A method for annealing aluminum alloy cold-rolled strip

Through the aluminum alloy annealing method that controls the temperature and rolling rate in the drum, combined with liquid nitrogen cooling technology, the problems of hardness reduction and surface damage in the annealing treatment of aluminum alloy are solved, and the low hardness, low stress and high machining of aluminum alloy are achieved meet customer needs.

CN118222947BActive Publication Date: 2024-11-15广西广投正润新材料科技有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410519460.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-11-15
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

The existing aluminum alloy annealing treatment is difficult to meet customer requirements, resulting in reduced hardness, insufficient processability, unelimination of residual stress and unadjusted tissue defects. Moreover, surface scratches or scratches are prone to rewinding after the finished product annealing, affecting the finished product rate. .

Method used

The aluminum alloy cold-rolled strip annealing method is adopted. The aluminum alloy temperature is controlled at 120-150°C at a cooling rate of 3-5°C/min in the drum, and then gradually cooled to 40-50°C, and carried out in an inert protective gas. Annealing treatment, combined with liquid nitrogen cooling technology, optimize the annealing process to reduce hardness and eliminate residual stress and tissue defects.

Benefits of technology

Effectively reduce the hardness of aluminum alloy, improve processability, stabilize size, reduce the tendency of deformation and cracks, refine grains, adjust tissue, eliminate tissue defects, avoid surface damage of finished products, and improve yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118222947B_ABST
    Figure CN118222947B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of aluminum processing, and specifically relates to a method for annealing an aluminum alloy cold-rolled strip. The method comprises the following steps: directly rolling an aluminum alloy in the final cold rolling pass with an iron sleeve having a wall thickness of 3 mm and then performing roller tumbling in batches. The temperature and tumbling time (tumbling rate) are controlled to reduce the hardness of the aluminum alloy, improve the machinability, eliminate residual stress, stabilize the size, reduce the tendency of deformation and cracking, refine the grains, adjust the structure, and eliminate the structure defects.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention belongs to the technical field of aluminum processing, and in particular relates to a method for annealing an aluminum alloy cold-rolled strip. [Background technology]

[0002] Electronic aluminum foil is the raw material of aluminum electrolytic capacitors. It uses high-purity aluminum with an aluminum purity of ≥99.99% as the raw material. It is remelted in a smelting and static holding furnace, and a certain amount of trace elements are added. It is then cast into a plate ingot with a length, width and thickness of about 6500mm*1060mm*365~520mm. The plate ingot is then processed into electronic aluminum foil through processes such as milling, heat treatment, hot rolling, cold rolling, foil rolling, intermediate annealing, foil rolling, cleaning, shearing, and finished product annealing. The aluminum foil is then corroded and chemically formed, and then stripped into anodes in aluminum electrolytic capacitors.

[0003] For our company's model 1060 soft annealed products, in order to meet customer requirements, reduce the hardness of aluminum alloy, improve machinability, eliminate residual stress, stabilize size, reduce deformation and crack tendency, refine grains, adjust structure, and eliminate structural defects, some products require finished product annealing.

[0004] There are many methods for preparing aluminum foil at present, for example, Chinese patent CN108300911A discloses a method for producing 8111 alloy aluminum foil from cast-rolled billets, which is divided into the following steps in sequence: furnace loading, batching, powder spraying refining, first liquid refining, slag removal, furnace pouring, second liquid refining, static filtration, cast-rolling, first cold rolling, homogenization annealing, second cold rolling, rewinding intermediate trimming, third cold rolling, intermediate annealing, fourth cold rolling, rewinding finished product trimming, inspection, and finished product packaging. The 8111 alloy aluminum foil billet produced by the cast-rolling method has good processing structure performance, and the aluminum foil has a fine surface, which can completely replace the hot rolling method product. The 8111 alloy produced by the cast-rolling method overcomes the defect of many pinholes in the hot rolling method, saves energy, shortens the production cycle, and reduces production costs. CN116967284A discloses a medium-high voltage electronic aluminum foil for aluminum electrolytic capacitors and a preparation method thereof. The method comprises: placing aluminum ingots and aluminum master alloys in a melting furnace, heating and melting to obtain aluminum liquid, heat preservation, refining, standing, casting, sawing, milling, homogenization annealing, hot rolling, cold rolling, rewinding and trimming, cold rolling, foil rolling, intermediate annealing, foil rolling, cleaning, shearing and coiling, and finished product annealing to obtain medium-high voltage electronic aluminum foil for aluminum electrolytic capacitors. The method reduces the hot rolling process passes and increases the average pass reduction rate on the basis of the existing medium-high voltage electronic aluminum foil production process, that is, the hot rolling process is reduced from 17 passes to 11-15 passes, and the average pass reduction rate is increased from 20% to more than 22%. The non-cubic grains of the medium-high voltage electronic aluminum foil for aluminum electrolytic capacitors obtained by the method do not have linear aggregation, which solves the problem of being unable to eliminate the linear aggregation of non-cubic grains and has good application prospects. [Summary of the invention]

[0005] In the actual production process of the prior art, in order to meet customer requirements, reduce the hardness of aluminum alloy, improve machinability, eliminate residual stress, stabilize size, reduce deformation and crack tendency, refine grains, adjust structure, and eliminate structural defects, some products require finished product annealing. However, in many cases, the annealing and cooling operation may not necessarily meet customer requirements, and it is found that after annealing, the steel sleeve must be rewound and poured out. When rewinding the soft product, a lot of scratches or scratches will be generated on the surface, affecting the yield rate; in view of this situation, the present invention provides a method for annealing aluminum alloy cold-rolled strip, which can effectively reduce the hardness of aluminum alloy, improve machinability, eliminate residual stress, stabilize size, reduce deformation and crack tendency, refine grains, adjust structure, and eliminate structural defects.

[0006] The purpose of the present invention is achieved through the following technical solutions:

[0007] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0008] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0009] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0010] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 120-150°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds, for a time of 15-35S;

[0011] 4) Control the drum to roll clockwise, control the temperature of the aluminum alloy at 70-100°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 15-30S;

[0012] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 40-50°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 10-25S, and then enter the annealing process.

[0013] In the present invention, a further preferred solution is that the cooling in steps 3) to 5) is carried out by cooling with liquid nitrogen.

[0014] In the present invention, a further preferred solution is that in step 3), when the temperature of the aluminum alloy is controlled at 130-140° C., the tumbling time is controlled at 20-30 seconds.

[0015] In the present invention, a further preferred solution is that in step 4), when the temperature of the aluminum alloy is controlled at 80-90° C., the tumbling time is controlled at 20-25 seconds.

[0016] In the present invention, a further preferred solution is that in step 5), when the temperature of the aluminum alloy is controlled at 43-48° C., the tumbling time is controlled at 15-20 seconds.

[0017] In the present invention, a further preferred solution is that in step 5), the annealing process needs to be carried out in an inert protective gas.

[0018] The inert protective gas is nitrogen or argon.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] The present invention discloses a method for annealing an aluminum alloy cold-rolled strip. First, the aluminum alloy of the final cold-rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then roller tumbling is performed in batches. Controlling the temperature and tumbling time (tumbling rate) can reduce the hardness of the aluminum alloy, improve the machinability, eliminate residual stress, stabilize the size, reduce deformation and crack tendency, refine the grains, adjust the structure, and eliminate structural defects.

Brief Description of the Drawings

[0021] Figure 1-3 They are respectively the grain maps of the aluminum foils of Examples 1-3 of the present application;

[0022] Figure 4 It is a grain map of some comparative examples, specifically the grain map of the aluminum foil of comparative example 12. [Specific implementation method]

[0023] The specific implementation modes of the present invention are further described below in conjunction with examples.

[0024] Embodiment 1:

[0025] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0026] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0027] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0028] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 120°C at a cooling rate of 3-5°C / min, and at the same time, turn one circle every 5 seconds for 15 seconds;

[0029] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 70°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 15S;

[0030] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 40°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 10S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling.

[0031] Embodiment 2:

[0032] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0033] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0034] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0035] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 130°C at a cooling rate of 3-5°C / min, and at the same time, rotate one circle every 5 seconds for 20 seconds;

[0036] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 80°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S;

[0037] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 43°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 15S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling.

[0038] Embodiment 3:

[0039] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0040] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0041] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0042] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0043] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0044] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling.

[0045] Embodiment 4:

[0046] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0047] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0048] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0049] 3) Control the roller to roll clockwise, control the temperature of the aluminum alloy within 150°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds, for 35 seconds;

[0050] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 100°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 30S;

[0051] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 50°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. Comparative Example 1:

[0052] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0053] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0054] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0055] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 1°C / min, and at the same time rotate one circle every 5 seconds for 25 seconds;

[0056] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0057] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. Comparative Example 2:

[0058] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0059] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0060] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0061] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0062] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 5°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0063] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. Comparative Example 3:

[0064] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0065] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0066] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0067] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0068] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 5°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0069] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 5°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling.

[0070] Comparative Example 4:

[0071] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0072] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0073] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0074] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0075] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 60°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0076] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to turn one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. Comparative Example 5:

[0077] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0078] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0079] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0080] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0081] 4) Control the drum to roll clockwise, control the temperature of the aluminum alloy at 110°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0082] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. . Comparative Example 6:

[0083] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0084] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0085] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0086] 3) Control the roller to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds for 10 seconds;

[0087] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0088] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. The cooling method used in steps 3)-5) is liquid nitrogen cooling. Comparative Example 7:

[0089] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0090] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0091] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0092] 3) Control the roller to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds for 40 seconds;

[0093] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0094] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to turn one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. Comparative Example 8:

[0095] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0096] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0097] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0098] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0099] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, and control the rolling rate to one circle every 5 seconds, for 10 seconds;

[0100] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to turn one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. Comparative Example 9:

[0101] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0102] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0103] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0104] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0105] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 35S;

[0106] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. Comparative Example 10:

[0107] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0108] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0109] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0110] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0111] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0112] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to turn one circle every 5 seconds, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling.

[0113] Comparative Example 11:

[0114] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0115] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0116] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0117] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0118] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0119] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 30S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. Comparative Example 12:

[0120] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0121] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0122] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0123] 3) Control the roller to roll counterclockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0124] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0125] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. The cooling method used in steps 3)-5) is liquid nitrogen cooling. Comparative Example 13:

[0126] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0127] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0128] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0129] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0130] 4) Control the roller to roll counterclockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0131] 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling. Comparative Example 14:

[0132] A method for annealing an aluminum alloy cold-rolled strip comprises the following steps:

[0133] 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s;

[0134] 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum;

[0135] 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 140°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds at a rolling rate, for 25 seconds;

[0136] 4) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 90°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 25S;

[0137] 5) Control the roller to roll counterclockwise, control the temperature of the aluminum alloy at 48°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 20S, and then enter the annealing process; the annealing process needs to be carried out in an inert protective gas. The inert protective gas is nitrogen or argon. Steps 3)-5) use liquid nitrogen cooling.

[0138] test:

[0139] The aluminum alloys prepared in Examples 1-4 and Comparative Examples 1-14 were tested for tensile strength, elongation, yield strength, and grain cracking.

[0140] Table 1

[0141] Tensile strength(MPa) Elongation(%) Yield strength (MPa) Grain Example 1 119 11 117 Refinement Example 2 121 7 117 Refinement Example 3 125 10.5 111 Refinement Example 4 124 8.5 122 Refinement Comparative Example 1 105 16 103 Too small Comparative Example 2 168 3.5 161 Too big Comparative Example 3 164 3.5 161 Too big Comparative Example 4 173 4.3 163 Too big Comparative Example 5 179 3 171 Too big Comparative Example 6 179 3.3 168 Too big Comparative Example 7 165 3.5 157 Too big Comparative Example 8 184 3.0 176 Too big Comparative Example 9 170 3.5 162 Too big Comparative Example 10 174 3.0 165 Too big Comparative Example 11 185 3.8 175 Too big Comparative Example 12 176 4.0 169 Too big Comparative Example 13 174 5.2 167 Too big Comparative Example 14 182 3.0 172 Too big

[0142] in conclusion:

[0143] The aluminum alloy surfaces of Examples 1, 2, 3, and 4 have no cracks, bubbles, or peeling; the hardness is correspondingly reduced, and the residual stress is eliminated.

[0144] In Comparative Example 1, the cooling rate in the first stage is too slow, and the surface hardness of the aluminum alloy decreases too much.

[0145] In Comparative Example 2, the cooling rate in the second stage is too fast, and the surface hardness of the aluminum alloy is too high.

[0146] In comparative example 3, the cooling rate in the third stage is too fast, and the surface hardness of the aluminum alloy is too high.

[0147] In Comparative Example 4, the temperature in the second stage is controlled too low, and the surface hardness of the aluminum alloy is too high.

[0148] In Comparative Example 5, the temperature in the second stage is controlled too high, and the surface hardness of the aluminum alloy is too high.

[0149] In comparative example 6, the first stage controlled flipping time is too short, and the surface hardness of the aluminum alloy is too high.

[0150] In comparative example 7, the first stage controlled flipping time is too long, and the surface hardness of the aluminum alloy is too high.

[0151] In Comparative Example 8, the second stage controlled flipping time is too short, and the surface hardness of the aluminum alloy is too high.

[0152] In comparative example 9, the second stage controlled flipping time is too long, and the surface hardness of the aluminum alloy is too high.

[0153] In comparative example 10, the third stage controlled flipping time is too short, and the surface hardness of the aluminum alloy is too high.

[0154] In comparative example 11, the third stage controlled flipping time is too long and the surface hardness of the aluminum alloy is too high.

[0155] In comparative example 12, counterclockwise tumbling was adopted in the first stage, and clockwise tumbling was adopted in the second and third stages, and the surface hardness of the aluminum alloy was relatively large.

[0156] In comparative example 13, counterclockwise tumbling was adopted in the second stage, and clockwise tumbling was adopted in the first and third stages, and the surface hardness of the aluminum alloy was relatively large.

[0157] In comparative example 14, counterclockwise tumbling was adopted in the third stage, and clockwise tumbling was adopted in the first and second stages, and the surface hardness of the aluminum alloy was relatively large.

[0158] Figure 1-3 These are the grain refinement effect diagrams of the aluminum foils of Examples 1-3 of the present application, respectively, indicating that the grain refinement effect is obvious after the treatment of the examples. Figure 4 This is a graph showing the grain refinement effect of the aluminum foil of comparative example 12. The grains are relatively coarse, and the tensile strength and yield strength are relatively high, which is not conducive to further stamping processing.

[0159] In summary, the aluminum foil obtained by the method of the present invention meets customer needs and can reduce the hardness of aluminum alloy, improve machinability, eliminate residual stress, stabilize size, reduce deformation and crack tendency, refine grains, adjust structure, and eliminate tissue defects.

[0160] The above description is a detailed description of the preferred feasible embodiments of the present invention, but the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modified changes completed under the technical spirit suggested by the present invention should fall within the patent scope covered by the present invention.

Claims

1. A method for annealing an aluminum alloy cold-rolled strip, characterized in that: The steps include: 1) cold rolling the aluminum alloy, wherein the cold rolling speed is ≤0.5 m / s; 2) The aluminum alloy of the final cold rolling pass is directly rolled onto an iron sleeve with a wall thickness of 3 mm and then placed into the drum; 3) Control the drum to roll clockwise, control the temperature of the aluminum alloy within 120-150°C at a cooling rate of 3-5°C / min, and at the same time rotate one circle every 5 seconds, for a time of 15-35S; 4) Control the drum to roll clockwise, control the temperature of the aluminum alloy at 70-100°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 15-30S; 5) Control the roller to roll clockwise, control the temperature of the aluminum alloy at 40-50°C at a cooling rate of 1-3°C / min, control the rolling rate to one circle every 5 seconds, and the time is 10-25S, and then enter the annealing process.

2. The method for annealing an aluminum alloy cold-rolled strip according to claim 1, characterized in that: The cooling in steps 3) to 5) is carried out by cooling with liquid nitrogen.

3. The method for annealing an aluminum alloy cold-rolled strip according to claim 1, characterized in that: In step 3), when the temperature of the aluminum alloy is controlled at 130-140° C., the tumbling time is controlled at 20-30 seconds.

4. The method for annealing an aluminum alloy cold-rolled strip according to claim 1, characterized in that: In step 4), when the temperature of the aluminum alloy is controlled at 80-90° C., the tumbling time is controlled at 20-25 seconds.

5. The method for annealing an aluminum alloy cold-rolled strip according to claim 1, characterized in that: In step 5), when the temperature of the aluminum alloy is controlled at 43-48° C., the tumbling time is controlled at 15-20 seconds.

6. The method for annealing an aluminum alloy cold-rolled strip according to claim 1, characterized in that: In step 5), the annealing process needs to be performed in an inert protective gas.

Citation Information

Patent Citations

  • Method for producing 8111 alloy aluminum foil using cast-rolled billets

    CN108300911A

  • Medium-high voltage electronic aluminum foil for aluminum electrolytic capacitor and preparation method of medium-high voltage electronic aluminum foil

    CN116967284A

  • Method for producing high-strength low-residual-stress aluminum foil

    CN109554642A

  • Method for solving aluminum foil annealing wrinkles

    CN112662968A

  • WINDING METHOD OF COLD-ROLLED STRIP INTO A ROLL

    RU2006110714A