A low compression ratio thick Q690 high-strength steel plate and a manufacturing method thereof
Through specific chemical composition and production process, it solves the problem in the existing technology that it is difficult to produce low-compression bit-thick Q690 high-strength steel plates with a thickness of more than 180mm, achieving improvements in high strength, toughness and crack resistance, and satisfying the application of engineering machinery. need.
Patent Information
- Application Number
- CN202211668537.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-24
AI Technical Summary
It is difficult to produce low-compression bit-thick Q690 high-strength steel plates with a thickness of more than 180mm using existing technology, and hydrogen-induced delayed cracks are prone to occur during the cutting and welding processes, affecting equipment safety.
Using a specific chemical composition combination and production process, including molten steel smelting, continuous casting, hot rolling, hydrogen expansion and quenching and tempering steps, the chemical composition and organizational structure of the steel plate are controlled to ensure the low compression ratio and high strength of the steel plate. At the same time, through expansion The hydrogen process reduces the hydrogen content and internal stress, and improves the toughness and crack resistance of the steel plate.
Achieved the production of 180-220mm thick Q690 high-strength steel plate with low compression ratio, which has high yield strength, tensile strength and excellent cold bending performance, reduces the risk of hydrogen-induced delayed cracking, and meets the application needs in engineering machinery and other fields.
Smart Images

Figure BDA0004015577220000061 
Figure BDA0004015577220000071 
Figure BDA0004015577220000072
Abstract
Description
Technical Field
[0001] The invention belongs to the field of iron and steel metallurgy, and in particular relates to a Q690 high-strength steel plate with a thickness of 180 to 220 mm and a production method thereof. Background Art
[0002] Q690 steel plate has the characteristics of high strength, good toughness and excellent processing performance, and is widely used in engineering machinery, bridge construction and other fields. In recent years, with the rise of large and super-large projects at home and abroad, engineering machinery and equipment have become increasingly large-scale, and the demand for thick and high-strength steel plates has become increasingly strong. At present, the maximum thickness of Q690 steel defined in the national standard GB / T16270-2009 is 180mm, which can no longer fully meet the product demand for extra-thick steel plates for key components of some special engineering equipment.
[0003] The main difficulties in producing Q690 extra-thick steel plates are: (1) Due to the thickness restrictions of the continuous casting slabs of each steel mill, the thicker the finished steel plate, the smaller the compression ratio, resulting in coarse grains and difficulty in ensuring the strength and toughness of the steel plate; (2) The thicker the steel plate, the greater the temperature gradient from the surface to the core of the steel plate, and the uneven cooling in the thickness direction, resulting in the lower strength of the steel plate towards the core; (3) Q690 steel plates are mostly designed with martensitic structure, which has high strength and is more sensitive to hydrogen-induced delayed cracking. Due to the large thickness of the steel plate, the diffusion path of hydrogen atoms is long and difficult to escape, resulting in delayed cracks in the steel plate during subsequent cutting, welding and even use, affecting equipment safety. How to overcome the above difficulties and develop extra-thick Q690 steel plates above 180mm is an urgent problem that steel mills need to solve.
[0004] Chinese patent document CN104264064A discloses a super thick Q690 high-strength structural steel plate and its manufacturing method. Two-stage rolling is adopted. In order to ensure the deformation amount of fine rolling, the ratio of the thickness of the steel plate after rough rolling to the thickness of the finished product is required to be above 1.4. After rolling, the steel plate is quenched online using the DQ+ACC cooling method. Due to the different water entry temperatures at the head and tail of the steel plate, online quenching will lead to uneven performance at the head and tail of the steel plate, and its use in key parts of engineering equipment is limited. The production thickness of the steel plate disclosed in the document is 160-180mm.
[0005] Chinese patent document CN106756544A discloses a method for producing a low carbon equivalent thick Q690D high strength steel plate. The steel plate has a CEV of ≤0.56 and is produced by offline quenching, but the maximum production thickness is only 100mm, which is not enough to be used as a thick plate.
[0006] Chinese patent document CN106319380A discloses a low compression ratio 690MPa grade extra-thick steel plate and its production method. After rough rolling, the steel plate directly enters laminar cooling, and the surface temperature drops to 30-50°C below Ar3, and then returns to temperature for 1-3 minutes. When the surface temperature of the steel plate reaches 760-860°C, fine rolling is carried out. The process control is relatively complex and does not conform to the traditional rolling process. The rolling cooling sequence needs to be changed, the operation is difficult, and the efficiency is low. In addition, in order to ensure the uniformity of the structure of the extra-thick steel plate, the invention adds a normalizing process before the traditional quenching and tempering process, which increases the production process and cost. And the maximum production thickness is 115mm.
[0007] In summary, the existing production technologies for ultra-thick Q690 high-strength steel plates are mainly quenching and tempering or online quenching. In order to ensure that rolling penetrates into the core, the method of ensuring the deformation of the finishing rolling or performing low-temperature finishing rolling is often adopted. The maximum thickness of the finished steel plate is 180mm, and the production of low-compression ultra-thick steel plates above 180mm has not yet been involved. At the same time, no feasible solution has been given to the problem of hydrogen-induced delayed cracking of ultra-thick high-strength steel plates. Summary of the invention
[0008] The object of the present invention is to provide a quenched and tempered high-strength steel plate with low compression ratio and specific thickness Q690 and a production method thereof to meet the requirements.
[0009] The technical solution adopted by the present invention to solve the above problem is: a low compression ratio thick Q690 high-strength steel plate, the chemical composition of the steel plate is C: 0.15-0.20%, Si: 0.10-0.40%, Mn: 1.20-1.50%, Nb: 0.040%-0.060%, V: 0.030%-0.060%, Ti: 0.020%-0.030%, Al: 0.02-0.05%, Ni: 1.00 ~1.20%, Cu: ≤0.30%, Cr: 0.60~1.00%, Mo: 0.40~0.70%, B: 0.0015~0.0025%, Ca: 0.001~0.005%, P: ≤0.012%, S: ≤0.002%, O: ≤0.002%, N: ≤0.004%, H: ≤0.0002%, the balance is Fe and unavoidable impurity elements; Carbon equivalent CEV: 0.65~0.75%.
[0010] Furthermore, the thickness of the high-strength steel plate is 180 to 220 mm.
[0011] Furthermore, the microstructure of the steel plate is tempered troostite and bainite.
[0012] Furthermore, the yield strength is ≥630MPa, the tensile strength is ≥710MPa, the elongation is ≥14%; the low temperature Charpy impact energy of -40°C is ≥47J; d=3a, and there is no crack in 180° cold bending.
[0013] The reasons for limiting the element composition of the Q690 high-strength steel plate of the present invention are as follows:
[0014] C: Carbon as a solid solution element can significantly improve the strength of the steel plate, but it has an adverse effect on the plasticity, toughness, cold bending performance and welding performance of the steel plate. Based on the requirements of steel plate strength and toughness matching and cold bending performance, the carbon content in the present invention is controlled to be 0.15-0.20%.
[0015] Si: It plays a role of solid solution strengthening in the steel. However, too high Si content will deteriorate the toughness of martensitic high-strength steel and increase the cold crack sensitivity of the steel plate. In the present invention, Si content is controlled between 0.10 and 0.40%.
[0016] Mn: improves hardenability, promotes martensitic transformation, and improves strength in the steel. However, Mn is a major segregation element. Excessive Mn content will cause central segregation of the continuous casting billet to form MnS, which will adversely affect the toughness, lamellar tearing resistance, and welding performance of the steel plate. The present invention stipulates that the amount of manganese added is within the range of 1.20-1.50%.
[0017] Nb: can produce significant grain refinement, precipitation strengthening and precipitation strengthening effects. Nb dissolved in austenite can improve hardenability, and the carbide precipitation phase of Nb has the effect of refining grains and improving matrix strength. In the present invention, the Nb content is controlled to be 0.040-0.060%.
[0018] V: grain refining element; it can play a certain precipitation strengthening role during tempering. When the V content is too high, the toughness and welding performance of the steel plate will deteriorate. Therefore, the V content of the present invention is controlled to be 0.030-0.060%.
[0019] Ti: Ti (C / N) has a high dissolution temperature, usually above 1400°C, and has a strong pinning effect on the grain boundary at high temperature, preventing the coarsening of austenite grains during heating. The present invention requires rolling at high temperature, and the Ti content is controlled to be 0.020-0.030%.
[0020] Al: deoxidation and grain refinement element. The present invention stipulates that the Al content is 0.02-0.05%.
[0021] Cr: It is an element that improves the hardenability of steel, can inhibit the formation of polygonal ferrite and pearlite, promote the transformation of low-temperature microstructures bainite or martensite, and improve the strength of steel. However, too high a Cr content will affect the toughness of the steel and reduce the welding performance of the steel plate. The Cr content of the present invention is controlled at 0.60-1.00%.
[0022] Mo: It is an element that improves the hardenability of steel and is beneficial to the formation of bainite or martensite during cooling. Adding a certain amount of Mo to the steel will increase the strength of the steel plate without affecting the low-temperature impact performance of the steel plate. Mo can increase the tempering resistance of the steel plate and can prevent the strength of the steel plate from decreasing at a higher temperature. The Mo content of the present invention is controlled at 0.40-0.70%.
[0023] Ca: inclusion modification element, which can react with long strips of MnS to generate spherical CaS, change the anisotropy of the steel plate, and can also modify the Al2O3 inclusions generated by Al deoxidation into spherical low-melting-point inclusions, promote the removal of inclusions, and improve the plastic toughness of the steel plate. In the present invention, the Ca content is controlled to be 0.001-0.005%.
[0024] P: harmful element in steel, easy to segregate, adversely affecting the plasticity and toughness of the material, high P content increases the brittleness of the steel plate. The present invention stipulates that P: ≤ 0.012%
[0025] S: harmful element in steel, easy to segregate. Mn element easily forms MnS segregation inclusions, leading to delamination and cracking of steel plate. The present invention stipulates that S: ≤0.002%.
[0026] O, N, H: harmful gas elements, high content, many inclusions, reduce the plastic toughness of steel plates, and have a high risk of cracking of steel plates. The present invention strictly controls the O content to be no higher than 0.002%; the N content to be no higher than 0.0004%; and the H content to be no higher than 0.0002%.
[0027] CEV: The present invention adopts the carbon equivalent formula CEV = C + Mn / 6 + (Cr + Mo + V) / 5 + (Ni + Cu) / 15; carbon equivalent has a great influence on the strength and weldability of steel. High CEV has high strength, but reduced weldability; to ensure the hardenability of the steel plate, the present invention controls 0.65 ≤ CEV ≤ 0.75.
[0028] The manufacturing method of the above-mentioned low shrinkage thick Q690 high-strength steel plate includes molten steel smelting, continuous casting, hot rolling, hydrogen expansion and quenching and tempering steps, wherein:
[0029] (1) Molten steel smelting
[0030] Molten steel is smelted according to the chemical composition of the steel plate. The smelting of the molten steel adopts converter smelting, refining outside the furnace and vacuum degassing treatment.
[0031] (2) Continuous casting
[0032] During continuous casting, the superheat of molten steel is controlled at 5-20℃, and heavy pressure is applied at the end of solidification of the ingot. Due to the low compression ratio of the steel plate, the process must be optimized in the continuous casting stage to ensure the quality of the core of the continuous casting ingot. The present invention adopts a heavy pressure reduction process at the end of solidification of the ingot to fully bridge the defects of pores and looseness in the core of the ingot, and the reduction amount is not less than 10mm and not more than 15mm; the center segregation of the ingot is controlled to be not higher than C1.0 level, and the center looseness is not higher than 1.0 level.
[0033] (3) Heating and rolling
[0034] The ingot is heated to 1200-1250℃ for 8-14min / cm, so that the alloy elements in the steel are fully dissolved to ensure the uniformity of the composition and performance of the final product. After the billet is removed from the furnace and descaled by high-pressure water, it is subjected to two-stage controlled rolling of rough rolling + finishing rolling. In order to increase the rolling deformation of the core of the steel plate, the rough rolling is carried out in the high temperature zone, and the final rolling temperature of the rough rolling is 1050-1100℃. The ratio of the thickness of the steel plate after rough rolling to the thickness of the finished product is controlled to be less than 1.2 times, and the number of passes with a reduction of ≥30mm is not less than 3; the starting rolling temperature of the finishing rolling is 920-950℃, and the final rolling temperature is ≥850℃. In order to avoid grain growth without generating large stress, the steel plate is cooled by ACC after rolling, and the final cooling temperature is 600-700℃.
[0035] (4) Steel plate hydrogen expansion
[0036] After rolling, the steel plate is put into the furnace for hydrogen expansion. The furnace temperature is ≥300℃, the steel plate is heated to 600-700℃, and the furnace time is ≥72 hours. This promotes the homogenization of the core structure and properties of the steel plate, reduces the H content and internal stress, greatly improves the toughness of the steel plate, and reduces the risk of hydrogen-induced delayed cracking of extra-thick high-strength steel plates.
[0037] (5) Quenching and tempering: After hydrogen expansion, the steel plate is quenched at a temperature of 880-940°C. After the furnace reaches the temperature, it is kept warm for 30-90 minutes. To ensure the uniformity of the steel plate, the temperature control accuracy is ±10°C. The steel plate is tempered at a temperature of 560-640°C. After the furnace reaches the temperature, it is kept warm for 50-120 minutes.
[0038] In order to produce steel plates with a thickness of 180 mm or more, in step (2), a 450 mm cross-section continuous casting machine is used to cast the continuous casting ingot.
[0039] In step (3), the ratio of the thickness of the steel plate after rough rolling to the thickness of the finished product is preferably controlled to be less than 1.1 times.
[0040] Compared with the prior art, the advantages of the present invention are:
[0041] The present application provides a Q690 high-strength steel plate with a compression ratio of ≤2.5 and a thickness of 180-220 mm and a manufacturing method thereof, wherein the steel plate has excellent hardenability.
[0042] This application uses a 450mm cross-section continuous casting machine for low superheat casting. Different from the traditional dynamic light reduction process with a reduction of about 5mm, the present invention uses a heavy reduction process at the end of solidification of the billet. The heavy reduction of the billet is not less than 10mm and not more than 15mm, which fully compensates for defects such as pores and looseness in the center of the billet. The center segregation of the billet is not higher than C1.0 level, and the center looseness is not higher than 1.0 level.
[0043] In order to increase the rolling deformation of the core of the steel plate, the rough rolling is carried out in a high temperature zone, and the rough rolling final rolling temperature is between 1050 and 1100° C. The Nb / V / Ti microalloying is fully utilized to ensure the grain refinement of the extra-thick steel plate during high temperature and large deformation rolling, thereby improving the strength and toughness.
[0044] Unlike the traditional two-stage rolling method that ensures the reduction in the finishing stage, the rolling deformation in this application is mainly completed in the rough rolling stage. The ratio of the thickness of the steel plate after rough rolling to the thickness of the finished product is controlled to be less than 1.2 times (preferably less than 1.1 times), and the number of passes with a reduction of ≥30mm is not less than 3.
[0045] In order to solve the problem of hydrogen-induced delayed cracking of extra-thick high-strength steel plates during subsequent cutting, welding and application, this application adopts a steel plate hydrogen expansion process, with the hydrogen expansion temperature set to 600-700°C and the hydrogen expansion time ≥72 hours.
[0046] The yield strength of the 180-220mm extra-thick steel plate in this application is Rp0.2≥630MPa, the tensile strength is Rm≥710MPa, the elongation is A≥14%; -40℃ low-temperature impact Akv≥47J. The cold bending performance of the steel plate is excellent, d=3a, and there is no crack in 180° cold bending. The steel plate structure is mainly fine tempered troostite and bainite, which meets the application needs of Q690 steel plate for engineering machinery.
[0047] The method of the present application can be extended and applied to other high-strength steel plates, such as high-strength offshore ship plates, high-rise building plates, bridge plates, engineering machinery plates, pressure vessel plates, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is a typical structure of the steel plate involved in Example 1 of the present invention. DETAILED DESCRIPTION
[0049] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0050] The production process of the high-strength steel in this application is: converter steelmaking->LF refining->VD or RH vacuum degassing->Ca treatment->continuous casting->heating->rolling->steel plate hydrogen expansion->quenching and tempering.
[0051] The production method of the extra-thick Q690 high-strength steel plate of Example 1-2 comprises the following steps:
[0052] (1) Smelting: The steel is smelted in a 150-ton converter, then sent to a LF furnace for refining and RH vacuum degassing, and then degassing for Ca treatment. The final composition of the molten steel is shown in Table 1.
[0053] (2) Continuous casting: Molten steel is cast into 450mm thick continuous casting billets. The casting temperature is controlled at 5-20℃ above the liquidus. During the casting process, heavy pressure is applied at the end of the solidification of the billet, and the amount of heavy pressure is not less than 10mm and not more than 15mm. The center segregation of the billet is controlled to be no higher than C1.0 level, and the center looseness is controlled to be no higher than 1.0 level. The relevant process parameters are shown in Table 2.
[0054] (3) Rolling and cooling: The continuous casting billet obtained in step (1) is placed in a walking beam heating furnace and heated to 1200-1250°C for 8-14 min / cm2 to fully dissolve the alloy elements in the steel to ensure the uniformity of the composition and performance of the final product. After the billet is removed from the furnace, it is descaled by high-pressure water and then subjected to two-stage controlled rolling of rough rolling and finishing rolling. In order to increase the rolling deformation of the core of the steel plate, the rough rolling is carried out in a high temperature zone, and the rough rolling and finishing temperatures are between 1050 and 1100°C. The ratio of the thickness of the steel plate after rough rolling to the thickness of the finished product is controlled to be less than 1.2 times, and the number of passes with a reduction of ≥30 mm is not less than 3. The starting rolling temperature of the steel plate finishing rolling is 920-950°C, and the final rolling temperature is ≥850°C. In order to avoid grain growth and not generate large stress, ACC controlled cooling is adopted, and the final cooling temperature is 600-700°C. The relevant process parameters are shown in Table 3.
[0055] (4) Steel plate hydrogen expansion process: After rolling, the steel plate enters the electric furnace with a furnace temperature of ≥300°C, and the steel plate is heated to 600-700°C for ≥72 hours in the furnace to promote the homogenization of the core structure and properties of the steel plate, reduce the H content and internal stress, greatly improve the toughness of the steel plate, and reduce the risk of hydrogen-induced delayed cracking of extra-thick high-strength steel plates. The relevant process parameters are shown in Table 4.
[0056] (5) Heat treatment process: After hydrogen expansion, the steel plate is quenched at a temperature of 880-940°C. After the furnace temperature reaches the temperature, the holding time is 30-90 minutes. To ensure the uniformity of the steel plate, the temperature control accuracy is ±10°C. The steel plate tempering temperature is 560-640°C. After the furnace temperature reaches the temperature, the holding time is 50-120 minutes. The relevant process parameters are shown in Table 4.
[0057] The specific composition and process parameters are shown in Tables 1 to 5. The corresponding properties of each example sample are shown in Table 5.
[0058] Figure 1The microstructure metallographic photograph of the test steel of Example 1 is given. The matrix structure of the steel plate is fine tempered troostite and a small amount of bainite structure, and the grain size of the structure is ≥ 7 levels, ensuring that the steel plate has excellent strength and toughness.
[0059] The present invention adopts a high-cleanliness steelmaking continuous casting process, controlled rolling and controlled cooling, steel plate hydrogen expansion and tempering process, and controls from the perspectives of chemical composition design, parent material structure, rolling deformation, heat treatment temperature and time, etc., to ensure that the steel plate has high strength, high toughness and excellent cold bending performance. It can be widely used in the manufacture of large-scale engineering machinery equipment or steel structures such as high-rise buildings, bridges, and offshore platforms that have strict requirements on formability and weldability.
[0060] Table 1 Chemical composition of the super-strong steel plate of the embodiment (wt%)
[0061]
[0062] Table 2 Continuous casting process control
[0063] Example Superheat, ℃ Weight reduction, mm Center Segregation Loose center 1 20 13 C0.5 0.5 2 15 12 C0.5 0.5
[0064] Table 3 Rolling process control
[0065]
[0066] Table 4 Heat treatment process control
[0067]
[0068] Table 5 Tensile, impact and bending properties of the embodiments of the present invention
[0069]
Claims
1. A low compression ratio thick Q690 high strength steel plate, characterized by: The chemical composition of the steel plate is calculated by mass percentage as follows: C: 0.15-0.20%, Si: 0.10-0.40%, Mn: 1.20-1.50%, Nb: 0.040%-0.060%, V: 0.030%-0.060%, Ti: 0.020%-0.030%, Al: 0.02-0.05%, Ni: 1.00-1.20%, Cu: ≤0.30%, Cr: 0.60-1.00%, Mo: 0.40-0.70%, B: 0.0015-0.0025%, Ca: 0.001-0.005%, P: ≤0.012%, S: ≤0.002%, O: ≤0.002%, N: ≤0.004%, H: ≤0.0002%, the balance is Fe and unavoidable impurity elements; Carbon equivalent CEV: 0.65-0.75%; the thickness of the high-strength steel plate is 180-220 mm; the manufacturing method of the steel plate includes molten steel smelting, continuous casting, hot rolling, hydrogen expansion and tempering steps, wherein: (1) Molten steel smelting Molten steel is smelted according to the chemical composition of the steel plate. The smelting of the molten steel adopts converter smelting, refining outside the furnace and vacuum degassing treatment; (2) Continuous casting During continuous casting, the superheat of molten steel is controlled at 5-20℃, and heavy pressure is applied to the solidification end of the ingot, with the pressure reduction not less than 10mm and not more than 15mm; the center segregation of the ingot is controlled not to be higher than C1.0 level, and the center porosity is controlled not to be higher than 1.0 level; (3) Heating rolling The ingot is heated to 1200-1250℃, and the heating time is 8-14min / cm. After the ingot is taken out of the furnace, it is subjected to two-stage controlled rolling of rough rolling + finishing rolling. The final rolling temperature of rough rolling is 1050-1100℃, and the ratio of the thickness of the steel plate after rough rolling to the thickness of the finished product is controlled to be less than 1.2 times, and the number of passes with a reduction of ≥30mm is not less than 3; the starting rolling temperature of finishing rolling is 920-950℃, and the final rolling temperature is ≥850℃. After the steel plate is rolled, ACC is used for controlled cooling, and the final cooling temperature is 600-700℃; (4) Hydrogen expansion of steel plates After rolling, the steel plate is put into the furnace for hydrogen expansion. The furnace temperature is ≥300℃. The steel plate is heated to 600~700℃ and the furnace time is ≥72 hours. (5) Quenching and tempering: After hydrogen expansion, the steel plate is quenched at a temperature of 880-940°C. After the furnace temperature reaches the required temperature, the steel plate is kept warm for 30-90 minutes. The steel plate is tempered at a temperature of 560-640°C. After the furnace temperature reaches the required temperature, the steel plate is kept warm for 50-120 minutes.
2. The low compression specific thickness Q690 high strength steel plate according to claim 1, characterized in that: The microstructure of the steel plate is tempered troostite and bainite.
3. The low compression specific thickness Q690 high strength steel plate according to claim 1, characterized in that: Yield strength ≥630MPa, tensile strength ≥710MPa, elongation ≥14%; -40℃ low temperature Charpy impact energy ≥47J; d=3a, 180° cold bending without cracks.
4. The low compression specific thickness Q690 high strength steel plate according to claim 1, characterized in that: In step (2), a 450 mm cross-section continuous casting machine is used to cast the continuous casting billet.
5. The low compression specific thickness Q690 high strength steel plate according to claim 1, characterized in that: In step (3), the ratio of the thickness of the steel plate after rough rolling to the thickness of the finished product is controlled to be less than 1.1 times.
Citation Information
Cited By
Small-compression-bit thick quenched and tempered steel plate and production method thereof
CN117926105A