In-situ polymerized solid electrolyte, method for preparing solid electrolyte by in-situ polymerization, solid-state battery, method for preparing solid-state battery, and electrical device
By using a combined in-situ polymerization method of room temperature initiators and high temperature initiators in lithium metal batteries, the energy density and safety issues of traditional lithium metal batteries are solved, the uniformity and stability of solid-state batteries are improved, and the finished product of the battery is improved Rate.
Patent Information
- Application Number
- CN202410645789.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-05-23
AI Technical Summary
The energy density of traditional lithium metal batteries is limited by traditional electrolyte leakage and flammability and explosion problems. In addition, the polymerization inhomogeneity of in-situ polymerized solid electrolytes results in a low yield rate of solid-state batteries, making it difficult to meet industrial promotion.
Using an in-situ polymerization method that combines room temperature initiators and high temperature initiators, through room temperature prepolymerization and high temperature thermal polymerization, a uniform solid electrolyte is formed to improve the molding quality stability of the battery.
It improves the uniformity and safety of solid-state batteries, enhances lithium-ion transmission efficiency, and improves the molding quality stability and yield rate of solid-state batteries.
Smart Images

Figure CN118231759B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to an in-situ polymerized solid electrolyte, a method for preparing a solid electrolyte by in-situ polymerization, a solid-state battery, a method for preparing a solid-state battery, and an electrical device. Background Art
[0002] With the continuous development of social economy, portable devices, electric vehicles and long-range energy storage devices require rechargeable batteries with long cycle and high energy density. Lithium-ion batteries have profoundly changed our daily life. However, the energy density of lithium-ion batteries is approaching 350 Wh∙kg. −1 Compared with lithium-ion batteries, the practical energy density of lithium metal batteries can exceed 400 Wh∙kg −1 , which is due to the high specific capacity and low electrode potential of lithium metal anode. However, the leakage of traditional electrolyte and safety issues such as flammability and explosion limit the application of lithium metal batteries.
[0003] Solid electrolytes such as polymer electrolytes can improve such problems and promote the practical application of lithium metal batteries. Traditional polymer preparation methods such as solution casting are complicated and often have safety and environmental issues caused by solvent evaporation. In addition, polymer electrolytes prepared by traditional methods are generally thicker, which reduces the energy density of the battery, increases the transmission distance of lithium ions, and is difficult to fill the gaps in the electrodes to achieve good contact between the electrolyte and the electrodes.
[0004] In-situ polymerization is a simple method for preparing polymer electrolytes that is compatible with existing commercial battery production. It can obtain thin and uniform polymer electrolytes, and it has excellent compatibility with the electrode interface, which helps to reduce the interface impedance and increase the lithium ion transmission flux at the interface. However, in-situ polymerized solid electrolytes often have the phenomenon of uneven polymerization, which makes the yield of solid-state batteries too low and difficult to meet the requirements of industrial promotion. Therefore, the polymerization uniformity of in-situ polymerized solid electrolytes needs to be further improved to improve the molding quality stability of solid-state batteries.
[0005] The methods described in this section are not necessarily methods that have been previously conceived or employed. Unless otherwise indicated, it should not be assumed that any method described in this section is considered to be prior art simply because it is included in this section. Similarly, unless otherwise indicated, the issues mentioned in this section should not be considered to have been recognized in any prior art. Summary of the invention
[0006] The present application is made in view of the above-mentioned demands, and its purpose is to provide an in-situ polymerized solid electrolyte, a method for preparing a solid electrolyte by in-situ polymerization, a solid-state battery, a method for preparing a solid-state battery, and an electrical device.
[0007] The first aspect of the present application provides an in-situ polymerized solid electrolyte, comprising: a room temperature initiator, a high temperature initiator, and a cyclic monomer polymer.
[0008] The second aspect of the present application provides a method for preparing a solid electrolyte by in-situ polymerization, comprising: mixing raw materials including a room temperature initiator, a high temperature initiator, and a cyclic monomer to form a precursor solution; after the precursor solution is allowed to stand at room temperature, thermally polymerize at a high temperature to obtain the solid electrolyte.
[0009] The third aspect of the present application provides a solid-state battery, comprising the solid-state electrolyte of the first aspect or the solid-state electrolyte prepared by the preparation method of the second aspect.
[0010] The fourth aspect of the present application provides a method for preparing a solid-state battery, comprising: mixing raw materials including a room temperature initiator, a high temperature initiator, a cyclic monomer, and an electrolyte salt to form a precursor solution; injecting the precursor solution into a battery cell; after the battery is allowed to stand at room temperature, thermally polymerizing at a high temperature to obtain the solid-state battery.
[0011] The fifth aspect of the present application provides an electrical device, comprising the solid-state battery of the third aspect of the present application or the solid-state battery prepared by the preparation method of the fourth aspect.
[0012] In the present application, the room temperature initiator can play a role during the static period after the battery is filled with liquid, and the precursor solution can be pre-polymerized at room temperature while satisfying the electrolyte infiltration of the electrode, thereby improving the uniformity of the precursor solution contained in each part of the battery and avoiding the solid-liquid stratification phenomenon in the precursor solution. The high temperature initiator can improve the solidification degree of the entire electrolyte, improve the ion transmission efficiency and safety of the solid electrolyte. In summary, through the joint action of the room temperature initiator and the high temperature initiator, the uniformity of the in-situ polymerized solid electrolyte can be improved, and the molding quality stability of the solid-state battery can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Further details, features and advantages of the present disclosure are disclosed in the following description of exemplary embodiments in conjunction with the accompanying drawings, in which:
[0014] Figure 1 is a diagram of the dispersion state of an in-situ polymerized solid electrolyte according to an exemplary embodiment and the prior art. DETAILED DESCRIPTION
[0015] The following embodiments of the technical solution of the present application will be described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0016] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0017] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0018] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0019] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0020] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0021] It should be understood that in this specification, the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships or dimensions that are based on the orientations or positional relationships or dimensions shown in the accompanying drawings, and these terms are used only for the convenience of description and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the scope of protection of the present application.
[0022] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0023] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0024] In-situ polymerized solid electrolytes in the prior art are usually synthesized by thermal polymerization of precursor solutions. However, in the actual application of batteries, a long period of standing is required before thermal polymerization to promote the infiltration of the precursor solution in the pole piece to reduce the interface resistance of the solid-state battery. During the standing process, the components in the precursor solution will gradually be unevenly distributed, resulting in uneven curing of the various parts after polymerization, and even solid-liquid stratification, which will have an adverse effect on the safety, batch stability and electrochemical performance of the battery.
[0025] Based on this, the first aspect of the present application provides an in-situ polymerized solid electrolyte, comprising: a room temperature initiator, a high temperature initiator and a cyclic monomer polymer.
[0026] Herein, a room temperature initiator refers to an initiator that can generate Lewis acid to initiate the in-situ polymerization of cyclic monomers to form polymers at room temperature, such as 0-29°C. Lewis acid, also known as an electrophilic reagent, refers to a substance (including ions, atomic groups or molecules) that can accept electron pairs.
[0027] Herein, the high temperature initiator refers to an initiator that can generate Lewis acid to initiate the in-situ polymerization of cyclic monomers to generate polymers under high temperature conditions, such as 30-100°C.
[0028] Herein, the cyclic monomer polymer refers to the product generated by polymerization of the cyclic monomer by an initiator, and there is no limitation on the degree of polymerization.
[0029] Room temperature initiators can play a role during the static period after the battery is filled with liquid, allowing the precursor solution to undergo room temperature prepolymerization while satisfying the electrolyte infiltration of the electrode, thereby improving the uniformity of the precursor solution contained in each part of the battery and avoiding the solid-liquid stratification phenomenon in the precursor solution. High temperature initiators can improve the solidification degree of the entire electrolyte, improve the ion transfer efficiency and safety of the solid electrolyte. In summary, through the joint action of room temperature initiators and high temperature initiators, the uniformity of the in-situ polymerized solid electrolyte can be improved, and the molding quality stability of the solid-state battery can be improved.
[0030] In some embodiments, the room temperature initiator includes one or more of lithium hexafluorophosphate, aluminum trifluoromethanesulfonate (Al(OTF)3), scandium trifluoromethanesulfonate (Sc(OTf)3), tin difluoride (SnF2), and copper trifluoromethanesulfonate (Cu(OTf)2).
[0031] In some embodiments, the room temperature initiator includes lithium hexafluorophosphate.
[0032] Lithium hexafluorophosphate can be used as a room temperature initiator and is also a commonly used electrolyte salt. Its addition will not have a negative impact on other battery properties and is beneficial to improving the overall performance of the battery.
[0033] In some embodiments, the high temperature initiator includes one or more of stannous octoate, lithium difluorooxalatoborate (LIDFOB), lithium borohydride (LiBH4), lithium aluminum hydride (LiAlH4, LAH), and lithium tri-tert-butoxyaluminum hydride (LiAlH[OC(CH3)3]3, LTBA).
[0034] In some embodiments, the cyclic monomer includes one or more of cyclic monoolefins, cyclic polyolefins, cycloalkanes, cyclic ethers, cyclic acetals, cyclic esters, cyclic amides, cyclosiloxanes, cyclic ketones, and cyclic thiols; optionally, the cyclic monomer includes cyclic ethers, which can be one or more of 1,3,5-trioxane (TXE), 1,3-dioxane, 1,4-dioxane, and 1,3-dioxolane (DOL).
[0035] In some embodiments, the solid electrolyte further includes an electrolyte salt, and the electrolyte salt includes one or more of lithium bis(trifluoromethane)sulfonyl imide (LITFSI), lithium bis(fluorosulfonyl)imide (LIFSI), lithium bis(oxalate borate) (LIBOB), and lithium tetrafluoroborate (LIBF4).
[0036] Electrolyte salts can adjust the solvation structure of lithium ions and further improve the cycle performance of solid-state batteries.
[0037] In some embodiments, the mass ratio of the room temperature initiator to the high temperature initiator is 1:1-1:10.
[0038] In some embodiments, the mass ratio of the room temperature initiator to the high temperature initiator may be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10 or any range therebetween.
[0039] The solid electrolyte having a mass ratio of the room temperature initiator to the high temperature initiator within the above range can have both good curing degree and uniformity, and comprehensively improve the molding quality stability of the battery.
[0040] In some embodiments, the mass ratio of the high temperature initiator to the cyclic monomer polymer is 1:100-10:100.
[0041] In some embodiments, the mass ratio of the high temperature initiator to the cyclic monomer polymer may be 1:100, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100, 10:100 or any range therebetween.
[0042] In some embodiments, the mass ratio of the electrolyte salt to the cyclic monomer polymer is 5:100-10:100.
[0043] In some embodiments, the mass ratio of the electrolyte salt to the cyclic monomer polymer may be 5:100, 6:100, 7:100, 8:100, 9:100, 10:100 or any range therebetween.
[0044] In some embodiments, the solid electrolyte further includes an additive.
[0045] In some embodiments, the additive includes one or more of lithium nitrate, imidazole ionic liquids, pyrrole ionic liquids, and fluorinated solvents. Optionally, the fluorinated solvent includes one or more of fluoroethylene carbonate, methyl trifluoroethyl carbonate (FEMC), bisfluoroethylene carbonate (DFEC), tris(2,2,2-trifluoroethyl) phosphate (TFEP), bis(2,2,2-trifluoroethyl) carbonate (TFEC), 2,2,2-trifluoroethyl ether (BTFE), ethyl trifluoroacetate (ETFA), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.
[0046] The above additives can improve the stability of the solid electrolyte interface film on the surface of the negative electrode, protect the negative electrode, especially the lithium metal negative electrode, and further improve the cycle life of the battery.
[0047] In some embodiments, the mass ratio of the additive to the cyclic monomer polymer is 1:100-5:100.
[0048] In some embodiments, the mass ratio of the additive to the cyclic monomer polymer may be 1:100, 2:100, 3:100, 4:100, 5:100 or any range therebetween.
[0049] The second aspect of the present application provides a method for preparing a solid electrolyte by in-situ polymerization, comprising: mixing raw materials including a room temperature initiator, a high temperature initiator, and a cyclic monomer to form a precursor solution; after the precursor solution is allowed to stand at room temperature, thermally polymerize at a high temperature to obtain the solid electrolyte.
[0050] The room temperature initiator can play a role during the static period, allowing the precursor solution to undergo room temperature prepolymerization while satisfying the electrolyte infiltration of the electrode, thereby improving the uniformity of the precursor solution contained in each part of the battery and avoiding the solid-liquid stratification phenomenon in the precursor solution. The high temperature initiator can improve the solidification degree of the entire electrolyte, improve the ion transfer efficiency and safety of the solid electrolyte. In summary, through the joint action of the room temperature initiator and the high temperature initiator, the uniformity of the in-situ polymerized solid electrolyte can be improved, and the molding quality stability of the solid-state battery can be improved.
[0051] In some embodiments, the precursor solution is allowed to stand at room temperature for 36-50 hours.
[0052] In some embodiments, the standing time of the precursor solution at room temperature can be 36 hours, 40 hours, 45 hours, 50 hours, or any range therebetween.
[0053] In some embodiments, the polymerization temperature of the thermal polymerization at high temperature is 30-100° C.; and / or the polymerization time of the thermal polymerization at high temperature is 0.5-1.5 hours.
[0054] In some embodiments, the polymerization temperature of the thermal polymerization at high temperature can be selected as 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C or any range therebetween.
[0055] In some embodiments, the polymerization time of thermal polymerization at high temperature can be selected as 0.5 hours, 1 hour, 1.5 hours, or any range therebetween.
[0056] In some embodiments, the raw materials also include electrolyte salts and additives, and the mixing of raw materials including a room temperature initiator, a high temperature initiator, and a cyclic monomer to form a precursor solution includes: mixing the cyclic monomer, the electrolyte salt, and the additive to obtain a first mixture; mixing the first mixture with a high temperature initiator to obtain a second mixture; mixing the second mixture with a room temperature initiator to obtain a precursor solution.
[0057] The above method can minimize the effect of adding a room temperature initiator on the viscosity of the precursor solution, thereby improving the injectability of the precursor solution.
[0058] In some embodiments, the mass ratio of the room temperature initiator to the high temperature initiator is 1:1-1:10.
[0059] In some embodiments, the mass ratio of the high temperature initiator to the cyclic monomer is 1:100-10:100.
[0060] In some embodiments, the mass ratio of the electrolyte salt to the cyclic monomer is 5:100-10:100.
[0061] A third aspect of the present application provides a solid-state battery, comprising a solid-state electrolyte according to any embodiment or a solid-state electrolyte prepared by a method according to any embodiment.
[0062] In some embodiments, the solid-state battery includes a lithium metal anode.
[0063] The fourth aspect of the present application provides a method for preparing a solid-state battery, comprising: mixing raw materials including a room temperature initiator, a high temperature initiator, a cyclic monomer, and an electrolyte salt to form a precursor solution; injecting the precursor solution into a battery cell; after the battery is allowed to stand at room temperature, thermally polymerizing at a high temperature to obtain the solid-state battery.
[0064] The solid electrolyte obtained by the solid-state battery prepared by this method is thin and uniform, and has a low interface impedance with the electrolytic interface, so that the solid-state battery has high molding quality stability.
[0065] A fifth aspect of the present application provides an electrical device, comprising a solid-state battery of any embodiment or a solid-state battery prepared by a preparation method of any embodiment.
[0066] Example
[0067] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0068] 1. Preparation method
[0069] Example 1
[0070] 1) Preparation of precursor solution
[0071] At room temperature, 100 parts by mass, 5 parts by mass, 4 parts by mass, and 1 part by mass of cyclic monomer 1,3,5-trioxane (TXE), electrolyte salt lithium bis(oxalyl)borate (LiBOB), additive FEC, and N-propyl-N-methylpyrrolidine nitrate were weighed and put into a glass bottle, respectively, and mixed evenly to obtain a first mixture; 5 parts by mass of high-temperature initiator LIDFOB were added, and mixed evenly to obtain a second mixture. 1 part by mass of room-temperature initiator lithium hexafluorophosphate LIPF6 was added to the second mixture to form a precursor solution.
[0072] 2) Battery assembly
[0073] NCM811 is used as the positive electrode active material of the battery, and lithium is used as the negative electrode of the battery. After the positive electrode sheet, separator, and negative electrode sheet are stacked, the newly configured precursor solution is injected to complete the assembly of the battery.
[0074] The battery was left standing at room temperature for 48 hours to allow the room temperature initiator to take effect, and then placed in an oven at 80 degrees Celsius for thermal polymerization for 1 hour to allow the high temperature initiator to take effect, thereby forming a solid electrolyte in situ.
[0075] Example 2
[0076] The battery assembly method of Example 2 is consistent with that of Example 1, except that the preparation method of the precursor solution is different: the room temperature initiator in the precursor solution in Example 2 is aluminum trifluoromethanesulfonate (Al(OTF)3).
[0077] Example 3
[0078] The battery assembly method of Example 3 is consistent with that of Example 1, except that the preparation method of the precursor solution is different: the high-temperature initiator in the precursor solution of Example 3 is stannous octoate.
[0079] Example 4
[0080] The battery assembly method of Example 4 is consistent with that of Example 1, except that the preparation method of the precursor solution is different: in Example 4, the mass ratio of the room temperature initiator to the high temperature initiator in the precursor solution is 1:1.
[0081] Example 5
[0082] The battery assembly method of Example 5 is consistent with that of Example 1, except that the preparation method of the precursor solution is different: in Example 5, the mass ratio of the room temperature initiator to the high temperature initiator in the precursor solution is 1:10.
[0083] Comparative Example 1
[0084] The battery assembly method of Comparative Example 1 is consistent with that of Example 1, except that the preparation method of the precursor solution is different: the preparation method of the precursor solution in Comparative Example 1 is as follows:
[0085] At room temperature, 100 parts by mass, 5 parts by mass, 4 parts by mass and 1 part by mass of cyclic monomer 1,3,5-trioxane (TXE), electrolyte salt lithium bis(oxalyl)borate (LiBOB), additive FEC and N-propyl-N-methylpyrrolidine nitrate were weighed and put into a glass bottle respectively, and mixed evenly to obtain a first mixture; then 5 parts by mass of high temperature initiator LIDFOB was added, and mixed evenly to obtain a second mixture.
[0086] Comparative Example 2
[0087] The battery assembly method of Comparative Example 2 is consistent with that of Example 1, except that the preparation method of the precursor solution is different: the preparation method of the precursor solution in Comparative Example 2 is as follows:
[0088] At room temperature, 100 parts by mass, 5 parts by mass, 4 parts by mass, and 1 part by mass of cyclic monomer 1,3,5-trioxane (TXE), electrolyte salt lithium bis(oxalyl)borate (LiBOB), additive FEC, and N-propyl-N-methylpyrrolidine nitrate were weighed and put into a glass bottle, and mixed evenly to obtain a first mixture. Then, 1 part by mass of room temperature initiator lithium hexafluorophosphate LIPF6 was added to the first mixture to form a precursor solution.
[0089] 2. Performance Test
[0090] 1) Uniformity test
[0091] Place the precursor solution in a glass bottle and observe the uniformity of the solution in the glass bottle; after standing for 48 hours, observe the uniformity of the solution in the glass bottle; continue to place it in an 80 degree Celsius oven for one hour and observe the solid electrolyte.
[0092] If the solid electrolyte is uniform and completely solidified, the precursor solution is determined to be uniformly solidified, which is Y; if the solid electrolyte is not completely solidified or there is stratification, the precursor solution is determined to be non-uniformly solidified, which is N.
[0093] 2) Yield test of solid-state batteries
[0094] The discharge capacity / cycle capacity retention rate of solid-state batteries was tested using a Xinwei electrochemical workstation. A discharge capacity higher than 0.23Ah was considered good, otherwise it was considered defective. Using the same batch of precursor solutions, 50 secondary batteries were prepared and their yield rate was measured. The yield rate is the number of good products / total number of samples.
[0095] III. Analysis of test results of various embodiments and comparative examples
[0096] The batteries of the embodiments and comparative examples were prepared according to the above method, and various performance parameters were measured. The results are shown in the table below.
[0097] Table 1
[0098]
[0099] The solid electrolytes after in-situ polymerization in Example 1, Comparative Example 1 and Comparative Example 2 are respectively Figure 1 As shown in (a), (b), and (c) in the figure, it can be seen that the solid electrolyte after in-situ polymerization in Example 1 presents a uniform latex state; while the solid electrolyte after in-situ polymerization in Comparative Example 1 presents an obvious solid-liquid separation phenomenon, and the solid electrolyte after in-situ polymerization in Comparative Example 2 presents a flocculent state due to insufficient polymerization degree.
[0100] From the comparison between the embodiment and the comparative example, it can be seen that by including both a room temperature initiator and a high temperature initiator in the solid electrolyte, the uniformity of the in-situ polymerization of the electrolyte can be improved, thereby increasing the yield rate of the solid-state battery.
[0101] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing a solid electrolyte by in-situ polymerization, characterized in that: include: Mixing raw materials including a room temperature initiator, a high temperature initiator, a cyclic monomer, and an electrolyte salt to form a precursor solution; After the precursor solution is allowed to stand at room temperature, it is thermally polymerized at high temperature to obtain the solid electrolyte; The standing time of the precursor solution at room temperature is 36-50 hours; the polymerization temperature of the thermal polymerization at high temperature is 30-100 degrees Celsius; The room temperature initiator includes one or more of lithium hexafluorophosphate, aluminum trifluoromethanesulfonate (Al(OTF)3), scandium trifluoromethanesulfonate (Sc(OTf)3), tin difluoride (SnF2), and copper trifluoromethanesulfonate (Cu(OTf)2); The high temperature initiator includes one or more of stannous octoate, lithium difluorooxalatoborate (LIDFOB), lithium borohydride (LiBH4), lithium aluminum hydride (LiAlH4, LAH), and lithium tri-tert-butoxyaluminum hydride (LiAlH[OC(CH3)3]3, LTBA); The cyclic monomer includes one or more of cyclic monoolefins, cyclic polyolefins, cycloalkanes, cyclic ethers, cyclic acetals, cyclic esters, cyclic amides, cyclosiloxanes, cyclic ketones, and cyclic thiols; The electrolyte salt includes one or more of lithium bis(trifluoromethane)sulfonyl imide (LITFSI), lithium bis(fluorosulfonyl)imide (LIFSI), lithium bis(oxalatoborate) (LIBOB), and lithium tetrafluoroborate (LIBF4).
2. The method according to claim 1, characterized in that The cyclic monomers include cyclic ethers.
3. The method according to claim 1, characterized in that The cyclic monomer includes one or more of 1,3,5-trioxane (TXE), 1,3-dioxane, 1,4-dioxane, and 1,3-dioxolane (DOL).
4. The method according to claim 1, characterized in that: The polymerization time of the thermal polymerization at high temperature is 0.5-1.5 hours.
5. The method according to claim 1, characterized in that The raw materials also include additives, which include one or more of lithium nitrate, imidazole ionic liquids, pyrrole ionic liquids, and fluorinated solvents.
6. The method according to claim 5, characterized in that The fluorinated solvent includes one or more of fluoroethylene carbonate, trifluoroethyl methyl carbonate (FEMC), bisfluoroethylene carbonate (DFEC), tris(2,2,2-trifluoroethyl) phosphate (TFEP), bis(2,2,2-trifluoroethyl) carbonate (TFEC), 2,2,2-trifluoroethyl ether (BTFE), ethyl trifluoroacetate (ETFA), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.
7. The method according to claim 1, characterized in that The raw materials including room temperature initiator, high temperature initiator, cyclic monomer and electrolyte salt are mixed to form a precursor solution, including: mixing a cyclic monomer, an electrolyte salt, and an additive to obtain a first mixture; mixing the first mixture with a high temperature initiator to obtain a second mixture; The second mixture is mixed with a room temperature initiator to obtain a precursor solution.
8. The method according to any one of claims 1 to 7, characterized in that The solid electrolyte satisfies at least one of the following conditions: (1) The mass ratio of the room temperature initiator to the high temperature initiator is 1:1-1:10; (2) The mass ratio of the high temperature initiator to the cyclic monomer is 1:100-10:100; (3) The mass ratio of the electrolyte salt to the cyclic monomer is 5:100-10:
100.
9. The method according to any one of claims 1 to 7, characterized in that The mass ratio of the additive to the cyclic monomer is 1:100-5:
100.
10. A solid electrolyte, characterized in that: The solid electrolyte is prepared by the method according to any one of claims 1 to 9.
11. A solid-state battery, characterized in that: The invention comprises the solid electrolyte according to claim 10 or the solid electrolyte prepared by the method according to any one of claims 1 to 9.
12. The solid-state battery according to claim 11, characterized in that: The solid-state battery includes a lithium metal anode.
13. A method for preparing a solid-state battery, characterized in that: include: Mixing raw materials including a room temperature initiator, a high temperature initiator, a cyclic monomer, and an electrolyte salt to form a precursor solution; injecting the precursor solution into the battery cell; After the battery is left standing at room temperature, it is thermally polymerized at high temperature to obtain the solid-state battery; The standing time of the precursor solution at room temperature is 36-50 hours; the polymerization temperature of the thermal polymerization at high temperature is 30-100 degrees Celsius; The room temperature initiator includes one or more of lithium hexafluorophosphate, aluminum trifluoromethanesulfonate (Al(OTF)3), scandium trifluoromethanesulfonate (Sc(OTf)3), tin difluoride (SnF2), and copper trifluoromethanesulfonate (Cu(OTf)2); The high temperature initiator includes one or more of stannous octoate, lithium difluorooxalatoborate (LIDFOB), lithium borohydride (LiBH4), lithium aluminum hydride (LiAlH4, LAH), and lithium tri-tert-butoxyaluminum hydride (LiAlH[OC(CH3)3]3, LTBA); The cyclic monomer includes one or more of cyclic monoolefins, cyclic polyolefins, cycloalkanes, cyclic ethers, cyclic acetals, cyclic esters, cyclic amides, cyclosiloxanes, cyclic ketones, and cyclic thiols; The electrolyte salt includes one or more of lithium bis(trifluoromethane)sulfonyl imide (LITFSI), lithium bis(fluorosulfonyl)imide (LIFSI), lithium bis(oxalatoborate) (LIBOB), and lithium tetrafluoroborate (LIBF4).
14. An electrical device, characterized in that: Including the solid-state battery according to claim 11 or 12 or a solid-state battery prepared by the preparation method according to claim 13.
Citation Information
Patent Citations
Gel polymer electrolyte for low-temperature operation, solid-state battery and preparation method of solid-state battery