Lithium-rich manganese-based solid-state lithium battery and preparation method thereof
By adopting the collaborative design of ferroelectric polymer positive electrode and modified separator in lithium-rich manganese-based batteries, combined with in-situ assembly and gradient heat treatment, the capacity and cycle stability of lithium-rich manganese-based materials in solid-state batteries is solved. Problem, achieving better battery performance.
Patent Information
- Application Number
- CN202410286315.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-03-13
AI Technical Summary
The capacity and high-rate cycle stability of lithium-rich manganese-based materials in solid-state batteries are not ideal, and it is difficult to adapt to the application requirements of solid-state batteries, resulting in deteriorating capacity and cycle stability at high-rates.
By using a co-design of a positive electrode material containing ferroelectric polymer and a ferroelectric polymer modified separator in lithium-rich manganese-based batteries, combined with in-situ assembly and gradient heat treatment technology, the physical and chemical characteristics and interface contact of lithium-rich manganese-based materials are improved by combining with the following methods: Effects, enhance its adaptability to solid-state batteries.
The capacity and high-rate cycle stability of lithium-rich manganese-based batteries in solid-state batteries have been significantly improved, and their adaptation problems in solid-state batteries have been solved, thus achieving better capacity and cycle stability performance.
Smart Images

Figure CN118213598B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium battery materials and manufacturing technology, and in particular to a high-specific-energy and high-rate lithium-rich manganese-based solid-state lithium battery and a manufacturing method thereof. Background Art
[0002] Since Sony launched the first commercialized LiCoO2 lithium battery in 1991, lithium-ion batteries have experienced explosive growth. However, from the perspective of battery technology development, the actual energy density of lithium-ion batteries at this stage is approaching the limit of improvement, and cannot meet the increasingly thin, intelligent and multifunctional development of electronic devices. In addition, according to the battery technology development route, in 2025, the energy density of lithium-ion batteries will be further increased to 400Wh / kg, and the battery cost will be reduced to less than 0.6 yuan / Wh. By 2030, the battery energy density can reach 500Wh / kg. To achieve this goal, the positive electrode material needs to transition from high-nickel ternary positive electrode to lithium-rich manganese-based positive electrode material with higher specific capacity and lower cost, while the negative electrode material will shift from graphite negative electrode to silicon-based negative electrode or metal negative electrode. In addition, in order to solve the problems of transition metal ion dissolution, interface instability and safety hazards of high-voltage and high-energy lithium-rich batteries, the electrolyte will shift from liquid to semi-solid or all-solid.
[0003] Unfortunately, due to the intrinsic properties of the lithium-rich manganese-based positive electrode, it is difficult to effectively exert its high capacity and stability. In addition, it is difficult to adapt to the application requirements of solid-state batteries and difficult to adapt to the (semi-) solid electrolytes in solid-state batteries. This will further amplify the intrinsic disadvantages of the lithium-rich manganese-based positive electrode, and further deteriorate the rate performance and cycle stability of the lithium-rich manganese-based solid-state battery, which limits its application areas.
[0004] In view of the problem that lithium-rich manganese-based materials are difficult to adapt to the application requirements of solid-state batteries, the existing means mainly lie in the modification research of lithium-rich manganese-based positive electrode materials. For example, the Chinese patent document with publication number CN115676910A discloses a lithium-rich manganese-based positive electrode material and a preparation method thereof, and specifically reports a scheme of coating by a material containing an A element compound and a lithium source. For another example, the Chinese patent document with publication number CN109638233A discloses a solid ion conductor and a lithium-rich manganese-based material composite electrode and a lithium ion battery, wherein the positive electrode material includes a lithium-rich manganese-based material and a solid ion conductor, wherein the chemical formula of the lithium-rich manganese-based material is xLi2MnO3·(1-x)LiMO2, wherein 0<x<1, and M is one or more of Mn, Ni, and Co; and the chemical formula of the solid ion conductor is Li1+a[AbB2-c(DO4)3] or Li2+αEβG3+γ.
[0005] In summary, most of the existing technologies focus on the modification of lithium-rich manganese-based positive electrode materials. There are few reports on improving the capacity and high-rate cycling stability of lithium-rich manganese-based solid-state batteries through the coordination between battery components such as positive electrodes and separators without changing the basic physical and chemical structure of lithium-rich manganese. Summary of the invention
[0006] In response to the problems of unsatisfactory capacity and high-rate cycle stability of solid-state batteries caused by intrinsic defects of lithium-rich manganese-based materials, the present invention provides a lithium-rich manganese-based solid-state battery, which aims to improve the problems of unsatisfactory capacity and high-rate cycle stability caused by intrinsic defects of lithium-rich manganese-based batteries through coordinated control of positive electrodes and separators.
[0007] The second purpose of the present invention is to provide a method for preparing the lithium-rich manganese-based solid-state battery.
[0008] The intrinsic physical and chemical characteristics of lithium-rich manganese-based materials make it difficult for them to exert ideal capacity and high-rate cycle stability. Building them into solid-state batteries will further increase the degradation of capacity and high-rate cycle stability of lithium-rich manganese-based materials. In view of this problem, the present invention has conducted in-depth research and provided the following improvement scheme:
[0009] A lithium-rich manganese-based solid-state battery, comprising a battery cell and a solid or semi-solid electrolyte arranged in the battery cell; wherein the battery cell comprises a positive electrode, a separator and a negative electrode which are composited in sequence;
[0010] The positive electrode comprises a current collector and a positive electrode material composited on the surface thereof, wherein the positive electrode material comprises a conductive agent, a ferroelectric polymer and a lithium-rich manganese-based active material;
[0011] The diaphragm comprises a base film and a ferroelectric polymer modified layer compounded on the surface thereof;
[0012] The ferroelectric polymer includes at least one of ferroelectric PVDF, ferroelectric P (VDF-TrFE), ferroelectric P (VDF-TrFE-CTFE), and ferroelectric P (VDF-HFP).
[0013] The innovative research of the present invention shows that the combination of a lithium-manganese-rich positive electrode containing a ferroelectric polymer and the ferroelectric polymer modified diaphragm can unexpectedly achieve synergy. Without changing the basic characteristics of the lithium-manganese-rich positive electrode, it can also effectively solve the problem of its difficulty in adapting to the applicable requirements of solid-state batteries, and can enable it to still exhibit excellent capacity and cycle stability at high rates in a solid-state battery system.
[0014] In the present invention, the lithium-rich manganese-based active material can be any lithium-rich manganese-based active material known in the industry, for example, it can be: Li a Mn b Nic Co d O2; 1 of them<a≤1.5;0.4≤b≤0.8;0≤c≤0.4;0≤d≤0.4;b> c>d, or a lithium-rich material obtained by doping and / or coating thereof. The doped and / or coated elements include at least one of Al, La, Ce, Nd, and Y, and the content thereof can be adjusted according to conventional principles, for example, below 1 mol%.
[0015] In the present invention, the conductive agent includes at least one of Super P, KS-6 and Ketjen black; further, the weight ratio may be 0.1-2:0.1-2:0.1-2, further, the weight ratio may be 0.5-1.5:05-1.5:0.5-1.5 of Super P, KS-6 and Ketjen black composite conductive agent.
[0016] In the present invention, the ferroelectric polymer can be a commercial product or constructed based on a known method. The present invention is preferably obtained by assembling a precursor polymer in DMF; the precursor polymer includes at least one of PVDF, P (VDF-TrFE), P (VDF-TrFE-CTFE), and P (VDF-HFP).
[0017] In the present invention, in the positive electrode material, the weight ratio of the conductive agent, the ferroelectric polymer and the lithium-rich manganese-based active material is 0.01-0.1:0.01-0.1:0.8-0.98, and can further be 0.02-0.05:0.01-0.05:0.9-0.98.
[0018] The positive electrode of the present invention is a non-in-situ assembled positive electrode or an in-situ assembled positive electrode; the non-in-situ assembled positive electrode is obtained by coating and drying a positive electrode material comprising a conductive agent, a ferroelectric polymer and a lithium-rich manganese-based active material after solvent slurry;
[0019] The in-situ assembled positive electrode is obtained by coating a conductive agent, a precursor polymer and a lithium-rich manganese-based active material on a current collector after being slurried with DMF, and then being in-situ assembled through heat treatment.
[0020] The innovative research of the present invention shows that the use of the in-situ assembled positive electrode can unexpectedly further improve the physicochemical characteristics and interface contact effects of the components, can unexpectedly further improve its synergy with the diaphragm, and can unexpectedly further make the lithium-rich manganese-based active material more adaptable to the solid-state battery, so that it can exhibit better capacity and high-rate cycle stability.
[0021] In the present invention, during the in-situ assembled positive electrode preparation process, the temperature of the heat treatment is 60-100°C;
[0022] Preferably, the heat treatment process includes two stages of heat treatment, wherein the first stage of heat treatment is carried out at normal pressure and the second stage of heat treatment is carried out at negative pressure. The negative pressure refers to a pressure below 1 atm (1 atmosphere), and considering the cost, it can be further 0.001 to 0.5 atm, and further can be 0.1 to 0.3 atm.
[0023] Preferably, the temperature of the first heat treatment is preferably 75-85°C, and the temperature of the second heat treatment is 95-100°C. Studies have shown that the two-stage gradient heat treatment is helpful to improve the in-situ phase assembly transformation and interface bonding effect of PVDF, and helps to synergistically improve the application requirements of lithium-rich manganese-based materials that are difficult to adapt to solid-state batteries, and can further improve its capacity and cycle stability in solid-state batteries.
[0024] In the present invention, the time of the first heat treatment process is 0.5 to 3 hours, preferably 1.5 to 2.5 hours;
[0025] Preferably, the second heat treatment time is 5 to 15 hours, preferably 6 to 15 hours, and more preferably 8 to 12 hours.
[0026] The research of the present invention also unexpectedly discovered that based on the in-situ assembly process, further coordinating the two-stage heat treatment process and the joint control of pressure can unexpectedly further improve the synergistic effect of the diaphragm, making it further adapted to the application requirements of solid-state batteries, and can enable it to exhibit better capacity and high-rate cycle stability.
[0027] In the present invention, in the separator, the base film is at least one of PE and PP;
[0028] Preferably, the diaphragm is an ex-situ assembled diaphragm or an in-situ assembled diaphragm, wherein the ex-situ assembled diaphragm is prepared by slurrying a ferroelectric polymer, coating it on a base film, and drying it;
[0029] The in-situ assembled diaphragm is obtained by coating the precursor polymer and DMF slurry on the base film and then thermally assembling it. The present invention has found that the in-situ assembled diaphragm can further improve the structural stability and conduction network of the diaphragm, and it can have better synergy with the positive electrode, making it more suitable for the application requirements of solid-state batteries, and making it show better capacity and high-rate cycle stability.
[0030] Preferably, the temperature of the thermal assembly process is 60-90°C.
[0031] Preferably, the thermal assembly process includes a first thermal process and a second thermal process, wherein the second thermal process is performed under a pressure of 0.05 to 0.1 atm.
[0032] Preferably, the temperature of the first heat treatment process is 60-65°C, and the temperature of the second heat treatment process is 70-80°C.
[0033] Preferably, the total time of thermal assembly is preferably 4 to 24 hours. When the preferred two-stage gradient assembly process is selected, the time of the first thermal process is preferably 1 to 3 hours, and the insulation time of the second thermal process is preferably 6 to 15 hours, and more preferably 8 to 12 hours.
[0034] The research of the present invention also unexpectedly discovered that based on the in-situ assembly process, further coordinating the two-stage heat treatment process and the joint control of pressure can unexpectedly further enhance the synergistic effect of the positive electrode, making it further adapted to the application requirements of solid-state batteries, and enabling it to exhibit better capacity and high-rate cycle stability.
[0035] In the battery of the present invention, except for the positive electrode and separator combined with the present invention, other components, structures and ingredients can be well known in the industry.
[0036] For example, the negative electrode described in the present invention is a graphite negative electrode, a silicon-carbon negative electrode, a silicon-oxygen negative electrode, a metal lithium negative electrode or a current collector negative electrode.
[0037] In the present invention, the solid electrolyte includes, for example, one or more of a polymer solid electrolyte, an oxide solid electrolyte, and a sulfide solid electrolyte;
[0038] In the present invention, the solid electrolyte is prepared by an in-situ or non-in-situ method.
[0039] In the present invention, the lithium-rich manganese-based solid-state battery is in the form of a soft pack, a cylinder, a square or a button.
[0040] The present invention also provides an in-situ preparation method of the lithium-rich manganese-based solid-state battery, obtaining the positive electrode and the separator, and then combining the positive electrode, the separator and the negative electrode to form a battery core, placing the battery core in a battery shell, injecting a precursor solution of a solid electrolyte, and encapsulating and in-situ curing to obtain the battery.
[0041] Beneficial Effects
[0042] In view of the problem that the inherent characteristics of lithium-rich manganese-based materials are difficult to adapt to the application requirements of solid-state batteries, the present invention, while retaining the inherent characteristics of lithium-rich manganese-based materials, innovatively uses the combined synergy of a ferroelectric polymer positive electrode and a ferroelectric polymer membrane. This can unexpectedly solve the problem that the inherent characteristics of lithium-rich manganese-based materials are difficult to adapt to the application requirements of solid-state batteries, and can significantly improve its capacity in solid-state batteries and its cycle stability at high rates.
[0043] The research of the present invention also shows that the innovative use of in-situ assembled positive electrode and separator, further coordinated with the in-situ assembled heat treatment mechanism and the joint control of pressure, can further unexpectedly improve the combined synergy of the positive electrode and the separator, further improve the adaptation effect of lithium-rich manganese-based materials to solid-state batteries, and further improve its capacity in solid-state batteries and its high-rate cycle stability performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 Comparison of rate performance between Example 1 and Comparative Example 1;
[0045] Figure 2 Comparison of cycle performance between Example 1 and Comparative Example 1; DETAILED DESCRIPTION
[0046] The lithium-rich manganese-based solid-state battery described in the present invention includes a battery cell and a solid or semi-solid electrolyte arranged in the battery cell (such as an electrolyte arranged between a positive electrode, a separator, and a negative electrode); wherein the battery cell includes a positive electrode, a separator, and a negative electrode compounded in sequence; the positive electrode includes a current collector and a positive electrode material compounded on its surface, and the positive electrode material includes a conductive agent, a ferroelectric polymer, and a lithium-rich manganese-based active material; the separator includes a base film and a ferroelectric polymer modified layer compounded on its surface.
[0047] For example, the method for manufacturing the lithium-rich manganese-based positive electrode plate of the present invention is as follows:
[0048] (I) Using N,N-dimethylformamide (DMF) as a solvent, pouring a PVDF-based polymer with a designed solid content into a DMF solution and stirring for 3-6 hours to form a gel;
[0049] (II) adding a conductive carbon material, wherein the conductive carbon material comprises at least one of Super P, KS-6, and Ketjen Black, and stirring for 0.5-3 hours or until uniform;
[0050] (III) adding a high-capacity, high-voltage lithium-rich cathode material in 2-3 batches, stirring for 5-10 minutes after each batch is added, and continuing to stir for 1-3 hours or until uniform after all the materials are added to obtain a cathode slurry;
[0051] (IV) The positive electrode slurry is coated on the surface of the aluminum foil, and a positive electrode sheet is obtained after heat treatment (ie, an in-situ assembled positive electrode).
[0052] The heat treatment process of the present invention has a temperature of 60 to 100°C;
[0053] The heat treatment process includes two stages of heat treatment, wherein the first stage of heat treatment is carried out under normal pressure and the second stage of heat treatment is carried out under negative pressure;
[0054] The time of the first heat treatment process is 0.5 to 3 hours, preferably 1.5 to 2.5 hours;
[0055] The time of the second heat treatment is 5 to 15 hours, preferably 6 to 15 hours, and more preferably 8 to 12 hours.
[0056] The manufacturing method of the diaphragm of the present invention is as follows:
[0057] (I) using N,N-dimethylformamide (DMF) as a solvent, pouring a certain amount of PVDF-based polymer into a DMF solution, controlling the concentration of the PVDF solution to be 5 wt% to 50 wt%, and stirring for 2 to 10 hours to form a glue solution;
[0058] (II) coating the adhesive on the surface of the PP or PE separator by conventional means such as gravure coating, doctor blade coating, and extrusion coating;
[0059] (III) placing the coated diaphragm in an environment of 60 to 80° C. for thermal assembly for 4 to 15 hours to obtain the diaphragm (eg, an in-situ diaphragm).
[0060] The thermal assembly process includes a first thermal process and a second thermal process, wherein the second thermal process is performed under a pressure of 0.05 to 0.1 atm.
[0061] The lithium-rich manganese-based solid-state battery described in the present invention, in addition to using the positive electrode and the separator described in the present invention, other components, structures and ingredients can be conventional, and can also be packaged and prepared with the help of conventional processes in the industry.
[0062] For example, the negative electrode plate described in the present invention is a graphite negative electrode, a silicon-carbon negative electrode, a silicon-oxygen negative electrode, a metal lithium negative electrode or a current collector negative electrode prepared by a conventional method.
[0063] The solid or semi-solid electrolyte may be an electrolyte known in the industry, or may be prepared based on conventional means. For example, the electrolyte may include one or more of a polymer solid electrolyte, an oxide solid electrolyte, and a sulfide solid electrolyte. For example, the polymer solid electrolyte may be formed by an in-situ solidification process.
[0064] The above-mentioned other auxiliary materials include necessary auxiliary materials such as well-known tabs, shells, insulating glue, packaging films, etc. required for the production of various types of batteries.
[0065] After obtaining the above-mentioned functional positive electrode sheets, negative electrode sheets, modified PP or PE separators, solid electrolytes and other auxiliary materials, they are assembled into batteries according to standard processes. The batteries can be in the form of soft packs, cylinders, squares, button types, etc. The battery production process is the same as the existing process, that is, the stacking process, winding process, etc. can be used.
[0066] Preferably, when a polymer solid electrolyte using an in-situ solidification process is used, after the battery is assembled, steps such as liquid injection, packaging, standing, high-temperature curing, formation, (secondary curing), secondary sealing, and capacity division need to be performed.
[0067] In the present invention, the solution added in the injection stage is a precursor solution of a conventional solid electrolyte, which can be a conventional electrolyte dissolved with a polymerized monomer. For example, as an illustrative scheme, in the following case, the precursor solution in the injection stage is a solution containing a monomer, a conductive lithium salt, and selectively containing at least one auxiliary agent of an initiator and a cross-linking agent. In the present invention, the conductive lithium salt is, for example, at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium difluoro oxalate borate, and lithium bisoxalate borate. The solvent is, for example, a solvent that can dissolve the monomer and the conductive lithium salt. The monomer is, for example, an acrylic monomer. The initiator can be, for example, azobisisobutyronitrile, dimethyl azobisisobutyrate, etc. As a further example, in the following case, the precursor solution (precursor solution of the solid electrolyte) in the injection stage is, for example: a composite electrolyte in which 4.5-5wt.% methyl methacrylate and 0.3-0.5wt.% AIBN are dissolved in a basic electrolyte. The basic electrolyte is 1 mol / L LiPF6 / ethylene carbonate (EC) / diethyl carbonate (DEC) / dimethyl carbonate (DMC) (volume ratio 1:1:1).
[0068] In the present invention, the injection amount is based on the battery standard injection; the standing time is 12 to 72 hours, and the temperature is 15 to 50 degrees; the high-temperature curing temperature and time are 45 to 70 degrees and 4 to 20 hours respectively; according to the production process of the battery company, if secondary curing is required after formation, the secondary curing process is retained, and the steps after the second sealing are the same as the battery production.
[0069] Embodiment 1:
[0070] A high-specific-energy and high-rate lithium-manganese-rich solid-state soft-pack battery is designed, which consists of a functional positive electrode sheet, a negative electrode sheet, a modified PP or PE composite diaphragm, a solid electrolyte and other auxiliary materials.
[0071] The manufacturing method of the functional positive electrode sheet is as follows:
[0072] (I) using N,N-dimethylformamide (DMF) as a solvent, pouring a binder PVDF-based polymer with a designed solid content into a DMF solution, wherein the PVDF content accounts for 1.5 wt % of the slurry mass, and stirring for 5 hours to form a glue solution;
[0073] (II) adding a composite conductive carbon material, accounting for 2.5 wt% of the slurry mass, wherein the composite conductive carbon material comprises a mixture of Super P, KS-6, and Ketjen black in a mass ratio of 1:1:1, and stirring for 1 hour or until uniform;
[0074] (III) Add conventional lithium-rich manganese-based active materials (in this case, La / Al co-doped lithium-rich manganese-based positive electrode active materials Li 1.165(6) Mn 0.530(1) Ni 0.266(1) Al 0.003(3) La 0.0009(4) O2), stirring for 10 minutes after each batch is added, and stirring for 3 hours after all are added until uniform, to obtain a positive electrode slurry (the weight ratio of PVDF: conductive agent: lithium-rich manganese-based positive electrode active material is 1.5:2.5:96);
[0075] (IV) In-situ conversion: The positive electrode slurry is coated on the surface of the aluminum foil (coated electrode sheet), and the first stage heat treatment is performed at atmospheric pressure and 80°C for 2 hours, and then the second stage heat treatment is performed at 0.3 atmospheric pressure and 100°C for 8 hours to obtain a positive electrode sheet.
[0076] Metal lithium is used as the negative electrode.
[0077] The manufacturing method of the modified PP composite diaphragm is as follows:
[0078] (1) Using N,N-dimethylformamide (DMF) as a solvent, pour a certain amount of PVDF-based polymer into a DMF solution, control the concentration of the PVDF solution to 30 wt%, and stir for 10 hours to form a glue solution;
[0079] (2) coating the adhesive on the surface of the base film (e.g., PP or PE diaphragm, PP is selected in this case) by gravure coating; the coating thickness is 0.9 to 1 times the thickness of the base film;
[0080] (3) In-situ transformation: The coated diaphragm is placed in an environment of 60°C and atmospheric pressure for the first stage heat treatment for 2 hours, and then subjected to a second stage heat treatment at 70°C under negative pressure (0.1 atm) for 12 hours to obtain a modified diaphragm.
[0081] The polymer solid electrolyte adopts the in-situ solidification process. The above-mentioned other auxiliary materials include tabs, aluminum-plastic film, insulating glue, packaging film, etc.
[0082] Using a stacking machine, lithium-metal-rich batteries are assembled based on the stacking process (positive electrode-diaphragm-negative electrode are sequentially combined to form a battery cell).
[0083] After the battery is assembled, it needs to be filled with solid-state electrolyte and packaged in situ, left to stand at 25°C for 72 hours, and then cured at 60°C for 6 hours. The formation process is to charge at a rate of 0.1C to a cut-off voltage of 4.7V, followed by secondary sealing and capacity division.
[0084] Test results see Figure 1 and 2 ;
[0085] Comparative Example 1: Non-ferroelectric PVDF positive electrode-non-ferroelectric PVDF diaphragm solution
[0086] Compared with Example 1, the only difference is that the positive electrode slurry solvent does not use the polarity inducing solvent DMF, but uses NMP (the amount used is the same as DMF in Example 1). In addition, an equal amount of DMF in the membrane preparation process is replaced with NMP (the amount used is the same as DMF in Example 1).
[0087] The assembly and electrochemical test were performed according to the method of Example 1. The results are shown in Figure 1 and 2 .
[0088] like Figure 1 , Figure 2 As shown, the rate performance of the obtained battery at room temperature is better than that of the comparative example, especially at 5C, a capacity of 161 mAh / g is released, which is higher than 141 mAh / g of comparative example 1. In terms of cycle performance, the initial discharge capacity of Example 1 at 1C is 219.6 mAh / g, and the capacity retention rate is 87% after 270 cycles, while the initial discharge capacity of comparative example 1 is 197.4 mAh / g, and the capacity retention rate is 78% after 270 cycles.
[0089] Embodiment 2:
[0090] Compared with Example 1, the only difference is that the coating in the diaphragm uses PVDF-based polymer P (VDF-TrFE) to replace the PVDF in equal amounts. Other operations and parameters are the same as those in Example 1, and the test is carried out according to the method of Example 1.
[0091] The obtained battery released a capacity of 158 mAh / g at 5C, an initial discharge specific capacity of 220 mAh / g at 1C, and a capacity retention rate of 86% after 270 cycles.
[0092] Example 3
[0093] Compared with Example 1, the only difference is that the positive electrode preparation process is changed. The experimental groups are:
[0094] Group A: non-in-situ process, the steps are as follows: dissolve PVDF in DMF in advance to obtain a 1.5wt% solution, then obtain ferroelectric PVDF by a dissolution recrystallization method (the solution is first heat treated at atmospheric pressure and 80°C for 2 hours, and then heat treated at 0.3atm and 100°C for 8 hours in the second stage), and then dissolve the ferroelectric PVDF as a binder in NMP, the same conductive agent and lithium-rich material as in Example 1 to obtain a positive electrode slurry, which is then coated and dried to obtain a positive electrode sheet.
[0095] Group B: In-situ process, and single-stage heat treatment, the process steps are: according to the process steps (IV) of Example 1, the coated electrode is subjected to a single-stage heat treatment at 0.3 atmospheres and 100°C for 10 hours to obtain a positive electrode.
[0096] Group C: In-situ process, the difference is that the second heat treatment process in (IV) is carried out under atmospheric pressure.
[0097] Group D: in-situ process, the difference is that in (IV), the temperature of the first stage is 75°C and the time is 2.5 h, and the pressure of the second stage is 0.1 atm, the temperature is 95°C and the time is 10 h.
[0098] The batteries were assembled according to the method of Example 1, and the performances were:
[0099] Group A: The initial discharge capacity at 1C is 208.3 mAh / g, and the capacity retention rate is 80% after 270 cycles;
[0100] Group B: The initial discharge capacity of 1C is 212.3 mAh / g, and the capacity retention rate after 270 cycles is 82%.
[0101] Group C: The initial discharge capacity at 1C was 213.6 mAh / g, and the capacity retention rate was 83% after 270 cycles.
[0102] Group D: The initial discharge capacity of 1C was 220.6 mAh / g, and the capacity retention rate was 88% after 270 cycles.
[0103] It can be seen from Examples 1 and 3 that the preferred in-situ ferroelectric PVDF assembly process can unexpectedly further improve the adaptation effect of the prepared lithium-rich manganese-based material to the solid-state battery, and further improve its capacity and cycle stability. In addition, under the control of the two-stage gradient assembly process and gas pressure, the performance of the prepared material can be unexpectedly further improved.
[0104] Example 4
[0105] Compared with Example 1, the only difference is that step (3) in the diaphragm process is changed:
[0106] Group A: non-in-situ process, the steps are: obtain ferroelectric PVDF (preparation process is the same as Example 3A), then dissolve the ferroelectric PVDF as a binder in NMP, and coat it on the surface of the diaphragm in the same way as in Example 1, and the subsequent drying process is the same.
[0107] Group B: In-situ process, the difference is that, and a single-stage heat treatment is performed, the coated diaphragm is kept at 70°C and 0.1atm for 14 hours to obtain a coated diaphragm.
[0108] Group C: In-situ process, the difference is that the second heat treatment process is carried out under atmospheric pressure.
[0109] Group D: in-situ process, the difference is that the temperature of the first stage is 65℃, the time is 1.5h; the temperature of the second stage heat treatment is 75℃, the pressure is 0.05atm, and the time is 10h;
[0110] The batteries were assembled according to the method of Example 1, and the performances were:
[0111] Group A: The initial discharge capacity at 1C is 205.5 mAh / g, and the capacity retention rate after 270 cycles is 81%;
[0112] Group B: The initial discharge capacity at 1C was 214.7 mAh / g, and the capacity retention rate after 270 cycles was 83%;
[0113] Group C: The initial discharge capacity at 1C was 215.2 mAh / g, and the capacity retention rate was 84% after 270 cycles.
[0114] Group D: The initial discharge capacity of 1C was 217.9 mAh / g, and the capacity retention rate was 86% after 270 cycles.
[0115] It can be seen from Examples 1 and 4 that the use of an in-situ diaphragm has better compatibility with the positive electrode, which can help solve the problem that lithium-rich manganese-based materials are difficult to adapt to solid-state battery systems. On this basis, the further use of a two-stage hot assembly process and the control of the assembly pressure can unexpectedly further improve the combined synergy of the positive electrode and the diaphragm.
[0116] Example 5
[0117] Compared with Example 1, the only difference is that the positive electrode is the positive electrode of Example 3A, and the separator is the separator of Example 4A. The battery is assembled according to the method of Example 1, and the performance is: the initial discharge capacity of 1C is 204.8 mAh / g, and the capacity retention rate after 270 cycles is 80%.
[0118] Example 6
[0119] Compared with Example 1, the only difference is that the lithium-rich material is Li 1.2 Mn 0.53 Ni 0.27 O2@1%LiAlO2, the conductive agent is Super P, and the weight ratio of PVDF: conductive agent: lithium-rich manganese-based positive electrode active material is 2:3:95; other operations, parameters and test methods are the same as in Example 1.
[0120] The obtained battery performance is that the initial discharge capacity at 1C is 202.1 mAh / g, and the capacity retention rate is 80% after 270 cycles.
[0121] Comparative Example 2: Non-ferroelectric PVDF positive electrode-ferroelectric PVDF diaphragm solution:
[0122] Compared with Example 1, the only difference is that the positive electrode slurry solvent does not use the polarity-inducing solvent DMF, but uses NMP. The obtained battery releases a capacity of 149 mAh / g at 5C, and the capacity retention rate after 270 cycles is 79.3%.
[0123] Comparative Example 3: Ferroelectric PVDF positive electrode-non-ferroelectric PVDF diaphragm solution:
[0124] The key steps are the same as those in Example 1, except that the separator is a pure PP separator. The obtained battery releases a capacity of 145 mAh / g at 5C, and the capacity retention rate is 79.6% after 270 cycles.
Claims
1. A lithium-rich manganese-based solid-state battery, comprising a battery cell and a solid or semi-solid electrolyte disposed in the battery cell; wherein: The battery cell comprises a positive electrode, a separator and a negative electrode which are compounded in sequence; the positive electrode comprises a current collector and a positive electrode material compounded on its surface, and the positive electrode material comprises a conductive agent, a ferroelectric polymer and a lithium-rich manganese-based active material; The diaphragm comprises a base film and a ferroelectric polymer modified layer compounded on the surface thereof; The ferroelectric polymer includes at least one of ferroelectric PVDF, ferroelectric P (VDF-TrFE), ferroelectric P (VDF-TrFE-CTFE), and ferroelectric P (VDF-HPP).
2. The lithium-rich manganese-based solid-state battery according to claim 1, characterized in that: The lithium-rich manganese-based active material is: Li a Mn b Ni c Co d O2; 1 of them<a≤1.5;0.4≤b≤0.8;0≤c≤0.4;0≤d≤0.4;b> c>d, or a lithium-rich material obtained by doping and / or coating thereof.
3. The lithium-rich manganese-based solid-state battery according to claim 1, characterized in that: The conductive agent includes at least one of Super P, KS-6 and Ketjen Black.
4. The lithium-rich manganese-based solid-state battery according to claim 1, characterized in that: The ferroelectric polymer is obtained by assembling a precursor polymer in DMF; the precursor polymer includes at least one of PVDF, P (VDF-TrFE), P (VDF-TrFE-CTFE), and P (VDF-HFP).
5. The lithium-rich manganese-based solid-state battery according to any one of claims 1 to 4, characterized in that: In the positive electrode material, the weight ratio of the conductive agent, the ferroelectric polymer and the lithium-rich manganese-based active material is 0.01-0.1: 0.01-0.1: 0.8-0.
98.
6. The lithium-rich manganese-based solid-state battery according to any one of claims 1 to 4, characterized in that: The positive electrode is a non-in-situ assembled positive electrode or an in-situ assembled positive electrode; The non-in-situ assembled positive electrode is obtained by coating and drying a positive electrode material comprising a conductive agent, a ferroelectric polymer and a lithium-rich manganese-based active material after solvent slurrying; The in-situ assembled positive electrode is obtained by coating a conductive agent, a precursor polymer and a lithium-rich manganese-based active material on a current collector after being slurried with DMF, and then being in-situ assembled through heat treatment.
7. The lithium-rich manganese-based solid-state battery according to claim 6, characterized in that: In the in-situ assembled positive electrode preparation process, the heat treatment temperature is 60-100°C.
8. The lithium-rich manganese-based solid-state battery according to claim 7, characterized in that: The heat treatment process includes two stages of heat treatment process, wherein the first stage of heat treatment process is carried out under normal pressure, and the second stage of heat treatment process is carried out under negative pressure.
9. The lithium-rich manganese-based solid-state battery according to claim 8, characterized in that: The temperature of the first heat treatment is 75~85℃, and the temperature of the second heat treatment is 95~100℃.
10. The lithium-rich manganese-based solid-state battery according to claim 9, characterized in that: The time of the first heat treatment process is 0.5~3H.
11. The lithium-rich manganese-based solid-state battery according to claim 9, characterized in that: The time of the first heat treatment process is 1.5~2.5h.
12. The lithium-rich manganese-based solid-state battery according to claim 9, characterized in that: The second heat treatment time is 5~15H.
13. The lithium-rich manganese-based solid-state battery according to claim 9, characterized in that: The second heat treatment time is 6~15h.
14. The lithium-rich manganese-based solid-state battery according to claim 9, characterized in that: The second heat treatment time is 8~12h.
15. The lithium-rich manganese-based solid-state battery according to claim 1, characterized in that: In the diaphragm, the base film is at least one of PE and PP.
16. The lithium-rich manganese-based solid-state battery according to claim 1, characterized in that: The diaphragm is a non-in-situ assembled diaphragm or an in-situ assembled diaphragm, wherein the non-in-situ assembled diaphragm is prepared by slurrying a ferroelectric polymer, coating it on a base film, and drying it; The in-situ assembled membrane is obtained by coating a precursor polymer with DMF slurry on a base membrane and then thermally assembling the slurry.
17. The lithium-rich manganese-based solid-state battery according to claim 16, characterized in that: The temperature of the thermal assembly process is 60-90°C.
18. The lithium-rich manganese-based solid-state battery according to claim 17, characterized in that: The total time for hot assembly is 4~24h.
19. The lithium-rich manganese-based solid-state battery according to claim 16, characterized in that: The thermal assembly process includes a first thermal process and a second thermal process, wherein the second thermal process is performed under a pressure of 0.05-0.1 atm.
20. The lithium-rich manganese-based solid-state battery according to claim 19, characterized in that: The temperature of the first thermal process is 60~65℃, and the temperature of the second thermal process is 70~80℃.
21. The lithium-rich manganese-based solid-state battery according to claim 20, characterized in that: The duration of the first thermal process is 1 to 3 hours, and the insulation time of the second thermal process is 6 to 15 hours.
22. The lithium-rich manganese-based solid-state battery according to claim 1, characterized in that: The negative electrode is a graphite negative electrode, a silicon-carbon negative electrode, a silicon-oxygen negative electrode, a metal lithium negative electrode or a current collector negative electrode.
23. The lithium-rich manganese-based solid-state battery according to claim 1, characterized in that: The solid or semi-solid electrolyte includes one or more of a polymer solid electrolyte, an oxide solid electrolyte, and a sulfide solid electrolyte.
24. The lithium-rich manganese-based solid-state battery according to claim 23, characterized in that: The solid electrolyte is prepared by an in-situ or non-in-situ method.
25. The lithium-rich manganese-based solid-state battery according to claim 1, characterized in that: Lithium-rich manganese-based solid-state batteries are soft-pack, cylindrical, square or button-type.
26. An in-situ preparation method for a lithium-rich manganese-based solid-state battery according to any one of claims 1 to 25, characterized in that: The positive electrode and the separator are obtained, and then the positive electrode, the separator and the negative electrode are combined to form a battery core, the battery core is placed in a battery shell, a precursor solution of a solid electrolyte is injected, and the battery core is cured in situ after packaging.
Citation Information
Patent Citations
Solid-state ion conductor and lithium-enrich manganese-based material composite electrode and lithium ion battery
CN109638233A
Preparation method of lithium-rich manganese-based positive electrode material
CN115676910A
Lithium-rich manganese-based anode material and method for manufacturing same
CN102916169A
Lithium ion battery and preparation method thereof
CN110190327A
Preparation method of high-rate lithium metal composite negative electrode and application of high-rate lithium metal composite negative electrode in solid battery
CN114551774A