A catalyst for the production of dimethyl ether from syngas with a high C / H ratio, its preparation method and application
By using CuMnMOx and metal-modified molecular sieve catalysts, the problems of low hydrogen-to-carbon ratio and high temperature in the direct conversion of syngas to dimethyl ether were solved, achieving low-energy consumption and high-selectivity dimethyl ether synthesis.
Patent Information
- Application Number
- CN202410134887.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-31
AI Technical Summary
Existing technologies for the direct conversion of syngas to dimethyl ether have low hydrogen-to-carbon ratios, high reaction temperatures, low space velocities, and high CO2 emissions and energy consumption during the water-gas conversion process.
The catalyst is composed of a methanol synthesis catalyst and a methanol dehydration catalyst. The catalyst is composed of CuMnMOx and metal-modified molecular sieves. The catalyst is prepared by controlling the pH value and calcination temperature. The reaction conditions are mild. The methanol synthesis catalyst can catalyze the water-gas shift reaction and improve the CO conversion rate.
This method enables the synthesis of dimethyl ether under low pressure and temperature, with high space velocity and high selectivity, reducing energy consumption and CO2 emissions while improving CO conversion rate.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of industrial catalysis technology, specifically relating to a catalyst for the production of dimethyl ether from syngas with a high carbon-to-hydrogen ratio, its preparation method, and its application. Background Technology
[0002] Dimethyl ether (DME) is one of the most widely used ethers and also the simplest in structure. It is an important chemical raw material and environmentally friendly product, used to synthesize bulk chemical products such as aerosols, refrigerants, and methyl acetate. DME can be used as a civilian fuel. Furthermore, its high cetane number makes it advantageous as a vehicle fuel due to its high efficiency, environmental friendliness, safety, and wide applicability.
[0003] Currently, there are two-step and one-step methods for synthesizing dimethyl ether. The two-step method converts carbon-containing gas into methanol, and then dehydrates the methanol to produce dimethyl ether. The one-step method directly converts syngas into dimethyl ether, that is, using a catalyst containing methanol synthesis components and methanol dehydration components to directly convert syngas into dimethyl ether in a single reactor.
[0004] The direct conversion of syngas to dimethyl ether (DME) has become a hot research topic in the field of catalysis in recent years. CN 115254180 A reports a catalyst and method for the direct synthesis of DME from syngas. A CuZnAl-based oxide and magnesium alkali zeolite co-precipitation catalyst catalyzes the synthesis of DME from syngas. At an H2 / CO+CO2 ratio of 2 and a reaction temperature of 250℃, the CO conversion rate is 37.0%. CN 102600852A reports a catalyst for the preparation of DME, its preparation method, and its application. The catalyst is composed of a methanol synthesis catalyst precursor and a zirconium oxide-alumina mixed oxide precursor. The reaction is carried out at an H2 / CO / CO2 ratio of 1:0.5:1, a reaction temperature of 250℃, a pressure of 4.0 MPa, and a space velocity of 1500 h⁻¹. -1 At that time, the CO conversion rate was 73% and the proportion of DME in the organic products was 99.54%. However, these reactions resulted in a high percentage of hydrogen and a relatively low percentage of CO in the syngas, high reaction temperatures (mostly above 250°C), and low space velocity.
[0005] Currently, in research on the direct conversion of syngas to dimethyl ether, the proportion of CO in the feedstock syngas is relatively low. Industrially, it is necessary to increase the hydrogen-to-carbon ratio through water-gas shift conversion, but this process results in high CO2 emissions and energy consumption. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a catalyst for the catalytic production of dimethyl ether from high C / H ratio syngas, its preparation method, and its application. The catalyst is composed of a methanol synthesis catalyst and a methanol dehydration catalyst. When catalyzing the direct conversion of high C / H ratio syngas into dimethyl ether, it has advantages such as low reaction pressure and temperature, high space velocity, and high dimethyl ether selectivity.
[0007] A catalyst for the catalytic production of dimethyl ether from high C / H ratio syngas, wherein the catalyst comprises a methanol synthesis catalyst and a methanol dehydration catalyst, wherein... The methanol synthesis catalyst is represented as CuMnMOx, where the metal M is two of Zn, Zr, Mg, Al, and Ce; the weight of the metals Cu, Mn, and M is 100%, and the content of each metal component is as follows: Cu 40-75%, Mn 5-15%, with the balance being M, and x is the number of oxygen atoms required to satisfy the oxidation states of the metal elements Cu, Mn, and M. The methanol dehydration catalyst is a metal-modified molecular sieve, wherein the metal is one of Cu, Co, Ni or La.
[0008] Preferably, the mass ratio of the methanol synthesis catalyst to the methanol dehydration catalyst is (1-8):1.
[0009] Preferably, the molecular sieve is an HZSM-5 molecular sieve, a MOR molecular sieve, or a ZSM-35 molecular sieve, and the SiO2 / Al2O3 ratio of the molecular sieve is 15-80.
[0010] The preparation method of the catalyst for catalyzing the synthesis of dimethyl ether from syngas with a high carbon-to-hydrogen ratio includes the following steps: (1) Preparation of methanol synthesis catalyst: (11) At 60-90℃, a mixed salt solution of metals Cu, Mn and M and a precipitant solution are simultaneously added dropwise to water. By controlling the dropwise addition rate of the precipitant solution, the pH value of the system is controlled to 7.0-9.5. (12) Continue aging reaction at 60-90℃ for 2h, then wash, dry, calcinate, press into tablets and sieve to obtain methanol synthesis catalyst; (2) Preparation of methanol dehydration catalyst: (21) Add molecular sieve to metal salt solution at a ratio of 1g:(10-50)mL, mix by ultrasonication, reflux at 60-90℃ for 3h, filter, wash, and dry; (22) Repeat step (21) 1-3 times after drying the molecular sieve, calcining, pressing into tablets, and sieving; (3) Preparation of catalyst: Weigh out the methanol synthesis catalyst and methanol dehydration catalyst, mix them, and the mixture is ready.
[0011] Preferably, the mixed salt solution of metals Cu, Mn, and M is a salt solution of nitrate, chloride, or acetate of the corresponding metals, and the total concentration of metal Cu, Mn, and M ions in the mixed salt solution is 0.1-1 mol / L.
[0012] Preferably, the precipitant solution is a NaOH solution, a Na2CO3 solution, or a KOH solution, and the concentration of the precipitant solution is 0.1-1 mol / L.
[0013] Preferably, the metal salt solution in step (21) is a nitrate or chloride solution of the corresponding metal, and the concentration of the metal salt solution is 0.1-1 mol / L.
[0014] Preferably, the drying conditions are drying at 90-150℃ for 5-15 hours, and the sieving is passing through a 20-60 mesh sieve; the calcination conditions in step (12) are calcination at 300-500℃ for 3-10 hours, and the calcination conditions in step (22) are calcination at 350-600℃ for 3-10 hours.
[0015] A method for producing dimethyl ether from syngas with a high C / H ratio via catalysis is as follows: a catalyst is loaded into a fixed-bed reactor, hydrogen-containing gas is introduced for reduction and activation, the reaction temperature is adjusted to 200-260°C, and then the syngas is introduced and pressurized to 1-5 MPa for reaction; the catalyst is the catalyst described in this invention.
[0016] Preferably, the hydrogen-containing gas consists of hydrogen gas with a volume ratio of 5-100% and a balance gas, wherein the balance gas is nitrogen, helium or argon. The conditions for reduction activation are: reduction temperature 250-350℃, reduction time 1-8h, reduction pressure at atmospheric pressure, and hydrogen gas flow rate of 30-100 mL / min. The volume ratio of CO to H2 in the synthesis gas is (2-4):1; the space velocity of the synthesis gas relative to the methanol synthesis catalyst in the catalyst is 2000-8000 h⁻¹. -1 .
[0017] Advantages of this invention: (1) The catalyst preparation method provided by the present invention is simple and the preparation process is environmentally friendly; (2) When used to catalyze the production of dimethyl ether from syngas with a high carbon-to-hydrogen ratio, it has the advantages of mild reaction conditions, high space velocity, and high dimethyl ether selectivity. (3) In this invention, the methanol synthesis catalyst can simultaneously catalyze the water-gas shift reaction, thereby increasing the CO conversion rate and promoting the reaction to proceed to the right. Detailed Implementation
[0018] Example 1 1. A catalyst for the catalytic production of dimethyl ether from syngas with a high C / H ratio, said catalyst comprising a methanol synthesis catalyst and a methanol dehydration catalyst in a mass ratio of 4:1, wherein, The methanol synthesis catalyst is represented as CuO-MnO2-ZnO-ZrO2, wherein the weight ratio of Cu, Mn, Zn, and Zr is 40:5:40:15. The methanol dehydration catalyst is a Cu-modified MOR molecular sieve, wherein the SiO2 / Al2O3 ratio of the MOR molecular sieve is 15. 2. The preparation method of the catalyst for catalyzing the production of dimethyl ether from syngas with a high C / H ratio includes the following steps: (1) Preparation of methanol synthesis catalyst: (11) Prepare a salt solution with a total metal ion concentration of 1 mol / L by mixing copper nitrate, manganese nitrate, zirconium nitrate and zinc nitrate. At the same time, prepare a 0.1 mol / L sodium carbonate solution as a precipitant. At 75°C, add the salt solution and the precipitant solution dropwise to water. Control the pH of the system to 7.0-8.0 by controlling the dropwise addition rate of the precipitant solution. (12) Continue aging reaction at 75℃ for 2h, then wash, dry at 110℃ for 10h, calcine at 350℃ in muffle furnace for 4h, press into tablets, and sieve through 40-60 mesh to obtain methanol synthesis catalyst; (2) Preparation of methanol dehydration catalyst: (21) Add MOR molecular sieve to 0.1 mol / L copper nitrate solution at a ratio of 1 g: 25 mL, mix by sonication, reflux at 75 °C for 3 h, filter and wash, and dry at 110 °C for 6 h. (22) Repeat step (21) once after drying the molecular sieve, calcine it in a muffle furnace at 500℃ for 5 hours, press it into tablets, and sieve it through a 40-60 mesh sieve. (3) Preparation of catalyst: Weigh out the methanol synthesis catalyst and methanol dehydration catalyst, mix them, and the mixture is ready.
[0019] 3. A method for catalytically producing dimethyl ether from syngas with a high C / H ratio, comprising the following steps: A catalyst is loaded into a fixed-bed reactor, and a hydrogen-containing gas is introduced at a flow rate of 30 mL / min. The catalyst is then activated by reduction at 250°C and atmospheric pressure for 8 h, wherein the hydrogen-containing gas is hydrogen gas. The reaction temperature is then adjusted to 230°C, and the syngas is introduced and pressurized to 4 MPa for further reaction. The volume ratio of CO to H2 in the syngas is 4:1, and the space velocity of the syngas relative to the methanol synthesis catalyst in the catalyst is 5500 h⁻¹. -1 The whole components were analyzed online by gas chromatography, and the results are shown in Table 1.
[0020] Example 2 1. A catalyst for the catalytic production of dimethyl ether from syngas with a high C / H ratio, said catalyst comprising a methanol synthesis catalyst and a methanol dehydration catalyst in a mass ratio of 8:1, wherein, The methanol synthesis catalyst is represented as CuO-MnO2-ZnO-MgO, wherein the weight ratio of Cu, Mn, Zn, and Mg is 75:5:16:4. The methanol dehydration catalyst is a Co-modified ZSM-35 molecular sieve, wherein the SiO2 / Al2O3 ratio of the ZSM-35 molecular sieve is 35. 2. The preparation method of the catalyst for catalyzing the production of dimethyl ether from syngas with a high C / H ratio includes the following steps: (1) Preparation of methanol synthesis catalyst: (11) Prepare a salt solution with a total metal ion concentration of 0.5 mol / L by mixing copper chloride, manganese chloride, zinc chloride and magnesium chloride. At the same time, prepare a 1 mol / L sodium hydroxide solution as a precipitant. At 90°C, add the salt solution and the precipitant solution dropwise to water. Control the pH of the system to 8.0-9.0 by controlling the dropwise addition rate of the precipitant solution. (12) Continue aging reaction at 90℃ for 2h, then wash, dry at 90℃ for 15h, calcine at 450℃ in muffle furnace for 4h, press into tablets, and sieve through a 20-60 mesh sieve to obtain methanol synthesis catalyst; (2) Preparation of methanol dehydration catalyst: (21) Add ZSM-35 molecular sieve to 0.5mol / L cobalt nitrate solution at a ratio of 1g:15mL, mix by sonication, reflux at 60℃ for 3h, filter and wash, and dry at 90℃ for 15h. (22) Repeat step (21) once after drying the molecular sieve, calcine it in a muffle furnace at 550℃ for 5 hours, press it into tablets, and sieve it through a 20-60 mesh sieve. (3) Preparation of catalyst: Weigh out the methanol synthesis catalyst and methanol dehydration catalyst, mix them, and the mixture is ready.
[0021] 3. A method for catalytically producing dimethyl ether from syngas with a high C / H ratio, comprising the following steps: A catalyst is loaded into a fixed-bed reactor, and a hydrogen-containing gas is introduced at a flow rate of 100 mL / min. The catalyst is then activated by reduction at 350°C and atmospheric pressure for 1 h, wherein the hydrogen-containing gas consists of 5% hydrogen by volume and the remainder nitrogen. The reaction temperature is then adjusted to 260°C, and the syngas is introduced and pressurized to 1 MPa for further reaction. The CO:H2 volume ratio of the syngas is 2:1, and the space velocity of the syngas relative to the methanol synthesis catalyst in the catalyst is 2000 h⁻¹. -1 The whole components were analyzed online by gas chromatography, and the results are shown in Table 1.
[0022] Example 3 1. A catalyst for the catalytic production of dimethyl ether from syngas with a high C / H ratio, said catalyst comprising a methanol synthesis catalyst and a methanol dehydration catalyst in a 1:1 mass ratio, wherein, The methanol synthesis catalyst is represented as CuO-MnO2-ZnO-Al2O3, wherein the weight ratio of Cu, Mn, Zn, and Al is 50:15:30:5; The methanol dehydration catalyst is a La-modified HZSM-35 molecular sieve, wherein the SiO2 / Al2O3 ratio of the HZSM-35 molecular sieve is 80. 2. The preparation method of the catalyst for catalyzing the production of dimethyl ether from syngas with a high C / H ratio includes the following steps: (1) Preparation of methanol synthesis catalyst: (11) Prepare a salt solution with a total metal ion concentration of 0.1 mol / L by mixing copper nitrate, manganese acetate, zinc acetate and aluminum nitrate. At the same time, prepare a 0.5 mol / L potassium hydroxide solution as a precipitant. At 60°C, add the salt solution and the precipitant solution dropwise to water. Control the pH of the system to 8.5-9.5 by controlling the dropwise addition rate of the precipitant solution. (12) Continue aging reaction at 60℃ for 2h, then wash, dry at 150℃ for 6h, calcine at 500℃ in muffle furnace for 3h, press into tablets, and sieve through a 20-40 mesh sieve to obtain methanol synthesis catalyst; (2) Preparation of methanol dehydration catalyst: (21) Add HZSM-35 molecular sieve to a 1 mol / L lanthanum chloride solution at a ratio of 1 g: 10 mL, mix by sonication, reflux at 90 °C for 3 h, filter and wash, and dry at 150 °C for 6 h. (22) Repeat step (21) 3 times after drying the molecular sieve, calcine it in a muffle furnace at 600℃ for 3 hours, press it into tablets, and sieve it through a 20-40 mesh sieve; (3) Preparation of catalyst: Weigh out the methanol synthesis catalyst and methanol dehydration catalyst, mix them, and the mixture is ready.
[0023] 3. A method for catalytically producing dimethyl ether from syngas with a high C / H ratio, comprising the following steps: A catalyst is loaded into a fixed-bed reactor, and a hydrogen-containing gas is introduced at a flow rate of 50 mL / min. The catalyst is then reduced and activated at 300°C under normal pressure for 3 h, wherein the hydrogen-containing gas consists of 20% hydrogen and the remainder helium by volume; the reaction temperature is then adjusted to 200°C, and the syngas is introduced and pressurized to 5 MPa for further reaction. The CO:H2 volume ratio of the syngas is 3:1, and the space velocity of the syngas relative to the methanol synthesis catalyst in the catalyst is 8000 h⁻¹. -1 The whole components were analyzed online by gas chromatography, and the results are shown in Table 1.
[0024] Example 4 1. A catalyst for the catalytic production of dimethyl ether from syngas with a high C / H ratio, said catalyst comprising a methanol synthesis catalyst and a methanol dehydration catalyst in a mass ratio of 6:1, wherein, The methanol synthesis catalyst is represented as CuO-MnO2-ZrO2-Al2O3, wherein the weight ratio of Cu, Mn, Zr, and Al is 60:9:27:4. The methanol dehydration catalyst is a Cu-modified HZSM-5 molecular sieve, wherein the SiO2 / Al2O3 ratio of the HZSM-5 molecular sieve is 30. 2. The preparation method of the catalyst for catalyzing the production of dimethyl ether from syngas with a high C / H ratio includes the following steps: (1) Preparation of methanol synthesis catalyst: (11) Prepare a salt solution with a total metal ion concentration of 0.8 mol / L by mixing copper nitrate, manganese acetate, zirconium nitrate and aluminum chloride. At the same time, prepare a 0.8 mol / L sodium carbonate solution as a precipitant. At 80°C, add the salt solution and the precipitant solution dropwise to water. Control the pH of the system to 7.0-8.0 by controlling the dropwise rate of the precipitant solution. (12) Continue aging reaction at 80℃ for 2h, then wash, dry at 120℃ for 6h, calcine in muffle furnace at 300℃ for 10h, press into tablets, and sieve through 40-60 mesh to obtain methanol synthesis catalyst; (2) Preparation of methanol dehydration catalyst: (21) Add HZSM-5 molecular sieve to 0.1mol / L copper acetate solution at a ratio of 1g:30mL, mix by sonication, reflux at 75℃ for 3h, filter and wash, and dry at 130℃ for 8h. (22) Repeat step (21) 3 times after drying the molecular sieve, calcine it in a muffle furnace at 450℃ for 4.5h, press it into tablets, and sieve it through a 40-60 mesh sieve. (3) Preparation of catalyst: Weigh out the methanol synthesis catalyst and methanol dehydration catalyst, mix them, and the mixture is ready.
[0025] 3. A method for catalytically producing dimethyl ether from syngas with a high C / H ratio, comprising the following steps: A catalyst is loaded into a fixed-bed reactor, and a hydrogen-containing gas is introduced at a flow rate of 30 mL / min. The catalyst is then activated by reduction at 280°C and atmospheric pressure for 5 h. The hydrogen-containing gas consists of 60% hydrogen by volume and the remainder is argon. The reaction temperature is then adjusted to 250°C, and the syngas is introduced and pressurized to 3 MPa for further reaction. The CO:H2 volume ratio of the syngas is 2:1, and the space velocity of the syngas relative to the methanol synthesis catalyst in the catalyst is 3000 h⁻¹. -1 The whole components were analyzed online by gas chromatography, and the results are shown in Table 1.
[0026] Example 5 1. A catalyst for the catalytic production of dimethyl ether from syngas with a high C / H ratio, said catalyst comprising a methanol synthesis catalyst and a methanol dehydration catalyst in a mass ratio of 5:1, wherein, The methanol synthesis catalyst is represented as CuO-MnO2-ZrO2-CeO2, wherein the weight ratio of Cu, Mn, Zr, and Ce is 55:5:25:15. The methanol dehydration catalyst is a Ni-modified MOR molecular sieve, wherein the SiO2 / Al2O3 ratio of the MOR molecular sieve is 50. 2. The preparation method of the catalyst for catalyzing the production of dimethyl ether from syngas with a high C / H ratio includes the following steps: (1) Preparation of methanol synthesis catalyst: (11) Prepare a salt solution with a total metal ion concentration of 0.4 mol / L by mixing copper chloride, manganese chloride, zirconium nitrate and cerium nitrate. At the same time, prepare a 0.5 mol / L sodium carbonate solution as a precipitant. At 75°C, add the salt solution and the precipitant solution dropwise to water. Control the pH of the system to 7.5-8.5 by controlling the dropwise addition rate of the precipitant solution. (12) Continue aging reaction at 75℃ for 2h, then wash, dry at 130℃ for 5h, calcine at 420℃ in muffle furnace for 6h, press into tablets, and sieve through a 40-60 mesh sieve to obtain methanol synthesis catalyst; (2) Preparation of methanol dehydration catalyst: (21) Add HZSM-5 molecular sieve to 1 mol / L nickel nitrate solution at a ratio of 1 g: 50 mL, mix by ultrasonication, reflux at 85 °C for 3 h, filter and wash, and dry at 100 °C for 10 h. (22) Repeat step (21) 3 times after drying the molecular sieve, calcine it in a muffle furnace at 350℃ for 10h, press it into tablets, and sieve it through a 40-60 mesh sieve. (3) Preparation of catalyst: Weigh out the methanol synthesis catalyst and methanol dehydration catalyst, mix them, and the mixture is ready.
[0027] 3. A method for catalytically producing dimethyl ether from syngas with a high C / H ratio, comprising the following steps: A catalyst is loaded into a fixed-bed reactor, and a hydrogen-containing gas is introduced at a flow rate of 70 mL / min. The catalyst is then activated by reduction at 320°C and atmospheric pressure for 4 h, wherein the hydrogen-containing gas consists of 30% hydrogen and the remainder nitrogen by volume; the reaction temperature is then adjusted to 240°C, and the syngas is introduced and pressurized to 2 MPa for further reaction. The volume ratio of CO to H2 in the syngas is 3:1, and the space velocity of the syngas relative to the methanol synthesis catalyst in the catalyst is 6000 h⁻¹. -1 The whole components were analyzed online by gas chromatography, and the results are shown in Table 1.
[0028] Comparative Example 1 A catalyst for the conversion of high C / H ratio syngas to dimethyl ether comprises a methanol synthesis catalyst and a methanol dehydration catalyst in a mass ratio of 4:1, wherein... The methanol synthesis catalyst is represented as CuO-ZnO-ZrO2, wherein the weight ratio of Cu, Mn, Zn, and Zr is 45:40:15. The methanol dehydration catalyst is a Cu-modified MOR molecular sieve; In its preparation method, manganese nitrate is not added in step (12), and the rest is the same as in Example 1.
[0029] The application of the catalyst in the catalytic synthesis of dimethyl ether from high C / H ratio syngas is the same as in Example 1, and the reaction results are shown in Table 1.
[0030] Table 1. Results of reactions using different catalysts for the direct conversion of syngas to dimethyl ether
[0031] Note: * Dimethyl ether exhibits selectivity in products other than CO2, with the remainder being small amounts of methanol and low-carbon hydrocarbons.
Claims
1. A catalyst for the catalytic production of dimethyl ether from syngas with a high C / H ratio, characterized in that: The volume ratio of CO to H2 in the synthesis gas is (2-4):1, and the catalyst consists of a methanol synthesis catalyst and a methanol dehydration catalyst. The methanol synthesis catalyst is represented as CuMnMOx, where the metal M is Zn-Zr, Zn-Mg, Zr-Al, or Zr-Ce; the weight of the metals Cu, Mn, and M is 100%, and the content of each metal component is as follows: Cu 40-75%, Mn 5-15%, with the balance being M, and x being the number of oxygen atoms required to satisfy the oxidation states of the metal elements Cu, Mn, and M. The methanol dehydration catalyst is a metal-modified molecular sieve, wherein the metal is one of Cu, Co, Ni or La; the molecular sieve is HZSM-5 molecular sieve, MOR molecular sieve or ZSM-35 molecular sieve, and the SiO2 / Al2O3 ratio of the molecular sieve is 15-80. The methanol dehydration catalyst is prepared through the following steps: (21) Add molecular sieve to metal salt solution at a ratio of 1g:(10-50)mL, mix by ultrasonication, reflux at 60-90℃ for 3h, filter, wash, and dry; (22) Repeat step (21) 1-3 times after drying the molecular sieve, calcining, pressing, and sieving.
2. The catalyst for catalyzing the production of dimethyl ether from high C / H ratio syngas according to claim 1, characterized in that: The mass ratio of the methanol synthesis catalyst to the methanol dehydration catalyst is (1-8):
1.
3. The method for preparing the catalyst for producing dimethyl ether from syngas with a high C / H ratio as described in claim 1, characterized in that: Includes the following steps: (1) Preparation of methanol synthesis catalyst: (11) At 60-90℃, a mixed salt solution of metals Cu, Mn and M and a precipitant solution are simultaneously added dropwise to water. By controlling the dropwise addition rate of the precipitant solution, the pH value of the system is controlled to 7.0-9.
5. (12) Continue aging reaction at 60-90℃ for 2h, then wash, dry, calcinate, press into tablets and sieve to obtain methanol synthesis catalyst; (2) Preparation of methanol dehydration catalyst: (21) Add molecular sieve to metal salt solution at a ratio of 1g:(10-50)mL, mix by ultrasonication, reflux at 60-90℃ for 3h, filter, wash, and dry; (22) Repeat step (21) 1-3 times after drying the molecular sieve, calcining, pressing into tablets, and sieving; (3) Preparation of catalyst: Weigh out the methanol synthesis catalyst and methanol dehydration catalyst, mix them, and the mixture is ready.
4. The method for preparing the catalyst for producing dimethyl ether from syngas with a high C / H ratio according to claim 3, characterized in that: The mixed salt solution of metals Cu, Mn, and M is a salt solution of nitrate, chloride, or acetate of the corresponding metals, and the total concentration of metal Cu, Mn, and M ions in the mixed salt solution is 0.1-1 mol / L.
5. The method for preparing the catalyst for producing dimethyl ether from syngas with a high C / H ratio according to claim 4, characterized in that: The precipitant solution is a NaOH solution, a Na2CO3 solution, or a KOH solution, and the concentration of the precipitant solution is 0.1-1 mol / L.
6. The method for preparing the catalyst for producing dimethyl ether from syngas with a high C / H ratio according to claim 5, characterized in that: The metal salt solution mentioned in step (21) is a nitrate or chloride solution of the corresponding metal, and the concentration of the metal salt solution is 0.1-1 mol / L.
7. The method for preparing the catalyst for producing dimethyl ether from syngas with a high C / H ratio according to claim 6, characterized in that: The drying conditions are drying at 90-150℃ for 5-15 hours, and the sieving is passing through a 20-60 mesh sieve; the roasting conditions in step (12) are roasting at 300-500℃ for 3-10 hours, and the roasting conditions in step (22) are roasting at 350-600℃ for 3-10 hours.
8. A method for catalytically producing dimethyl ether from high C / H ratio syngas, characterized in that: Specifically, the catalyst is loaded into a fixed-bed reactor, hydrogen-containing gas is introduced for reduction and activation, the reaction temperature is adjusted to 200-260℃, and then the syngas is introduced and pressurized to 1-5MPa for reaction; the catalyst is the catalyst described in claim 1.
9. The method for producing dimethyl ether from catalytic high C / H ratio syngas according to claim 8, characterized in that: The hydrogen-containing gas consists of 5-100% hydrogen by volume and the balance gas, which is nitrogen, helium or argon. The conditions for reduction activation are: reduction temperature 250-350℃, reduction time 1-8h, reduction pressure at atmospheric pressure, and hydrogen gas flow rate of 30-100 mL / min. The volume ratio of CO to H2 in the synthesis gas is (2-4):1; the space velocity of the synthesis gas relative to the methanol synthesis catalyst in the catalyst is 2000-8000 h⁻¹. -1 .
Citation Information
Patent Citations
Catalyst for preparing dimethyl ether as well as preparation method and application thereof
CN102600852A
Catalyst for synthesizing dimethyl ether from synthesis gas, method for producing same, and method for synthesizing dimethyl ether using same
CN115254180A
Process for production of hydrocarbons by synthetic gas conversion and catalysts used for process
CN104117380A
Low Pressure Dimethyl Ether Synthesis Catalyst
US20160318006A1