A low-carbon equivalent high-toughness NM400 wear-resistant steel plate and its production method
By controlling chemical composition and process steps, the problem of the reduction of toughness of NM400 wear-resistant steel is solved, and a low-carbon equivalent NM400 wear-resistant steel plate with high strength, high toughness and excellent welding performance is produced to meet the wear resistance of excavators and other equipment and impact performance requirements.
Patent Information
- Application Number
- CN202311082350.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-08-27
AI Technical Summary
When the existing NM400 wear-resistant steel increases hardness and improves wear resistance, its toughness will be reduced, making it difficult to meet the requirements of high wear resistance and high impact toughness at the same time.
By controlling the chemical composition range and process steps, including converter smelting, refining, continuous casting, heating, rolling and heat treatment, low-carbon equivalent chemical composition and alloy elements are used, combined with two-stage controlled rolling and quenching + tempering processes, the steel plate is controlled by controlling the steel plate. The hardness and grain refinement ensure the high strength and toughness characteristics of the steel plate and excellent welding performance.
It produces low-carbon equivalent high-toughness NM400 wear-resistant steel plate with excellent mechanical properties and welding properties, with a hardness of 370~430HBW, tensile strength ≥1200MPa, elongation ≥14%, satisfying high impact toughness and low temperature impact performance, suitable for Excavators and other equipment.
Smart Images

Figure CN117107155B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and relates to a low-carbon equivalent high-toughness NM400 wear-resistant steel plate and a production method thereof. Background Art
[0002] NM400 wear-resistant steel is widely used in special engineering equipment such as excavators and dump trucks. The wear resistance of steel can be effectively improved by increasing hardness; but too high hardness will reduce the toughness of steel. The performance of NM400 wear-resistant steel usually requires a hardness of 370-430 HBW and a tensile strength of ≥1200 MPa. Summary of the invention
[0003] The purpose of the present invention is to provide a low carbon equivalent high toughness NM400 wear-resistant steel plate and a production method thereof. The produced wear-resistant steel plate has a thickness specification of 6 to 25 mm and meets the requirements of high wear resistance and high impact toughness.
[0004] The technical solution of the present invention:
[0005] A low carbon equivalent high toughness NM400 wear-resistant steel plate, the chemical composition percentage of the steel is C = 0.14% ~ 0.16%, Si = 0.15% ~ 0.35%, Mn = 1.15% ~ 1.35%, P ≤ 0.012%, S ≤ 0.003%, Cr = 0.15% ~ 0.25%, Nb = 0.015% ~ 0.025%, Ti = 0.012% ~ 0.025%, Al = 0.020% ~ 0.0 60%, B=0.0014%~0.0030%, H≤0.0002%, N≤0.0060%, O≤0.0015%, the rest are Fe and unavoidable impurities, CEV≤0.42%; the hardness of the steel is 370~430HBW, the tensile strength is ≥1200MPa, the elongation is ≥14%, it meets 2a radius 180° cold bending, -20℃ impact Akv≥50J, -40℃ impact Akv≥40J.
[0006] Further, the chemical composition percentages of the optimized steel are C=0.14%~0.15%, Si=0.25%~0.30%, Mn=1.15%~1.25%, P≤0.012%, S≤0.003%, Cr=0.15%~0.20%, Nb=0.015%~0.025%, Ti=0.012%~0.020%, Al=0.030%~0.060%, B=0.0014%~0.0020%, H≤0.0002%, N≤0.0060%, O≤0.0010%, and the rest are Fe and unavoidable impurities, CEV≤0.40%.
[0007] A method for producing a low carbon equivalent high toughness NM400 wear-resistant steel plate, the key process steps comprising:
[0008] (1) Converter smelting: top and bottom double-blowing converter, control the tapping temperature at 1560-1640°C, converter tapping P ≤ 0.010%, add deoxidizer and alloy for deoxidation and alloying during tapping, and use low P alloy to avoid P increase in molten steel;
[0009] (2) Refining: After the molten steel in the ladle is heated by electricity in the LF furnace, the chemical composition is precisely adjusted, and then it enters the RH furnace or VD furnace for vacuum treatment. The gas content of the molten steel is measured at the exit station: H≤0.00015%, N≤0.0060%, and O≤0.0015%;
[0010] (3) Continuous casting: The tundish superheat is 8-30°C. Dynamic light pressure or heavy pressure technology is used to improve the internal quality of the continuous casting billet. The thickness of the continuous casting billet is 180-300 mm and the width is 1700-2500 mm.
[0011] (4) Heating: preheating section temperature 650 ~ 900 ° C, heating section temperature 1100 ~ 1260 ° C, soaking section temperature 1150 ~ 1250 ° C, furnace time 160 ~ 300 min;
[0012] (5) Rolling: two-stage controlled rolling is adopted, the rough rolling temperature is 1150-980°C, the rough rolling cumulative compression ratio is ≥2, the intermediate billet thickness is 60-90 mm, the finishing rolling start temperature is 880-1030°C, the finishing rolling cumulative compression ratio is ≥3, and the finishing rolling final rolling temperature is 800-860°C;
[0013] (6) Heat treatment: adopt quenching + tempering process, quenching heating temperature 860 ~ 900 ° C, heating rate 1.4 ~ 2.0 min / mm, holding time 10 ~ 30 min, quenching cooling rate 20 ~ 40 ° C / s; tempering heating temperature 180 ~ 230 ° C, heating rate 3.0 ~ 4.5 min / mm, holding time 10 ~ 20 min.
[0014] Optimized, step (3) continuous casting: in, the superheat of the middle package is 8-20°C.
[0015] Optimally, in step (6) of heat treatment, the quenching heating temperature is 880-900°C, and the tempering heating temperature is 200-220°C.
[0016] Principle of the invention: The wear-resistant steel of the present invention has high strength and high toughness characteristics, and also has good welding performance and forming performance. The hardness range of the steel plate is ensured to hit the target requirements by controlling the C range, the hardenability of the steel plate is improved by adding Mn, B and a small amount of Si and Cr to ensure uniform structure of the steel plate, the strength performance of the steel plate is improved by means of structure strengthening and alloy strengthening, the grains are refined by the precipitates of Nb, Ti and Al and the appropriate rolling heat treatment process to achieve the purpose of improving impact toughness, and at the same time, the P, S, H, N and O of the molten steel are strictly controlled. The present invention ensures a lower CEV and excellent mechanical properties, welding properties and processing properties through appropriate alloy element ratios and subsequent rolling heat treatment processes.
[0017] Beneficial effects of the present invention: The wear-resistant steel produced by the method of the present invention has excellent low-temperature toughness and weldability, and its mechanical properties are as follows: hardness 370-430 HBW, tensile strength ≥1200 MPa, elongation ≥14%, meeting 2a radius 180° cold bending, -20℃ impact Akv ≥50J, -40℃ impact Akv ≥40J. It can be used for wear-resistant parts and structural parts such as excavators and dump trucks, has excellent mechanical properties and excellent welding and forming properties, and is a promising green steel product. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 2 is a metallographic structure photograph of an embodiment of the present invention. DETAILED DESCRIPTION
[0019] Embodiment 1:
[0020] A furnace of wear-resistant steel is smelted to produce steel plates with specifications of 8mm, 14mm and 25mm respectively. The chemical composition weight percentage of the steel is shown in Table 1; the following key process steps are included:
[0021] (1) Converter smelting: top and bottom combined blowing converter smelting is adopted, the tapping temperature is 1568°C, the P content of converter tapping end point is 0.006%, alloying is carried out during the tapping process, deoxidizers such as aluminum iron and aluminum blocks are added, and low-phosphorus alloys such as low-carbon ferrochrome, silicon-manganese alloy, medium-carbon ferromanganese, and medium-carbon ferroboron are added;
[0022] (2) Refining: The LF furnace is heated and the composition is adjusted. After the composition adjustment, the temperature is raised to 1615°C and the furnace is put into the RH furnace for vacuum treatment. The vacuum time is maintained for 10 minutes. After the vacuum is broken, the furnace is soft-blown and allowed to stand for 20 minutes. Samples are taken for testing. H = 0.00013%, N = 0.0032%, O = 0.0007%;
[0023] (3) Continuous casting: The liquidus of molten steel is about 1514°C, the temperature of the tundish is controlled at 1525-1532°C, and the continuous casting adopts dynamic soft reduction. The cross-sectional size of the continuous casting billet is 220×2070mm;
[0024] (4) Heating: The heating system is as follows: preheating section 800°C, heating section 1100-1260°C, soaking section temperature 1170-1240°C, slab out-of-furnace temperature 1210-1250°C, and furnace time 180-230 min;
[0025] (5) Rolling: Rolling 8, 14, and 25 mm steel plates using two-stage controlled rolling. The rolling process parameters are shown in Table 2.
[0026] (6) Heat treatment: quenching heating temperature 880°C, tempering temperature 200°C. Detailed heat treatment parameters are shown in Table 3.
[0027] Embodiment 2:
[0028] One furnace of wear-resistant steel was smelted to produce steel plates with specifications of 12 mm and 20 mm. The chemical composition weight percentage of the steel is shown in Table 1. The key process steps are as follows:
[0029] (1) Converter smelting: top and bottom combined blowing converter smelting is adopted, the tapping temperature is 1582°C, the P content of converter tapping end point is 0.009%, alloying is carried out during the tapping process, deoxidizers such as aluminum iron and aluminum blocks are added, and low-phosphorus alloys such as low-carbon ferrochrome, silicon-manganese alloy, medium-carbon ferromanganese, and medium-carbon ferroboron are added;
[0030] (2) Refining: LF furnace is heated and the composition is adjusted. After the composition adjustment, the temperature is raised to 1631°C and the furnace is put into VD furnace for vacuum treatment. The vacuum time is 13 minutes. After the vacuum is broken, the furnace is soft-blown and left to stand for 21 minutes. Samples are taken for testing. H = 0.00016%, N = 0.0036%, O = 0.0008%;
[0031] (3) Continuous casting: The liquidus of molten steel is about 1514°C, the temperature of the tundish is controlled at 1526-1534°C, and the continuous casting adopts dynamic soft reduction. The cross-sectional size of the continuous casting billet is 260×2070mm;
[0032] (4) Heating: The heating system is as follows: preheating section 850°C, heating section 1100-1260°C, soaking section 1180-1240°C, slab out-of-furnace temperature 1200-1220°C, and furnace time 190-230 min;
[0033] (5) Rolling: Rolling 12 and 20 mm steel plates using two-stage controlled rolling. The rolling process parameters are shown in Table 2.
[0034] (6) Heat treatment: quenching heating temperature 900 °C, tempering temperature 230 °C, detailed heat treatment parameters are shown in Table 3.
[0035] The mechanical properties test results of the obtained steel plates are shown in Table 4.
[0036] Table 1 Chemical composition of the examples Mass percentage (wt.%)
[0037] Example C Si Mn P S Alt Nb V Ti Cr Mo Ni Cu B CEV 1 0.16 0.27 1.23 0.009 0.002 0.035 0.017 0.004 0.017 0.16 0.01 0.02 0.02 0.0013 0.40 2 0.15 0.25 1.19 0.012 0.001 0.044 0.014 0.003 0.020 0.19 0.02 0.02 0.02 0.0017 0.39
[0038] Table 2 Example rolling process parameters
[0039]
[0040] Table 3 Example heat treatment process parameters
[0041]
[0042] Table 4 Mechanical properties test results of the examples
[0043]
[0044] Note: 8mm impact is a thinned specimen with a size of 5mm×10mm; 10mm impact is a thinned specimen with a size of 7.5mm×10mm; ≥12mm impact is a standard specimen with a size of 10mm×10mm.
Claims
1. A method for producing a low carbon equivalent high toughness NM400 wear-resistant steel plate, producing an 8mm specification steel plate, characterized in that: The chemical composition of the steel is C=0.16%, Si=0.27%, Mn=1.23%, P=0.009%, S=0.002%, Alt=0.035%, Cr=0.16%, Nb=0.017%, V=0.004%, Ti=0.017%, Mo=0.01%, Ni=0.02%, Cu=0.02%, B=0.0013%, the rest is Fe and unavoidable impurities, CEV=0.40%; the hardness of the steel is 417 / 419 / 420HBW, the tensile strength is 1329MPa, the elongation is 15.5%, it meets the 2a radius 180° cold bending, the -20℃ impact Akv is 65 / 63 / 66J, and the -40℃ impact Akv is 41 / 45 / 42J; The process steps include: (1) Converter smelting: top and bottom combined blowing converter smelting is adopted, the tapping temperature is 1568℃, and the converter tapping P is 0.006%; deoxidizer aluminum iron and aluminum blocks are added during the tapping process for deoxidation; low carbon ferrochrome, silicon manganese alloy, medium carbon ferromanganese and medium carbon ferroboron with low P content are added for alloying to avoid P increase in molten steel; (2) Refining: The LF furnace is heated and the composition is adjusted. After the composition adjustment, the temperature is raised to 1615℃ and the furnace is put into the RH furnace for vacuum treatment. The vacuum time is 10 minutes. After the vacuum is broken, the furnace is soft-blown and left for 20 minutes. Samples are taken for testing. H=0.00013%, N=0.0032%, O=0.0007%; (3) Continuous casting: The temperature of the tundish is controlled at 1525-1532°C, dynamic soft reduction is adopted for continuous casting, and the cross-sectional size of the continuous casting billet is 220×2070mm; (4) Heating: The heating system is as follows: preheating section 800°C, heating section 1100-1260°C, soaking section temperature 1170-1240°C, slab out-of-furnace temperature 1210-1250°C, and furnace time 180-230 min; (5) Rolling: Rolling 8mm steel plate, billet thickness 220mm, intermediate billet thickness 60mm; adopt two-stage controlled rolling, finishing rolling start temperature 1022℃, final rolling temperature 857℃; (6) Heat treatment: quenching heating temperature 880℃, time 26 minutes, cooling method is water cooling; tempering heating temperature 200℃, time 40 minutes, cooling method is air cooling.
2. A method for producing a low carbon equivalent high toughness NM400 wear-resistant steel plate, producing a 14mm specification steel plate, characterized in that: The chemical composition of the steel is C=0.16%, Si=0.27%, Mn=1.23%, P=0.009%, S=0.002%, Alt=0.035%, Cr=0.16%, Nb=0.017%, V=0.004%, Ti=0.017%, Mo=0.01%, Ni=0.02%, Cu=0.02%, B=0.0013%, the rest is Fe and unavoidable impurities, CEV=0.40%; the hardness of the steel is 420 / 422 / 425HBW, the tensile strength is 1369MPa, the elongation is 18.0%, it meets the 2a radius 180° cold bending, the -20℃ impact Akv is 99 / 93 / 94J, and the -40℃ impact Akv is 68 / 65 / 70J; The process steps include: (1) Converter smelting: top and bottom combined blowing converter smelting is adopted, the tapping temperature is 1568℃, and the converter tapping P is 0.006%; deoxidizer aluminum iron and aluminum blocks are added during the tapping process for deoxidation; low carbon ferrochrome, silicon manganese alloy, medium carbon ferromanganese and medium carbon ferroboron with low P content are added for alloying to avoid P increase in molten steel; (2) Refining: The LF furnace is heated and the composition is adjusted. After the composition adjustment, the temperature is raised to 1615℃ and the furnace is put into the RH furnace for vacuum treatment. The vacuum time is 10 minutes. After the vacuum is broken, the furnace is soft-blown and left for 20 minutes. Samples are taken for testing. H=0.00013%, N=0.0032%, O=0.0007%; (3) Continuous casting: The temperature of the tundish is controlled at 1525-1532°C, dynamic soft reduction is adopted for continuous casting, and the cross-sectional size of the continuous casting billet is 220×2070mm; (4) Heating: The heating system is as follows: preheating section 800°C, heating section 1100-1260°C, soaking section temperature 1170-1240°C, slab out-of-furnace temperature 1210-1250°C, and furnace time 180-230 min; (5) Rolling: Rolling 14mm steel plate, billet thickness 220mm, intermediate billet thickness 70mm; adopt two-stage controlled rolling, finishing rolling start temperature 978℃, final rolling temperature 838℃; (6) Heat treatment: quenching heating temperature 880℃, time 31 minutes, cooling method is water cooling; tempering heating temperature 200℃, time 57 minutes, cooling method is air cooling.
3. A method for producing a low carbon equivalent high toughness NM400 wear-resistant steel plate, producing a 25mm specification steel plate, characterized in that: The chemical composition of the steel is C=0.16%, Si=0.27%, Mn=1.23%, P=0.009%, S=0.002%, Alt=0.035%, Cr=0.16%, Nb=0.017%, V=0.004%, Ti=0.017%, Mo=0.01%, Ni=0.02%, Cu=0.02%, B=0.0013%, the rest is Fe and unavoidable impurities, CEV=0.40%; the hardness of the steel is 414 / 417 / 420HBW, the tensile strength is 1240MPa, the elongation is 16.5%, it meets the 2a radius 180° cold bending, the -20℃ impact Akv is 62 / 75 / 68J, and the -40℃ impact Akv is 45 / 49 / 48J; The process steps include: (1) Converter smelting: top and bottom combined blowing converter smelting is adopted, the tapping temperature is 1568℃, and the converter tapping P is 0.006%; deoxidizer aluminum iron and aluminum blocks are added during the tapping process for deoxidation; low carbon ferrochrome, silicon manganese alloy, medium carbon ferromanganese and medium carbon ferroboron with low P content are added for alloying to avoid P increase in molten steel; (2) Refining: The LF furnace is heated and the composition is adjusted. After the composition adjustment, the temperature is raised to 1615℃ and the furnace is put into the RH furnace for vacuum treatment. The vacuum time is 10 minutes. After the vacuum is broken, the furnace is soft-blown and left for 20 minutes. Samples are taken for testing. H=0.00013%, N=0.0032%, O=0.0007%; (3) Continuous casting: The temperature of the tundish is controlled at 1525-1532°C, dynamic soft reduction is adopted for continuous casting, and the cross-sectional size of the continuous casting billet is 220×2070mm; (4) Heating: The heating system is as follows: preheating section 800°C, heating section 1100-1260°C, soaking section temperature 1170-1240°C, slab out-of-furnace temperature 1210-1250°C, and furnace time 180-230 min; (5) Rolling: Rolling 25mm steel plate, billet thickness 220mm, intermediate billet thickness 80mm; adopt two-stage controlled rolling, finishing rolling start temperature 886℃, final rolling temperature 826℃; (6) Heat treatment: quenching heating temperature 880℃, time 48 minutes, cooling method is water cooling; tempering heating temperature 200℃, time 102 minutes, cooling method is air cooling.
4. A method for producing a low carbon equivalent high toughness NM400 wear-resistant steel plate, producing a 12mm specification steel plate, the chemical composition of the steel is C=0.15%, Si=0.25%, Mn=1.19%, P=0.012%, S=0.001%, Alt=0.044%, Cr=0.19%, Nb=0.014%, V=0.003%, Ti=0.020%, Mo=0.02%, N i=0.02%, Cu=0.02%, B=0.0017%, the rest is Fe and unavoidable impurities, CEV=0.39%; the hardness of the steel is 411 / 412 / 415HBW, the tensile strength is 1337MPa, the elongation is 15.0%, it meets the 2a radius 180° cold bending, the -20℃ impact Akv is 70 / 74 / 69J, and the -40℃ impact Ak is 55 / 47 / 44J; the following process steps are included: (1) Converter smelting: top and bottom combined blowing converter smelting is adopted, the tapping temperature is 1582℃, the converter tapping end point P=0.009%, deoxidizer aluminum iron and aluminum block are added for deoxidation during the tapping process, and low carbon ferrochrome, silicon manganese alloy, medium carbon ferromanganese and medium carbon ferroboron with low P content are added for alloying to avoid P increase in molten steel; (2) Refining: LF furnace is heated and the composition is adjusted. After the composition adjustment, the temperature is raised to 1631℃ and the furnace is put into VD furnace for vacuum treatment. The vacuum time is 13 minutes. After the vacuum is broken, the furnace is soft-blown and left for 21 minutes. The samples are tested for H=0.00016%, N=0.0036%, and O=0.0008%; (3) Continuous casting: The temperature of the tundish is controlled at 1526-1534°C, dynamic soft reduction is adopted for continuous casting, and the cross-sectional size of the continuous casting billet is 260×2070mm; (4) Heating: The heating system is as follows: preheating section 850°C, heating section 1100-1260°C, soaking section 1180-1240°C, slab out-of-furnace temperature 1200-1220°C, and furnace time 190-230 min; (5) Rolling: Rolling 12mm steel plate, billet thickness 260mm, intermediate billet thickness 65mm; adopt two-stage controlled rolling, finishing rolling start temperature 933℃, final rolling temperature 803℃; (6) Heat treatment: quenching heating temperature 900℃, time 28 minutes, cooling method is water cooling; tempering heating temperature 230℃, time 49 minutes, cooling method is air cooling.
5. A method for producing a low carbon equivalent high toughness NM400 wear-resistant steel plate, producing a 20 mm specification steel plate, the chemical composition of the steel is C=0.15%, Si=0.25%, Mn=1.19%, P=0.012%, S=0.001%, Alt=0.044%, Cr=0.19%, Nb=0.014%, V=0.003%, Ti=0.020%, Mo=0.02%, N i=0.02%, Cu=0.02%, B=0.0017%, the rest is Fe and unavoidable impurities, CEV=0.39%; the hardness of the steel is 417 / 420 / 418 HBW, the tensile strength is 1361 MPa, the elongation is 15.5%, it meets the 2a radius 180° cold bending, the -20℃ impact Akv is 68 / 65 / 67J, and the -40℃ impact Akv is 42 / 48 / 46J; the following process steps are included: (1) Converter smelting: top and bottom combined blowing converter smelting is adopted, the tapping temperature is 1582℃, the converter tapping end point P=0.009%, deoxidizer aluminum iron and aluminum block are added for deoxidation during the tapping process, and low carbon ferrochrome, silicon manganese alloy, medium carbon ferromanganese and medium carbon ferroboron with low P content are added for alloying to avoid P increase in molten steel; (2) Refining: LF furnace is heated and the composition is adjusted. After the composition adjustment, the temperature is raised to 1631℃ and the furnace is put into VD furnace for vacuum treatment. The vacuum time is 13 minutes. After the vacuum is broken, the furnace is soft-blown and left for 21 minutes. The samples are tested for H=0.00016%, N=0.0036%, and O=0.0008%; (3) Continuous casting: The temperature of the tundish is controlled at 1526-1534°C, dynamic soft reduction is adopted for continuous casting, and the cross-sectional size of the continuous casting billet is 260×2070mm; (4) Heating: The heating system is as follows: preheating section 850°C, heating section 1100-1260°C, soaking section 1180-1240°C, slab out-of-furnace temperature 1200-1220°C, and furnace time 190-230 min; (5) Rolling: Rolling 20 mm steel plate, billet thickness 260 mm, intermediate billet thickness 85 mm; adopting two-stage controlled rolling, finishing rolling start temperature 881 ° C, final rolling temperature 811 ° C; (6) Heat treatment: quenching heating temperature 900℃, time 43 minutes, cooling method is water cooling; tempering heating temperature 230℃, time 88 minutes, cooling method is air cooling.
Citation Information
Patent Citations
Low-carbon-equivalent high-strength wear-resistant steel plate and production method thereof
CN101748333A
Wearable steel plate with low cost and high strength and producing method thereof
CN101928891A
Method for producing wear-resisting steel plate
CN102363859A
Production method of wear-resistant steel with high toughness
CN103540729A
Production method of wear-resistant steel plate having high strength and high toughness
CN104789881A
Cited By
Production method of NM400TiCe rare earth wear-resistant steel
CN121428224A