A biomass-based-iron-based organic framework composite material and its preparation method and application

By preparing biomass-iron-based organic frame composites, the adsorption and removal ability of phosphate is enhanced by using the electrostatic attraction of biomass-based organic frames, the problems of loss and unstable adsorption amount of iron-based organic frames are solved, and high-efficiency phosphate is achieved Adsorption and low-cost wastewater treatment.

CN118236986BActive Publication Date: 2024-11-15JIANGSU PROVINCIAL ACAD OF ENVIRONMENTAL SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410321388.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-20
Publication Date
2024-11-15
Estimated Expiration
2044-03-20

AI Technical Summary

Technical Problem

The existing iron-based organic frameworks have a risk of loss in wastewater treatment, resulting in high operating costs and unstable adsorption volume, and lack of effective recycling methods.

Method used

Using the preparation method of biomass-iron organic frame composite, chitosan, iron-based organic frame MIL-88 (B) and crosslinking agent are mixed in acetic acid solution, and the reaction is carried out in a water bath heating and dropping into the mixed solution. , form a biomass-iron-based organic framework composite material, and use the electrostatic attraction action of biomass-based to enhance the adsorption and removal ability of phosphate.

Benefits of technology

The adsorption removal capacity of iron-based organic framework to phosphate is improved, the adsorption amount reaches 1.1 mmol/g, the loss amount is less than 1%. The adsorption efficiency is still higher than 80% after 6 adsorption-regeneration cycles, reducing the cost of wastewater treatment .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118236986B_ABST
    Figure CN118236986B_ABST
Patent Text Reader

Abstract

The present invention discloses a biomass-based iron-based organic framework composite material and its preparation method and application, which belongs to the technical field of environmental material preparation and application. The method comprises: adding chitosan, iron-based organic framework MIL-88 (B) and a cross-linking agent to an acetic acid solution, heating in a water bath after mixing evenly, and reacting to obtain a biomass-based iron-based organic framework composite material after dropping into the mixed solution. The phosphate adsorption amount of the biomass-based iron-based organic framework composite material prepared by the present invention can reach 1.1 mmol / g, which is higher than that of pure iron-based organic framework materials and single biomass-based materials. When the optimal adsorption pH condition is near, the loss of the iron-based organic framework material is less than 1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of environmental material preparation and application, and specifically relates to a biomass-based-iron-based organic framework composite material and a preparation method and application thereof. Background Art

[0002] Phosphorus is one of the main elements that cause eutrophication of water bodies. It can accelerate the growth of phytoplankton, leading to oxygen consumption and the death of fish and aquatic organisms. Electroplating is an essential basic industry for human industry and life, but due to the large amount of phosphorus-containing polluted wastewater discharged during the process, the electroplating industry has become one of the most dangerous chemical-intensive industries in the world. A variety of phosphorus-containing agents, such as phosphoric acid, chelating agents, reducing agents, etc., are used in the production process, which produces a large amount of phosphorus-containing wastewater.

[0003] There are mainly chemical and physical methods for treating inorganic phosphorus wastewater, including ion exchange, membrane separation, adsorption and other processes. The ion exchange method has insufficient selectivity for phosphorus and poor anti-interference in complex water environment conditions; the membrane separation method has high selectivity for pollutants, and the membrane components need to be replaced frequently; compared with the above methods, the adsorption method has lower preparation costs and requires fewer processes. It is suitable for enriching and recovering low-concentration phosphorus using solid functional groups, and has the advantages of simplicity, low cost, and low carbon.

[0004] Domestic and foreign literature studies have shown that iron-based organic frameworks are a new type of porous coordination polymer material assembled by coordination between iron and organic ligands. They have a unique structure, large specific surface area, uniform, controllable and diverse pore structure, and are widely used in the field of adsorption. They have shown strong ability to absorb phosphorus and resist interference. Despite their good performance in phosphorus absorption, the use of fine particles in wastewater treatment may lead to the loss of elements and poor recovery and reuse after treatment, resulting in higher operating costs. Therefore, it is very important to find a suitable matrix to retain the adsorbent to facilitate the recycling and recovery of discarded adsorbents.

[0005] Chinese patent number CN202210404779.8 discloses a preparation method and application of MIL-100 (Fe) / cellulose porous composite beads. The iron-based organic framework is added to the cellulose solution, stirred evenly, and then added to the metal ion solution for immersion to obtain a composite bead hydrogel, which has the advantages of good mechanical properties, high porosity, and high adsorption efficiency. However, the preparation process does not accurately control whether the iron-based organic framework has a leakage risk.

[0006] Through searching, no relevant patents and public documents have been found for achieving phosphate adsorption in the form of biomass-iron-based organic framework composite materials. Therefore, it is urgent to develop a method to effectively improve the loss of iron-based organic frameworks and ensure that the material after loading the iron-based organic framework maintains a high adsorption capacity during continuous operation, so as to meet actual application needs. Summary of the invention

[0007] In view of the above problems existing in the prior art, the technical problem to be solved by the present invention is to provide a method for preparing a biomass-based-iron-based organic framework composite material, which has the advantages of simple preparation process and easy industrial production. Another technical problem to be solved by the present invention is to provide a biomass-based-iron-based organic framework composite material prepared by the above method, wherein the rich functional groups in the biomass base have an electrostatic attraction effect on phosphates, thereby enhancing the adsorption and removal ability of the iron-based organic framework material for phosphates. Another technical problem to be solved by the present invention is to provide the use of the above-mentioned biomass-based-iron-based organic framework composite material as an adsorbent in the adsorption of phosphate pollutants in water bodies.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a biomass-based-iron-based organic framework composite material comprises the following steps: adding chitosan, an iron-based organic framework MIL-88(B) and a crosslinking agent into an acetic acid solution, mixing them evenly, heating them in a water bath, and dropping the mixed solution into the mixture to react and obtain the biomass-based-iron-based organic framework composite material.

[0010] Preferably, the g / g / mL ratio of chitosan, iron-based organic framework MIL-88 (B) and cross-linking agent is 0.6:1:0.154.

[0011] Preferably, the cross-linking agent is epichlorohydrin.

[0012] Preferably, the mixed solution is a mixed solution of sodium hydroxide, sodium sulfate, anhydrous ethanol and water, wherein the g / g / mL / mL of sodium hydroxide, sodium sulfate, anhydrous ethanol and water is 16:12:2:300.

[0013] The method for preparing the biomass-based-iron-based organic framework composite material specifically comprises the following steps:

[0014] 1) Chitosan, iron-based organic framework MIL-88(B) and cross-linking agent were weighed separately and added into acetic acid solution, mixed evenly and heated in a water bath at 60°C for cross-linking for 2 h to obtain a mixed material;

[0015] 2) dropping a mixed solution containing sodium hydroxide, sodium sulfate, anhydrous ethanol and water into the mixed material obtained in step 1) to obtain hydrogel beads;

[0016] 3) placing the obtained hydrogel beads into a diluted cross-linking agent to enhance the mechanical strength, washing and drying at room temperature to obtain a biomass-based-iron-based organic framework composite material.

[0017] The method for preparing the biomass-based-iron-based organic framework composite material prepares the biomass-based-iron-based organic framework composite material.

[0018] The biomass-based-iron-based organic framework composite material is used as an adsorbent in the adsorption of phosphate pollutants in water bodies.

[0019] The application described above comprises the following steps of adsorption: adding the biomass-based iron-based organic framework composite material into a phosphate-containing water body, and performing oscillation adsorption at room temperature to adsorb the phosphate.

[0020] In the application described, the phosphate adsorption time is 24 hours, and the concentration of adsorbable phosphate is: 0.2~1.0 mg / L.

[0021] In the application, the adsorbed biomass-based-iron-based organic framework composite material is fully shaken and eluted in 100 mL of a mixed solution at 150 r / min for 12 h, and then adsorbed again; wherein the mixed solution is a mixed solution of 0.1 mol / L sodium hydroxide and 5 mol / L sodium nitrate.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The present invention uses the abundant functional groups in the biomass base to have an electrostatic attraction effect on phosphate, and in practical applications, the adsorption and removal ability of the iron-based organic framework material for phosphate is enhanced;

[0024] (2) The phosphate adsorption capacity of the biomass-based-iron-based organic framework composite material prepared by the present invention can reach 1.1 mmol / g, which is higher than that of pure iron-based organic framework materials and single biomass-based materials. When the optimal adsorption pH condition is near, the loss of the iron-based organic framework material is less than 1%;

[0025] (3) The regeneration method of the biomass-based-iron-based organic framework composite material of the present invention is simple and easy to implement, which saves the cost of wastewater treatment. After 6 adsorption-regeneration cycles, the adsorption efficiency can still be higher than 80%, and the regeneration efficiency is stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 SEM images of MIL-88(B), chitosan, and MIL-88(B) / chitosan; (a) and (d) are MIL-88(B) at 10.0 μm and 1.00 μm, respectively; (b) and (e) are chitosan at 500 μm and 5.00 μm, respectively; (c) and (f) are MIL-88(B) / chitosan at 500 μm and 5.00 μm, respectively;

[0027] Figure 2FTIR images of MIL-88(B), chitosan, and MIL-88(B) / chitosan;

[0028] Figure 3 XRD patterns of MIL-88(B), chitosan, and MIL-88(B) / chitosan;

[0029] Figure 4 The figure shows the removal effect of MIL-88(B), chitosan, and MIL-88(B) / chitosan on phosphates of different concentrations;

[0030] Figure 5 Phosphate adsorption performance and Fe-based organic framework loss graphs under different pH conditions for MIL-88(B), chitosan, and MIL-88(B) / chitosan;

[0031] Figure 6 This is the effect diagram of MIL-88(B) / chitosan cyclic adsorption-desorption of a certain electroplating tail water with an initial phosphate concentration of 0.85 mg / L;

[0032] Figure 7 This is a diagram showing the adsorption effect of phosphate on MIL-88(B), chitosan, and MIL-88(B) / chitosan hydrogel at different adsorption times. DETAILED DESCRIPTION

[0033] The present invention will be further illustrated below in conjunction with specific examples. The examples are implemented under the premise of the technical solution of the present invention. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. In the following examples, unless otherwise specified, the technical means used are conventional means well known to those skilled in the art. In the examples, those without specifying specific conditions are carried out according to conventional conditions or the conditions recommended by the manufacturer. Those without specifying the manufacturer for reagents used or instruments are conventional products that can be obtained by commercial purchase.

[0034] The performance testing method adopted by the present invention is as follows:

[0035] 1. The test method for the adsorption and desorption performance of phosphate is: ammonium molybdate spectrophotometry (GB / T 11893-1989).

[0036] 2. The test method for the loss of iron-based organic framework is: flame atomic absorption spectrophotometry (GB / T 11911-1989).

[0037] Example 1

[0038] 1 g of powdered MIL-88(B), 0.6 g of chitosan and 0.154 mL of epichlorohydrin were respectively added to 20 mL of 2% (V / V) acetic acid solution and cross-linked at 60°C for 2 h. A 300 mL mixed solution containing 16 g of sodium hydroxide, 12 g of sodium sulfate and 2 mL of anhydrous ethanol was added dropwise with a syringe to fully cross-link to form hydrogel beads. The beads were cross-linked in 100 mL of distilled water containing 0.5 mL of epichlorohydrin for 2 h to enhance the mechanical strength. After washing and drying at room temperature, 6 g of MIL-88(B) / chitosan hydrogel was obtained, i.e., a biomass-based-iron-based organic framework composite material.

[0039] Depend on Figure 1 and Figure 3 From the SEM and XRD images, it can be seen that there are many large pores on the surface of the MIL-88(B) / chitosan hydrogel prepared by the present invention. By further magnification, it can be found that these pores carry many small pores. MIL-88(B) maintains the same size and orderly shape. The appearance of iron element indicates the introduction of MIL-88(B), and the increase of N element indicates the appearance of chitosan. Figure 2 From the FTIR graph, we can see that 1650 cm -1 There is a peak at 3354 cm -1 The strong peaks nearby are related to the extended vibration of NH, which can be attributed to the protonated amino group.

[0040] Comparative Example 1

[0041] 4.32 g of ferric chloride hexahydrate and 2.66 g of terephthalic acid were added to 100 mL of N,N-dimethylformamide and completely dissolved. The mixture was kept at 150°C in an autoclave for 12 h, washed alternately with deionized water and methanol several times, and dried to obtain 2.51 g of pure iron-based organic framework material MIL-88(B).

[0042] Comparative Example 2

[0043] 0.6 g chitosan and 0.154 mL epichlorohydrin were respectively added to 20 mL of 2% (V / V) acetic acid solution, cross-linked at 60°C for 2 h, and 300 mL of a mixed solution containing 16 g sodium hydroxide, 12 g sodium sulfate, and 2 mL anhydrous ethanol was dropped into it with a syringe to fully cross-link and form hydrogel beads. The beads were cross-linked in 100 mL distilled water containing 0.5 mL epichlorohydrin for 2 h to enhance the mechanical strength. After washing, the beads were dried at room temperature to obtain 5.0 g of single biomass-based material chitosan.

[0044] Example 2

[0045] The MIL-88(B) / chitosan hydrogel prepared in Example 1, the MIL-88(B) prepared in Comparative Example 1, and the chitosan prepared in Comparative Example 2 were tested for their phosphate adsorption performance.

[0046] 50 mL of sodium dihydrogen phosphate solution with concentrations of 0.5, 1, 2, 4 and 8 mmol / L were prepared respectively, and the pH value was adjusted to 7.0. 0.5 g of the adsorbent to be tested was added, and the mixture was shaken at room temperature 25°C for 24 h. The phosphate concentration of the solution was determined by ammonium molybdate spectrophotometry (GB / T11893-1989). The results are shown in Table 1.

[0047] Table 1 Maximum adsorption of MIL-88(B), chitosan, and MIL-88(B) / chitosan

[0048]

[0049] As shown in Table 1, the maximum adsorption capacity of MIL-88(B) / chitosan at room temperature is 1.10 mmol / g, which is better than that of pure iron-based organic framework material MIL-88(B) and single biomass-based material chitosan.

[0050] like Figure 4 As shown, the adsorption process of phosphate by MIL-88(B) / chitosan hydrogel is more consistent with the Friedrich isotherm than the Langmuir isotherm, which indicates that MIL-88(B) / chitosan undergoes multilayer adsorption on the heterogeneous surface to remove phosphate.

[0051] Example 3

[0052] The MIL-88(B) / chitosan hydrogel prepared in Example 1, the MIL-88(B) prepared in Comparative Example 1, and the chitosan prepared in Comparative Example 2 were tested for their phosphate adsorption properties under different pH conditions.

[0053] 50 mL of sodium dihydrogen phosphate solution with a concentration of 1 mmol / L was prepared, and the pH value of the solution was adjusted to 4.0, 5.0, 6.0, 7.0, 8.0, 9.0 and 10.0 with sodium hydroxide and hydrochloric acid, respectively. 0.5 g of MIL-88(B) / chitosan hydrogel prepared in Example 1 was added, and the mixture was shaken at room temperature for 24 h. The phosphate concentration of the solution was determined by ammonium molybdate spectrophotometry (GB / T 11893-1989). The results are shown in FIG. Figure 5 As shown, the phosphate adsorption efficiency of MIL-88(B) / chitosan is over 80% at pH 4-8, the suitable pH range is 6-8, and the adsorption amount is the largest at pH 7, indicating that MIL-88(B) / chitosan can adapt to a wider range of acid and base conditions.

[0054] The MIL-88(B) / chitosan hydrogel prepared in Example 1 was tested for the loss of the iron-based organic framework. 1 mmol / L sodium dihydrogen phosphate solution with pH values ​​of 4, 5, 6, 7, 8, 9, and 10 was prepared, 0.5 g of the MIL-88(B) / chitosan hydrogel prepared in Example 1 was added, and the mixture was shaken at room temperature for 24 h. The iron ion concentration of the solution was determined by flame atomic absorption spectrophotometry (GB / T11911-1989). The results are shown in Table 1. Figure 5 As shown, the iron loss is always less than 1%, and the loss near the optimal pH 6-8 is less than 0.2%, proving that biomass is beneficial to reducing the loss and leakage of iron-based organic framework materials.

[0055] Example 4

[0056] The MIL-88(B) / chitosan hydrogel prepared in Example 1 adsorbed electroplating tail water with an initial phosphate concentration of 0.85 mg / L, and then desorbed and circulated.

[0057] Add 0.5 g of the MIL-88(B) / chitosan hydrogel prepared in Example 1 to 50 mL of wastewater and shake at room temperature for 24 h; prepare 100 mL of a mixed solution of 5 mol / L sodium nitrate and 0.1 mol / L sodium hydroxide as an eluent, add 0.5 g of the MIL-88(B) / chitosan hydrogel beads that have adsorbed phosphate, and shake at room temperature for 12 h to obtain the desorbed MIL-88(B) / chitosan hydrogel. The operation was repeated 6 times, and the phosphate concentrations in the effluent and the eluent were determined by ammonium molybdate spectrophotometry (GB / T 11893-1989). The results are shown in Figure 2. Figure 6 As shown in Table 2, after 6 cycles, the phosphate concentration in the electroplating tail water was always lower than 0.2 mg / L, the adsorption efficiency was stably higher than 80%, and the recovery and regeneration efficiency was not less than 97%, which proved that the desorption method was stable and efficient.

[0058] Table 2 Adsorption and desorption efficiency of MIL-88(B) / chitosan cyclic adsorption-desorption of electroplating tail water with an initial phosphate concentration of 0.85 mg / L

[0059]

[0060] Example 5

[0061] The MIL-88(B) / chitosan hydrogel prepared in Example 1, the MIL-88(B) prepared in Comparative Example 1, and the chitosan prepared in Comparative Example 2 were tested for the adsorption effect of phosphate at different adsorption times.

[0062] Prepare 200 mL of 1 mmol / L sodium dihydrogen phosphate solution, adjust the pH value to 7.0, add 0.5 g of the adsorbent to be tested, take samples at 0, 15, 30, 60, 90, 120, 180, 240, 360 and 1440 min, and determine the phosphate concentration of the solution using the ammonium molybdate spectrophotometry method (GB / T 11893-1989). The results are as follows: Figure 7 As shown, the pseudo-second-order kinetic model is more suitable for the process of phosphate adsorption by the MIL-88(B) / chitosan hydrogel prepared by the present invention than the pseudo-first-order kinetic model. The MIL-88(B) / chitosan hydrogel prepared by the present invention inherits the high efficiency of phosphate adsorption by the single iron-based organic framework MIL-88(B). More than 90% of the phosphate in the solution is adsorbed in only 180 minutes, and its adsorption efficiency is not greatly affected by the low phosphate adsorption rate of the single biomass-based chitosan, which proves that MIL-88(B) / chitosan has a faster phosphate adsorption speed and higher adsorption efficiency.

[0063] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A biomass-based iron-based organic framework composite material is used as an adsorbent in the adsorption of phosphate pollutants in water, characterized in that: The method for preparing the biomass-based-iron-based organic framework composite material specifically comprises the following steps: 1) Chitosan, iron-based organic framework MIL-88(B) and cross-linking agent were weighed separately and added into acetic acid solution, mixed evenly and heated in a water bath at 60°C for cross-linking for 2 h to obtain a mixed material; 2) dropping a mixed solution containing sodium hydroxide, sodium sulfate, anhydrous ethanol and water into the mixed material obtained in step 1) to obtain hydrogel beads; 3) placing the obtained hydrogel beads into a diluted cross-linking agent to enhance the mechanical strength, washing and drying at room temperature to obtain a biomass-based-iron-based organic framework composite material; In the step 1), the g / g / mL ratio of chitosan, iron-based organic framework MIL-88 (B) and cross-linking agent is 0.6:1:0.154; The cross-linking agents are all epichlorohydrin; In the mixed solution, the g / g / mL / mL ratio of sodium hydroxide, sodium sulfate, anhydrous ethanol and water is 16:12:2:

300.

2. The use according to claim 1, characterized in that: The adsorption process is: adding the biomass-based-iron-based organic framework composite material into the phosphate-containing water body and oscillating and adsorbing at room temperature.

3. The use according to claim 2, characterized in that: The adsorption time of phosphate is 24 h; the concentration of phosphate in phosphate-containing water is: 0.2~1.0 mg / L.

4. The use according to claim 3, characterized in that: The adsorbed biomass-based-iron-based organic framework composite material was fully shaken and eluted in 100 mL of mixed solution at 150 r / min for 12 h, and then adsorbed again; wherein the mixed solution was a mixed solution of 0.1 mol / L sodium hydroxide and 5 mol / L sodium nitrate.