the wire rod is then conveyed by a roller to pass through the second salt bath tank, and is rapidly heated to the molten salt temperature for online molten salt heating and tempering, and isothermal tempering The quenching process transforms the quenched bainite into tempered bainite and the quenched martensite into tempered martensite for toughening, and at the same time promotes the transformation of carbides into spheroidized structures, and softens the matrix structure at high temperature for a long time to ensure the strength and plasticity matching of the wire rod. Specifically: the molten salt ultra-fast cold quenching controls the quenching temperature to 375°C, the quenching treatment time to 20s, and the molten salt temperature rise to ≤8°C; the online molten salt heating and tempering controls the isothermal temperature to 565°C, the molten salt isothermal time to 436s, and the molten salt temperature rise to ≤5°C.
[0050] The roller slow cooling process is to convey the wire rod coming out of the second salt bath tank into the heat preservation cover by rollers for slow cooling treatment. The slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides, and improves the softening effect of the wire rod. Specifically, the wire rod is slowly cooled to 335°C at a cooling rate of 0.7°C / s until it is coiled; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 3 shown.
[0051] Comparative Example 3:
[0052] A method for manufacturing a cold heading steel wire rod, which differs from Example 2 in that: the molten salt ultra-fast cold quenching controls the quenching temperature to 310°C, the quenching treatment time is 25s, and the cold heading steel wire rod finished product is obtained after the coil is rolled off the line.
[0053] Comparative Example 4:
[0054] A method for manufacturing a cold heading steel wire rod, which differs from Example 2 in that: the molten salt ultra-fast cold quenching controls the quenching temperature to 430°C, the quenching treatment time is 5s, and the cold heading steel wire rod finished product is obtained after the coil is rolled off the line. Embodiment 3:
[0055] A preferred embodiment of the manufacturing method of the 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.39%, Si: 0.2%, Mn: 0.66%, Cr: 0.38%, P: 0.013%, S: 0.006%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of converter smelting → refining → continuous casting → controlled rolling → wire laying → molten salt ultra-fast cold quenching and isothermal → roller slow cooling → coiling, specifically:
[0056] The converter smelting is used to smelt the molten iron raw material into primary molten steel through a blast furnace, control the basicity of the protective slag to 5, reduce the S content in the smelting process, and reduce the risk of cold working cracking caused by sulfides; the refining is used to further adjust the composition, deoxidize and desulfurize the primary molten steel, and remove inclusions in the refining station; the continuous casting is used to pour the refined molten steel into a continuous casting machine, and the continuous casting produces steel billets with a specification of 160mm×160mm; the controlled rolling is used to heat the steel billet through a heating furnace to achieve a high-temperature steel billet that can be rolled and then pass through a rolling line to produce a high-temperature steel billet from the heating furnace. The incoming steel billet is rolled into wire with a specification of 8mm, and the columnar crystals are broken as much as possible by high temperature and large reduction to prepare for grain refinement. Specifically: the steel billet soaking time is controlled to be 1.7 hours, the oxygen content in the furnace is 1.4%, the initial rolling temperature is 1030℃, the initial rolling reduction is 42%, the final rolling temperature is 880℃, and the final rolling reduction is 33%; the wire-spinning process is used to convert the wire rod exiting the rolling line into a wire rod through a wire-spinning mechanism, and the wire-spinning temperature is controlled to be 862℃. Austenitization is performed to prepare for subsequent organization, and the wire rod is spread on the roller and transported along the roller.
[0057] The molten salt ultra-fast cold quenching and isothermal treatment adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, and is rapidly cooled to the molten salt temperature for molten salt ultra-fast cold quenching, so that the wire rod is cooled at a cooling rate of 34°C / s to a temperature range dominated by the bainite phase region, so that the austenite structure is transformed into a mixed structure of quenched bainite and quenched martensite, providing matrix strength; the wire rod is then conveyed by a roller to pass through the second salt bath tank, and is rapidly heated to the molten salt temperature for online molten salt heating and tempering, and isothermal tempering The quenching process transforms the quenched bainite into tempered bainite and the quenched martensite into tempered martensite for toughening, and at the same time promotes the transformation of carbides into spheroidized structures, and softens the matrix structure at high temperature for a long time to ensure the strength and plasticity matching of the wire rod. Specifically: the molten salt ultra-fast cold quenching controls the quenching temperature to 403°C, the quenching treatment time to 12s, and the molten salt temperature rise to ≤8°C; the online molten salt heating and tempering controls the isothermal temperature to 585°C, the molten salt isothermal time to 515s, and the molten salt temperature rise to ≤5°C.
[0058] The roller slow cooling process uses rollers to convey the wire rods coming out of the second salt bath tank into the insulation cover for slow cooling. The slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides, and improves the softening effect of the wire rod. Specifically: the wire rod is slowly cooled to 330°C at a cooling rate of 1°C / s until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage.
[0059] Comparative Example 5:
[0060] A method for manufacturing a cold heading steel wire rod, which differs from Example 3 in that: the online molten salt heating and tempering controls the isothermal temperature to be 625°C, the molten salt isothermal time to be 300s, and the cold heading steel wire rod finished product is obtained after the coil is rolled off the line.
[0061] Comparative Example 6:
[0062] A method for manufacturing a cold heading steel wire rod, which differs from Example 3 in that: the online molten salt heating and tempering controls the isothermal temperature to be 500°C, the molten salt isothermal time to be 600s, and the cold heading steel wire rod finished product is obtained after the coil is rolled off the line. Embodiment 4:
[0063] A preferred embodiment of the manufacturing method of the 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.37%, Si: 0.32%, Mn: 0.75%, Cr: 0.32%, P: 0.015%, S: 0.007%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of converter smelting → refining → continuous casting → controlled rolling → wire laying → molten salt ultra-fast cold quenching and isothermal → roller slow cooling → coiling, specifically:
[0064] The converter smelting is used to smelt the molten iron raw material into primary molten steel through a blast furnace, control the basicity of the protective slag to 2.5, reduce the S content in the smelting process, and reduce the risk of cold working cracking caused by sulfides; the refining is used to further adjust the composition, deoxidize and desulfurize the primary molten steel, and remove inclusions in the refining station; the continuous casting is used to pour the refined molten steel into a continuous casting machine, and the continuous casting production specification is 160mm×160mm steel billet; the controlled rolling is used to heat the steel billet through a heating furnace to achieve a high-temperature steel billet that can be rolled through a rolling line. The steel billet is rolled into a wire with a specification of 6 mm, and the columnar crystals are broken as much as possible by high temperature and large reduction to prepare for grain refinement. Specifically: the steel billet soaking time is controlled to be 1.5 hours, the oxygen content in the furnace is 1.3%, the initial rolling temperature is 1050°C, the initial rolling reduction is 45%, the final rolling temperature is 900°C, and the final rolling reduction is 36%; the wire-spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a wire-spinning mechanism, and the wire-spinning temperature is controlled to be 880°C. Austenitization is performed to prepare for subsequent organization, and the wire rod is spread on the roller and transported along the roller.
[0065] The molten salt ultra-fast cold quenching and isothermal treatment adopts a two-stage salt bath tank with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath tank, and is rapidly cooled to the molten salt temperature for molten salt ultra-fast cold quenching, so that the wire rod is cooled at a cooling rate of 34°C / s to a temperature range dominated by the bainite phase region, so that the austenite structure is transformed into a mixed structure of quenched bainite and quenched martensite, providing matrix strength; the wire rod is then conveyed by a roller to pass through the second salt bath tank, and is rapidly heated to the molten salt temperature for online molten salt heating and tempering, and isothermal treatment is performed. Tempering transforms quenched bainite into tempered bainite, and quenched martensite into tempered martensite for toughening, while promoting the transformation of carbides into spheroidized structures, and softening the matrix structure at high temperature for a long time to ensure the strength and plasticity matching of the wire rod. Specifically: the molten salt ultra-fast cold quenching controls the quenching temperature to 415°C, the quenching treatment time to 8s, and the molten salt temperature rise to ≤8°C; the online molten salt heating tempering controls the isothermal temperature to 550°C, the molten salt isothermal time to 380s, and the molten salt temperature rise to ≤5°C.
[0066] The roller slow cooling process is to convey the wire rod coming out of the second salt bath tank into the heat preservation cover by rollers for slow cooling treatment. The slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides, and improves the softening effect of the wire rod. Specifically, the wire rod is slowly cooled to 340°C at a cooling rate of 0.5°C / s until it is coiled; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 4 shown.
[0067] Comparative Example 7:
[0068] A method for manufacturing a cold heading steel wire rod, which differs from Example 4 in that: the manufacturing method is manufactured according to the process flow of converter smelting → refining → continuous casting → controlled rolling → wire laying → molten salt ultra-fast cold quenching and isothermal → air cooling → coiling, and the air cooling is carried out by opening the insulation cover and conveying the wire rod coming out of the second salt bath tank with a roller, and controlling the wire rod to be slowly cooled to 340°C at a cooling rate of 3.3°C / s until it is coiled, and the cold heading steel wire rod finished product is obtained after the coiling is off the line.
[0069] The cold heading steel wire rods obtained in the above embodiments and comparative examples were subjected to organizational and performance tests: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organizational test was conducted according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:
[0070] Table 1. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods
[0071]
[0072] From the comparison results of Examples 1 to 4 with Comparative Example 1, it can be seen that compared with the existing low-temperature wire spinning and Stelmor slow cooling process, the present invention adopts a low-cost, low-hardenability chemical composition design that reduces the Cr and Mn content and does not contain micro-alloy components such as Mo, combined with ultra-fast cold quenching and isothermal technology directly after wire spinning, firstly promotes the high-temperature austenite structure to transform into a mixed structure of bainite and martensite after ultra-fast cold quenching in a temperature range dominated by the bainite phase region, which can avoid the production of soft phase pearlite and ferrite structure by Stelmor slow cooling, can provide matrix strength, use ultra-fast cooling to make up for the hardenability loss of the composition, and improve the hardenability of the steel grade; From the comparison results of Examples 1 to 4 with Comparative Example 2, it can be seen that compared with the high-temperature austenite structure in the wire rod after wire spinning, the martensite phase region is transformed into acicular martensite through ultra-fast cold quenching of molten salt, and the present invention obtains bainite. On the basis of the mixed organization of bainite and martensite, the organization of the cold heading steel wire rod is adjusted to the tempered state, and the wire rod organization is further toughened and the carbide is spheroidized, so that the microstructure includes a complex phase organization composed of mainly tempered bainite, a small amount of tempered martensite, and the rest is quasi-spheroidized carbide. The plasticity of the cold heading steel wire rod can be significantly improved, and the strength and plasticity matching of the cold heading steel wire rod can be achieved. The tensile strength can reach 1012~1063MPa, and the cross-sectional shrinkage rate can reach 55%~59%. The work hardening and cold heading cracking problems caused by large drawing are effectively improved, and the fracture problems caused by hard and brittle phases in the unwinding process of downstream processing coils, the transportation process from steel mills to downstream, and even the coiling process of steel mill wire rods are avoided. It can be used in the manufacture of 12.9 grade annealing-free high-strength fasteners bolts and other application fields, and has good industrial adaptability and application prospects.
[0073] From the comparison of Examples 1 to 4, it can be seen from the comparison results of Example 2 and Comparative Example 3 that the lower the quenching temperature and the longer the quenching treatment time, the greater the proportion of quenched martensite in the mixed structure, resulting in an increase in the content of tempered martensite in the complex phase structure, causing the strength of the cold heading steel wire rod to increase and the plasticity to decrease; from the comparison of Examples 1 to 4, it can be seen from the comparison results of Example 2 and Comparative Example 4 that the higher the quenching temperature and the shorter the quenching treatment time, the greater the proportion of quenched bainite in the mixed structure, resulting in an increase in the content of tempered bainite in the complex phase structure, causing the strength of the cold heading steel wire rod to decrease and the plasticity to increase; the quenching temperature and the quenching treatment time can be controlled to prepare the organization for the subsequent online molten salt temperature rising and tempering.
[0074] From the comparison of Examples 1 to 4, it can be seen from the comparison results of Example 3 and Comparative Example 5 that if the isothermal temperature is too high and the molten salt isothermal time is too short, part of the quenched bainite is not completely transformed into tempered martensite, the softening effect is reduced, and the plasticity of the cold heading steel wire rod is significantly reduced; from the comparison of Examples 1 to 4, it can be seen from the comparison results of Example 3 and Comparative Example 6 that if the isothermal temperature is too low and the molten salt isothermal time is too long, the wire rod strength and plasticity loss is large, and the energy consumption is large; therefore, the molten salt heating and tempering can be further controlled to control the isothermal temperature and the molten salt isothermal time, promote the transformation of the wire rod structure, regulate the softening effect of structure toughening and spheroidization, and promote the strength and plasticity matching of the wire rod on the basis of economic production.
[0075] From the comparison results of Examples 1 to 4 and Comparative Example 7, it can be seen that slow cooling on a roller can utilize the high temperature state of the wire rod out of the molten salt to continue the softening effect in the later stage of the online heating and tempering stage. Slow cooling promotes further toughening of the wire rod structure and further spheroidization of carbides, thereby improving the softening effect of the wire rod. Compared with extending the high-temperature isothermal time, slow cooling on a roller consumes less energy and is more economical.
[0076] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for manufacturing 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.37% to 0.43%, Si: 0.20% to 0.35%, Mn: 0.50% to 0.75%, Cr: 0.32% to 0.47%, P≤0.015%, S≤0.008%, and the rest is Fe and unavoidable impurities; the manufacturing method thereof includes: The wire rod produced by spinning in a controlled rolling process is first subjected to ultra-fast cold quenching in molten salt, so that the wire rod is cooled at a cooling rate of ≥30°C / s to a temperature range dominated by a bainite phase region, so that the austenite structure is transformed into a mixed structure of quenched bainite and quenched martensite, and then subjected to online molten salt heating tempering, isothermal tempering to transform the quenched bainite into tempered bainite, and the quenched martensite into tempered martensite, while promoting the transformation of carbides into spheroidized structures, and finally subjected to roller slow cooling to obtain a cold heading steel wire rod having a microstructure consisting of a composite structure dominated by tempered bainite, a small amount of tempered martensite, and the rest being quasi-spheroidized carbides; The controlled rolling process controls the final rolling temperature to 850-900°C, the molten salt ultra-fast quenching controls the quenching temperature to 375-415°C, and the quenching treatment time is 8-20s; the online molten salt heating and tempering controls the isothermal temperature to 550-615°C, and the molten salt isothermal time is 380-580s, and the roller slow cooling uses a roller to transport the wire rod into the insulation cover, so that the wire rod is slowly cooled to below 350°C at a cooling rate of 0.5-1.2°C / s for coiling.
2. The method for manufacturing the 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod according to claim 1, characterized in that: The steel billet before controlled rolling is produced by converter smelting, refining and continuous casting, wherein the basicity of the protective slag is controlled to be 1.5-5 during the converter smelting.
3. The method for manufacturing the 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod according to claim 1, characterized in that: The controlled rolling process controls the initial rolling temperature to 1000-1050°C, the initial rolling reduction to 35%-45%, and the final rolling reduction to 26%-36%.
4. The method for manufacturing the 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod according to claim 3, characterized in that: In the controlled rolling process, the steel billet soaking time is controlled to be ≤2 hours and the oxygen content in the furnace is controlled to be ≤1.5% before rolling.
5. The method for manufacturing 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod according to claim 1, characterized in that: The ultra-fast quenching of the molten salt controls the temperature rise of the molten salt to ≤8°C; the online molten salt heating and tempering controls the temperature rise of the molten salt to ≤5°C.
6. A 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod, characterized in that: Obtained according to the manufacturing method of 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod according to any one of claims 1 to 5.
7. The 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod according to claim 6, characterized in that: The volume percentage of the tempered bainite is 55% to 60%, and the volume percentage of the tempered martensite is 35% to 40%.
8. The 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod according to claim 6, characterized in that: The cold heading steel wire rod has a diameter of 6.0-12.0 mm, a tensile strength of 1012-1063 MPa, and a cross-sectional shrinkage of 55%-59%.