A kind of water-based chloroprene adhesive for automobile interior lamination and preparation method thereof

By using chloroprene emulsion, CPP emulsion, VAE emulsion and modified rosin emulsion in aqueous neoprene, combined with modified zinc oxide and antioxidants, the high activation temperature of aqueous neoprene and high treatment cost of PP material is solved. Problem, low activation temperature and PP processing-free features are achieved, suitable for automotive interior fitting.

CN118222219BActive Publication Date: 2024-12-06FOSHAN DINGSHENG POLYMER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410435087.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-11
Publication Date
2024-12-06
Estimated Expiration
2044-04-11

AI Technical Summary

Technical Problem

The existing water-based chloroprene has a high activation temperature in automotive interior fitting and requires flame, plasma and other treatment of polypropylene (PP) materials, resulting in high cost and energy consumption, which cannot meet the needs of automotive interior fitting.

Method used

Using chloroprene emulsion, CPP emulsion, VAE emulsion and modified rosin emulsion as main components, and adding modified zinc oxide and antioxidants to reduce the activation temperature of aqueous chloroprene by controlling the molecular weight and proportion, and using modified zinc oxide and The modification technology of rosin emulsion improves its dispersion and bonding properties, and realizes the treatment-free characteristics of PP materials.

Benefits of technology

It realizes the low activation temperature of water-based chloroprene and good bonding of PP materials, reduces production costs and energy consumption, is suitable for automotive interior fitting, and has good commercial application value.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a kind of water-based chloroprene rubber for automobile interior fitting and preparation method thereof, wherein the water-based chloroprene rubber comprises the following raw materials by weight: 45-55 parts of chloroprene emulsion, 0.1-0.7 parts of modified zinc oxide, 25-35 parts of CPP emulsion, 5-15 parts of VAE emulsion, 5-15 parts of modified rosin emulsion, and 0.2-0.8 parts of antioxidant. The water-based chloroprene rubber provided by the present invention has low activation temperature and PP treatment-free performance, can be widely used in the field of automobile interior fitting, and has good commercial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of automobile interior lamination, specifically to the field of water-based chloroprene adhesive, and particularly to water-based chloroprene adhesive for automobile interior lamination and a preparation method thereof. Background Art

[0002] Chloroprene, also known as chloroprene rubber, is a synthetic rubber made through polymerization reaction with chlorinated butadiene as the main raw material. Chloroprene has good physical and chemical stability, can maintain elasticity and flexibility over a wide temperature range, and has the characteristics of high initial adhesion and high bonding strength, which makes it widely used in the automotive industry.

[0003] According to the different types of solvents, chloroprene rubber is mainly divided into solvent-based chloroprene rubber and water-based chloroprene rubber. Solvent-based chloroprene rubber contains volatile solvents, which are harmful to the environment, resulting in its limited development. Water-based chloroprene rubber also has some advantages that solvent-based chloroprene rubber does not have, such as good film-forming properties, high cohesive strength, and low price. With the development of environmentally friendly water-based products in the entire industry and people's higher requirements for the performance of chloroprene rubber, water-based chloroprene rubber will become the focus of future development.

[0004] Although water-based chloroprene adhesive has many advantages mentioned above, there are still some unresolved defects. For example, the water-based chloroprene adhesive currently on the market can only be used for sponge bonding and repair of car seats, but cannot be used for interior bonding. This is because the activation temperature of water-based chloroprene adhesive is relatively high; the main material used for car interiors is polypropylene (PP), and whether it is solvent-based or water-based chloroprene adhesive, the PP substrate needs to be treated by flame, plasma, primer, etc. before bonding on the PP material, resulting in a large amount of cost and energy consumption.

[0005] Patent CN 103805097A discloses an environmentally friendly water-based chloroprene type all-purpose adhesive and a preparation method thereof. The water-based chloroprene adhesive of the application is composed of main components such as water-based anionic chloroprene latex, water-based rosin glycerol ester emulsion, and water-based petroleum resin emulsion. It has the advantages of excellent bonding performance, heat resistance, aging resistance, and fast drying time, but does not solve the problem of high activation temperature of water-based chloroprene adhesive. Therefore, whether it can be used for automotive interior bonding still needs to be considered; Patent CN 102876257B discloses a water-based adhesive for automotive interior. The water-based adhesive of the application is a single-component adhesive composed of chloroprene latex, polymer emulsion, water-based thickener, and water-based cross-linking agent. It has the characteristics of fast curing speed and high initial adhesion, but does not mention the problem of no treatment of PP materials commonly used in automotive interiors.

[0006] Therefore, there is an urgent need in the market for a water-based chloroprene adhesive for automotive interior lamination that has a low activation temperature and PP treatment-free performance. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention selects chloroprene emulsion, CPP emulsion, VAE emulsion and modified rosin emulsion as the main components of water-based chloroprene rubber, and then adds modified zinc oxide and antioxidant to prepare a water-based chloroprene rubber for automobile interior lamination, which has the advantages of low activation temperature and PP treatment-free.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] On one hand, the present invention provides a water-based chloroprene rubber for laminating automobile interiors. The water-based chloroprene rubber comprises the following raw materials in parts by weight: 45-55 parts of chloroprene emulsion, 0.1-0.7 parts of modified zinc oxide, 25-35 parts of CPP emulsion, 5-15 parts of VAE emulsion, 5-15 parts of modified rosin emulsion, and 0.2-0.8 parts of antioxidant.

[0010] In some embodiments of the present invention, the chloroprene emulsion is an aqueous chloroprene emulsion with a number average molecular weight of 100,000-200,000.

[0011] The present invention does not impose any special restrictions on the source of the aqueous chloroprene emulsion, which can be purchased commercially, including but not limited to from Nanjing Baiju Technology Co., Ltd.

[0012] The applicant controls the molecular weight of the chloroprene emulsion and its proportion in the water-based chloroprene rubber to make the water-based chloroprene rubber have a lower activation temperature and good initial adhesion strength.

[0013] In some embodiments of the present invention, the method for preparing the modified zinc oxide comprises the following steps:

[0014] 1) mixing halloysite nanotubes and cyclohexane, adding disulfur dichloride dropwise while stirring, heating and stirring under the protection of inert gas, filtering, washing, and drying to obtain product 1 for use;

[0015] 2) Take the product 1 obtained in step 1), add zinc acetate hexahydrate, cadmium nitrate tetrahydrate, glucose and deionized water, stir, ultrasonicate, dry, add titanium dioxide, and calcine to obtain modified zinc oxide.

[0016] In some embodiments of the present invention, in step 1), the mass ratio of halloysite nanotubes to disulfur dichloride is 1:(0.8-1.2); in step 2), the mass ratio of product 1, zinc acetate hexahydrate and cadmium nitrate tetrahydrate is 1:(1.2-1.8):(0.4-0.6).

[0017] Preferably, in step 1), the mass ratio of halloysite nanotubes to disulfur dichloride is 1:1; in step 2), the mass ratio of product 1, zinc acetate hexahydrate and cadmium nitrate tetrahydrate is 1:1.5:0.5.

[0018] The present invention does not impose any special restrictions on the source of the halloysite nanotubes, which can be purchased from commercial sources, including but not limited to Zhengzhou Golden Sunshine Co., Ltd.

[0019] Neoprene itself is self-reinforcing, has excellent mechanical properties, and contains chlorine atoms, which allow it to be used in harsh environments. However, the chlorine atoms it contains will mask the activity of the double bonds, making it unable to form effective chemical bonds under the action of vulcanizing agents such as sulfur, resulting in the inability of neoprene to effectively cross-link. The existing solution is to use metal oxides such as zinc oxide to replace sulfur as a vulcanizing agent, but the addition of zinc oxide will cause the activation temperature of neoprene to increase, which cannot meet the needs of automotive interior fitting.

[0020] The applicant uses the silanol and aluminum hydroxyl groups in the halloysite nanotubes to react with highly reactive dichlorodisulfide to prepare the carrier. The -SS- bonds between the dichlorodisulfide connect the single halloysite nanotubes together to form a stable large-sized tube cluster, thereby increasing the specific surface area of ​​the carrier, which is beneficial to the subsequent Zn 2+ and Cd 2+ The modified zinc oxide formed after loading on the carrier has good dispersibility in water-based chloroprene rubber, thereby reducing the activation temperature of water-based chloroprene rubber; and the applicant introduces zinc acetate hexahydrate and cadmium nitrate tetrahydrate into the carrier, and the two physical phases of zinc oxide and cadmium sulfide produced have a stable interface, and the acetate and Cd 2+ Coordination can be formed between them, which is beneficial to the stable loading of zinc oxide and cadmium sulfide on the carrier; further, the applicant selected glucose containing a large amount of carbon elements as the impregnation liquid during the loading process of zinc oxide and cadmium sulfide, and the CO-Zn bond formed by carbon doping can improve the dispersibility of the active components of zinc oxide, reduce the particle size of the active components of zinc oxide, thereby increasing the number of active sites of the modified zinc oxide, thereby improving the vulcanization effect of the modified zinc oxide on water-based chloroprene rubber; further, the applicant added titanium oxide for compounding, which is beneficial to improve the mechanical properties and heat resistance of the modified zinc oxide.

[0021] In some embodiments of the present invention, the average particle size of the CPP emulsion is 0.4-0.5 μm.

[0022] CPP (chlorinated polypropylene) emulsion can crystallize with the same chemical structure in polyolefins, generating mutually attractive inter-crystal forces, thus having excellent bonding properties to polyolefin non-polar materials, enabling good bonding with PP materials, and realizing the PP treatment-free characteristics of water-based chloroprene rubber.

[0023] In some embodiments of the present invention, the average particle size of the VAE emulsion is 0.3-0.5 μm.

[0024] In some embodiments of the present invention, the method for preparing the modified rosin emulsion comprises the following steps:

[0025] (1) mixing hexadecyltrimethylammonium bromide, ethanol and deionized water, stirring for 25-35 minutes, adding tetraethylenepentamine, stirring for 15-25 minutes, adding cardanol and formaldehyde aqueous solution, stirring, adding tetraethyl orthosilicate, stirring, centrifuging, washing, drying and calcining to obtain a carrier for use;

[0026] (2) taking the support obtained in step (1), adding nickel acetate tetrahydrate and anhydrous ethanol, ultrasonicating, stirring, rotary evaporating, drying and calcining to obtain a catalyst for use;

[0027] (3) mixing rosin and the catalyst obtained in step (2), stirring, adding a solvent and sealing, performing a hydrogenation reaction, cooling to room temperature, standing and collecting the upper oil phase for later use;

[0028] (4) Mix 2-hydroxyethyl acrylate, emulsifier, buffer and deionized water, stir at 50-60° C. for 20-30 min, heat to 70-80° C., add initiator, stir for 30-40 min, then drop the oil phase obtained in step (3), react for 3-4 h, heat to 85-90° C. for 55-65 min, cool to 45-55° C., then drop ammonia water to adjust pH to 6.5-7.5 to obtain modified rosin emulsion.

[0029] Among them, the rosin is loblolly pine rosin.

[0030] In some embodiments of the present invention, in step (2), the mass ratio of the carrier obtained in step (1) to nickel acetate tetrahydrate is 1:(0.4-0.8); in step (4), the mass ratio of 2-hydroxyethyl acrylate to the oil phase obtained in step (3) is (2-4):1.

[0031] Preferably, in step (2), the mass ratio of the carrier obtained in step (1) to nickel acetate tetrahydrate is 1:0.6; in step (4), the mass ratio of 2-hydroxyethyl acrylate to the oil phase obtained in step (3) is 3:1.

[0032] The present invention does not impose any special restrictions on the source of the slash pine rosin, which can be purchased commercially, including but not limited to from Jiangxi Fuda Spice Chemical Co., Ltd.

[0033] Rosin has good tackifying and quick-adhesive properties and is often used as the main component of glue, but it has the disadvantage of being easily oxidized. Acrylic acid ester has good weather resistance, UV resistance and heat resistance, and the high adhesion of acrylate can reduce the activation temperature of rosin emulsion. The applicant selected acrylate as the main component to modify the rosin emulsion, so that the rosin emulsion has a lower activation temperature and good oxidation resistance.

[0034] The applicant selected slash pine rosin as the main raw material of rosin emulsion. The resin acid in slash pine rosin contains a large amount of pimaric acid, which has only two non-conjugated double bonds in its structure and is not prone to isomerization, thereby making the rosin emulsion have a higher solid content and storage stability; further, the applicant prepared a catalyst to hydrogenate the rosin, and reduced the content of unsaturated conjugated double bonds in the rosin through the hydrogenation reaction, thereby increasing the antioxidant and high-temperature stability of the rosin emulsion. On the one hand, the applicant formed a phenolic amine with a network structure by tetraethylenepentamine, long-chain cardanol and formaldehyde, and wrapped tetraethyl orthosilicate in the outer layer of the phenolic amine and the long-chain hexadecyltrimethylammonium bromide, so that the carrier has an amphiphilic and hollow porous structure, which can effectively improve the dispersibility of the catalyst in water, thereby increasing the reaction effect; on the other hand, Ni 2+ The non-precious metal Ni nanoparticles can be coordinated with the N atoms in the carrier, so that the active component Ni nanoparticles anchored by the N atoms in the carrier have good selectivity and activity, thereby promoting the rosin hydrogenation reaction; further, the applicant reacts 2-hydroxyethyl acrylate with hydrogenated rosin to synthesize a modified rosin emulsion. 2-hydroxyethyl acrylate has good flexibility and a large number of cross-linking points, so that it can be well cross-linked with the hydrogenated rosin, and Ni 2+ It can coordinate with the double bond in 2-hydroxyethyl acrylate to form an active center, and the active center can further insert into hydrogenated rosin to form a new active center, which is beneficial to promote the synthesis of modified rosin emulsion; in addition, the hydroxyl group in 2-hydroxyethyl acrylate can also increase the polarity of CPP emulsion, thereby improving the compatibility of CPP emulsion in water-based chloroprene rubber, thereby improving the stability of water-based chloroprene rubber.

[0035] The applicant has made the water-based chloroprene rubber have a lower activation temperature by combining VAE emulsion and modified rosin emulsion, wherein the activation temperature of VAE emulsion is 60-70°C, while the activation temperature of modified rosin emulsion is 30-40°C. By controlling the ratio and using the two together, the activation temperature of the water-based chloroprene rubber can be 50-60°C, which can meet the simultaneous drying and glue activation of the water-based chloroprene rubber and meet the needs of automotive interior bonding.

[0036] In some embodiments of the present invention, the antioxidant is 2-mercaptobenzimidazole.

[0037] Another aspect of the present invention further provides a method for preparing the water-based chloroprene adhesive for automotive interior lamination described in the above technical solution, comprising the following steps:

[0038] S1. Add chloroprene emulsion and modified zinc oxide into a reaction kettle, stir at 80-100 r / min for 40-60 min, and obtain a reaction product for standby use;

[0039] S2. The reaction product obtained in step S1, CPP emulsion, VAE emulsion, modified rosin emulsion and antioxidant are mixed, and stirred at 150-200 r / min for 50-70 min to obtain water-based chloroprene adhesive for automotive interior lamination.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] (1) The present invention selects chloroprene emulsion, CPP emulsion, VAE emulsion and modified rosin emulsion as the main components of water-based chloroprene rubber, and then adds modified zinc oxide and antioxidant to prepare a water-based chloroprene rubber for automotive interior lamination. Through the synergistic effect between the components, the water-based chloroprene rubber has the characteristics of low activation temperature and PP treatment-free.

[0042] (2) The present invention synthesizes a modified zinc oxide as a vulcanizing agent for chloroprene rubber. By modifying the zinc oxide to make it have good dispersibility, the water-based chloroprene rubber has a lower activation temperature, and the water-based chloroprene rubber has good mechanical properties and heat resistance.

[0043] (3) The present invention adds an appropriate amount of CPP emulsion by weight, and utilizes its excellent adhesion to the PP material to make the water-based chloroprene rubber have good adhesion to the PP material, thereby realizing the PP treatment-free characteristic.

[0044] (4) The present invention combines VAE emulsion and modified rosin emulsion to make the water-based chloroprene rubber have a lower activation temperature, thereby meeting the requirements of automotive interior fitting, and the modification of the rosin emulsion further improves the oxidation resistance and stability of the water-based chloroprene rubber.

[0045] (5) The water-based chloroprene rubber prepared by the present invention has a low activation temperature and PP treatment-free performance, can be widely used in the field of automotive interior fitting, and has good commercial application value. DETAILED DESCRIPTION

[0046] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0047] In the following embodiments and comparative examples, except for modified zinc oxide and modified rosin emulsion, the other compound monomers and related reagents used can be purchased from the market, wherein the chloroprene emulsion is an aqueous chloroprene emulsion with a number average molecular weight of 150,000; the halloysite nanotubes are purchased from Zhengzhou Golden Sunshine Co., Ltd.; the CPP emulsion has an average particle size of 0.45 μm, purchased from Wuhan Hyperbranched Resin Technology Co., Ltd., Hubei Province; the VAE emulsion has an average particle size of 0.4 μm, purchased from Jinan Jinbang Environmental Protection Technology Co., Ltd.; and the rosin is slash pine rosin, purchased from Jiangxi Fuda Fragrance Chemical Co., Ltd.

[0048] Preparation Example 1

[0049] The synthesis method of modified zinc oxide A comprises the following steps:

[0050] 1) 10 g of halloysite nanotubes and 100 ml of cyclohexane were mixed, 10 g of disulfur dichloride was added dropwise while stirring, the mixture was heated to 60° C. and stirred for 8 h under nitrogen protection, filtered, washed with anhydrous ethanol for 3 times, and dried at 60° C. for 12 h to obtain product 1 for later use;

[0051] 2) Take 5 g of the product 1 obtained in step 1), add 7.5 g of zinc acetate hexahydrate, 2.5 g of cadmium nitrate tetrahydrate, 12.3 g of glucose and 20 ml of deionized water, stir for 1 h, ultrasonicate for 10 min, dry at 60 ° C for 2 h, add 5 g of titanium dioxide, and calcine at 450 ° C for 3 h to obtain modified zinc oxide A.

[0052] Preparation Example 2

[0053] Modified zinc oxide B, the synthesis method is the same as modified zinc oxide A, the raw materials used and the content of each raw material are basically the same as modified zinc oxide A, the difference is: in step 1), the mass of disulfur dichloride is replaced by 6g.

[0054] Preparation Example 3

[0055] Modified zinc oxide C has the same synthesis method as modified zinc oxide A, and the raw materials used and the content of each raw material are basically the same as modified zinc oxide A, except that: in step 2), the masses of zinc acetate hexahydrate and cadmium nitrate tetrahydrate are replaced by 5g and 1.5g respectively.

[0056] Preparation Example 4

[0057] The synthetic method of modified rosin emulsion A comprises the following steps:

[0058] (1) 0.6 g of hexadecyltrimethylammonium bromide, 75 ml of ethanol and 175 ml of deionized water were mixed and stirred for 30 min, 0.8 ml of tetraethylenepentamine was added and stirred for 20 min, 1.5 g of cardanol and 1.2 ml of 37t% formaldehyde aqueous solution were added and stirred for 2 h, 3 ml of tetraethyl orthosilicate was added and stirred for 4 h, centrifuged, washed with anhydrous ethanol and deionized water 3 times each, dried at 60° C. for 12 h, and calcined at 900° C. for 3 h to obtain a carrier for use;

[0059] (2) Take 2 g of the support obtained in step (1), add 1.2 g of nickel acetate tetrahydrate and 10 ml of anhydrous ethanol, ultrasonicate for 30 min, stir for 30 min, rotary evaporate, dry at 60° C. for 8 h, and calcine at 550° C. for 4 h to obtain a catalyst for use;

[0060] (3) 20 g of rosin and 2 g of the catalyst obtained in step (2) were mixed, stirred for 30 min, 15 ml of solvent (including 10 ml of 200# solvent oil and 5 ml of deionized water) was added, and the mixture was sealed. A hydrogenation device was connected and 4 MPa of H 2 Stir at 150°C for 4 h for hydrogenation reaction, cool to room temperature, stand until stratification, and take the upper oil phase for later use;

[0061] (4) 30 g of 2-hydroxyethyl acrylate, 1.2 g of sodium dodecyl diphenyl ether disulfonate, 5 g of sodium bicarbonate and 50 ml of deionized water were mixed, stirred at 55° C. for 25 min, heated to 75° C., 0.1 g of potassium persulfate was added, stirred for 35 min, 10 g of the oil phase obtained in step (3) was added dropwise, reacted for 3.5 h, heated to 87° C. for 60 min, cooled to 50° C., 25 wt % ammonia water was added dropwise to adjust the pH to 7.0, and modified rosin emulsion A was obtained.

[0062] Preparation Example 5

[0063] The modified rosin emulsion B is synthesized in the same manner as the modified rosin emulsion A. The raw materials and the content of each raw material used are basically the same as those of the modified rosin emulsion A. The difference is that in step (2), the mass of nickel acetate tetrahydrate is replaced by 0.6 g.

[0064] Preparation Example 6

[0065] Modified rosin emulsion C is synthesized in the same manner as modified rosin emulsion A. The raw materials used and the content of each raw material are basically the same as those of modified rosin emulsion A, except that in step (2), the mass of 2-hydroxyethyl acrylate is replaced by 15 g.

[0066] Example 1

[0067] A water-based chloroprene adhesive for automobile interior lamination comprises the following raw materials in parts by weight: 50 parts of chloroprene emulsion, 0.4 parts of modified zinc oxide A, 30 parts of CPP emulsion, 10 parts of VAE emulsion, 10 parts of modified rosin emulsion A, and 0.5 parts of 2-mercaptobenzimidazole.

[0068] The preparation method of water-based chloroprene adhesive for automotive interior lamination in this embodiment comprises the following steps:

[0069] S1. Add chloroprene emulsion and modified zinc oxide A into a reaction kettle, stir at 90 r / min for 50 min, and obtain a reaction product for standby use;

[0070] S2. The reaction product obtained in step S1, CPP emulsion, VAE emulsion, modified rosin emulsion A and 2-mercaptobenzimidazole are mixed, and stirred at 175 r / min for 60 min to obtain water-based chloroprene adhesive for automotive interior lamination.

[0071] Example 2

[0072] A water-based chloroprene adhesive for automobile interior lamination comprises the following raw materials in parts by weight: 45 parts of chloroprene emulsion, 0.4 parts of modified zinc oxide A, 25 parts of CPP emulsion, 5 parts of VAE emulsion, 5 parts of modified rosin emulsion A, and 0.2 parts of 2-mercaptobenzimidazole.

[0073] The preparation method of water-based chloroprene adhesive for automotive interior lamination in this embodiment comprises the following steps:

[0074] S1. Add chloroprene emulsion and modified zinc oxide A into a reactor, stir at 80 r / min for 40 min, and obtain a reaction product for standby use;

[0075] S2. The reaction product obtained in step S1, CPP emulsion, VAE emulsion, modified rosin emulsion A and 2-mercaptobenzimidazole are mixed, and stirred at 150 r / min for 50 min to obtain water-based chloroprene adhesive for automotive interior lamination.

[0076] Example 3

[0077] A water-based chloroprene adhesive for automobile interior lamination comprises the following raw materials in parts by weight: 55 parts of chloroprene emulsion, 0.4 parts of modified zinc oxide A, 35 parts of CPP emulsion, 15 parts of VAE emulsion, 15 parts of modified rosin emulsion A, and 0.8 parts of 2-mercaptobenzimidazole.

[0078] The preparation method of water-based chloroprene adhesive for automotive interior lamination in this embodiment comprises the following steps:

[0079] S1. Add chloroprene emulsion and modified zinc oxide A into a reactor, stir at 100 r / min for 60 min, and obtain a reaction product for standby use;

[0080] S2. The reaction product obtained in step S1, CPP emulsion, VAE emulsion, modified rosin emulsion A and 2-mercaptobenzimidazole are mixed, and stirred at 200 r / min for 70 min to obtain water-based chloroprene adhesive for automotive interior lamination.

[0081] Example 4

[0082] A water-based chloroprene adhesive for automobile interior lamination comprises the following raw materials, measured by weight: 47 parts of chloroprene emulsion, 0.1 parts of modified zinc oxide A, 27 parts of CPP emulsion, 8 parts of VAE emulsion, 10 parts of modified rosin emulsion A, and 0.2 parts of 2-mercaptobenzimidazole.

[0083] The preparation method of the water-based chloroprene adhesive for automobile interior lamination in this embodiment is the same as that in Example 1.

[0084] Example 5

[0085] A water-based chloroprene adhesive for automobile interior lamination comprises the following raw materials, measured by weight: 52 parts of chloroprene emulsion, 0.7 parts of modified zinc oxide A, 32 parts of CPP emulsion, 12 parts of VAE emulsion, 10 parts of modified rosin emulsion A, and 0.6 parts of 2-mercaptobenzimidazole.

[0086] The preparation method of the water-based chloroprene adhesive for automobile interior lamination in this embodiment is the same as that in Example 1.

[0087] Example 6

[0088] This embodiment provides a water-based chloroprene adhesive for automobile interior lamination and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified zinc oxide A is replaced by an equal amount of modified zinc oxide B.

[0089] Example 7

[0090] This embodiment provides a water-based chloroprene adhesive for automobile interior lamination and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that modified zinc oxide C replaces modified zinc oxide A in equal amounts.

[0091] Example 8

[0092] This embodiment provides a water-based chloroprene adhesive for automobile interior lamination and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified rosin emulsion B replaces the modified filler A in equal amounts.

[0093] Example 9

[0094] This embodiment provides a water-based chloroprene adhesive for automobile interior lamination and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified rosin emulsion C replaces the modified filler A in equal amounts.

[0095] Comparative Example 1

[0096] This comparative example provides a water-based chloroprene adhesive for automobile interior lamination and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that zinc oxide is used instead of modified zinc oxide A.

[0097] Comparative Example 2

[0098] This comparative example provides a water-based chloroprene adhesive for automobile interior lamination and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that rosin emulsion is used instead of modified rosin emulsion A.

[0099] Rosin emulsion was purchased from Shandong Haoshun Chemical Co., Ltd.

[0100] Performance Testing

[0101] The activation temperatures of the water-based chloroprene rubbers of Examples 1-9 and Comparative Examples 1-2 were tested, and the test results are shown in Table 1.

[0102] The water-based chloroprene adhesive prepared in the embodiment and the comparative example was sprayed on a PP sheet, heated to dry it and bonded to the PP sheet at the same time, and the lowest heating temperature when bonding was possible was recorded as the activation temperature. The activation temperature was within the range of 50-60°C, which was the water-based chloroprene adhesive suitable for automotive interior bonding.

[0103] Table 1

[0104] Group Activation temperature (℃) Example 1 50℃ Example 2 50.5℃ Example 3 50.8℃ Example 4 52.1℃ Example 5 51.7℃ Example 6 72.4℃ Example 7 65.2℃ Example 8 79.3℃ Example 9 82.2℃ Comparative Example 1 91.5℃ Comparative Example 2 94.1℃

[0105] As can be seen from the data in Table 1, the water-based chloroprene rubber in Examples 1-5 of the present invention has a relatively low activation temperature as a whole, and is suitable for automotive interior lamination. Among them, Examples 6-7 respectively change the ratio between the main components in the modified zinc oxide, so that the dispersibility of the modified zinc oxide decreases, thereby increasing the activation temperature of the water-based chloroprene rubber; Examples 8-9 change the ratio of the main components in the modified rosin emulsion when preparing the catalyst and the addition ratio of the acrylate, so that the cross-linking effect between the modified rosin emulsions decreases, resulting in a decrease in the viscosity of the modified rosin emulsion, thereby significantly increasing the activation temperature of the water-based chloroprene rubber; Comparative Examples 1 and 2 respectively use zinc oxide and rosin emulsion to replace modified zinc oxide A and modified rosin emulsion A. Tests show that the activation temperature of the water-based chloroprene rubber prepared in Comparative Example 1 shows poor results and cannot be used for automotive interior lamination.

[0106] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A water-based chloroprene adhesive for automotive interior lamination, characterized in that: According to weight, it includes the following raw materials: 45-55 parts of chloroprene emulsion, 0.1-0.7 parts of modified zinc oxide, 25-35 parts of CPP emulsion, 5-15 parts of VAE emulsion, 5-15 parts of modified rosin emulsion, 0.2-0.8 parts of antioxidant, The preparation method of the modified zinc oxide comprises the following steps: 1) mixing halloysite nanotubes and cyclohexane, adding disulfur dichloride dropwise while stirring, heating and stirring under the protection of inert gas, filtering, washing, and drying to obtain product 1 for use; 2) Take the product 1 obtained in step 1), add zinc acetate hexahydrate, cadmium nitrate tetrahydrate, glucose and deionized water, stir, ultrasonicate, dry, add titanium dioxide, and calcine to obtain modified zinc oxide. In the step 1), the mass ratio of the halloysite nanotubes to the disulfur dichloride is 1:(0.8-1.2); in the step 2), the mass ratio of the product 1, zinc acetate hexahydrate and cadmium nitrate tetrahydrate is 1:(1.2-1.8):(0.4-0.6); The preparation method of the modified rosin emulsion comprises the following steps: (1) Mix hexadecyltrimethylammonium bromide, ethanol and deionized water, stir for 25-35 minutes, add tetraethylenepentamine, stir for 15-25 minutes, add cardanol and formaldehyde aqueous solution, stir, add tetraethyl orthosilicate, stir, centrifuge, wash, dry and calcine to obtain a carrier for use; (2) taking the carrier obtained in step (1), adding nickel acetate tetrahydrate and anhydrous ethanol, ultrasonicating, stirring, rotary evaporating, drying and calcining to obtain a catalyst for use; (3) mixing the rosin and the catalyst obtained in step (2), stirring, adding a solvent and sealing, performing a hydrogenation reaction, cooling to room temperature, standing and collecting the upper oil phase for later use; (4) Mix 2-hydroxyethyl acrylate, emulsifier, buffer and deionized water, stir at 50-60°C for 20-30 minutes, heat to 70-80°C, add initiator, stir for 30-40 minutes, then drop the oil phase obtained in step (3), react for 3-4 hours, heat to 85-90°C for 55-65 minutes, cool to 45-55°C, drop ammonia water to adjust pH to 6.5-7.5, and obtain modified rosin emulsion. In the step (2), the mass ratio of the carrier obtained in the step (1) to nickel acetate tetrahydrate is 1:(0.4-0.8); in the step (4), the mass ratio of 2-hydroxyethyl acrylate to the oil phase obtained in the step (3) is (2-4):

1.

2. The water-based chloroprene adhesive for automotive interior lamination according to claim 1, characterized in that: The chloroprene emulsion is an aqueous chloroprene emulsion with a number average molecular weight of 100,000-200,000.

3. The water-based chloroprene adhesive for automotive interior lamination according to claim 1, characterized in that: The average particle size of the CPP emulsion is 0.4-0.5 μm.

4. The water-based chloroprene adhesive for automotive interior lamination according to claim 1, characterized in that: The average particle size of the VAE emulsion is 0.3-0.5 μm.

5. The water-based chloroprene adhesive for automotive interior lamination according to claim 1, wherein the antioxidant is 2-mercaptobenzimidazole.

6. A method for preparing the water-based chloroprene adhesive for automotive interior lamination according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Add chloroprene emulsion and modified zinc oxide into a reaction kettle, stir at 80-100 r / min for 40-60 min, and obtain a reaction product for standby use; S2. Mix the reaction product obtained in step S1, CPP emulsion, VAE emulsion, modified rosin emulsion and antioxidant, and stir at 150-200 r / min for 50-70 min to obtain water-based chloroprene adhesive for automotive interior lamination.