A production process for hot-rolled round steel for hydraulic support

By carrying out water cooling and fine heating before the final rolling in the production process of hot-rolled round steel for hydraulic supports, the problems of excessive use of micro-alloying elements in non-quenched and tempered steel and poor controlled rolling and cooling effects are solved, achieving It improves the uniform mechanical properties and high strength and toughness of large-size round steel and reduces production costs.

CN118237397BActive Publication Date: 2024-09-24JIANGSU LIANFENG ENERGY EQUIP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410659919.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-09-24
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

The existing non-quenched and tempered steel requires a large amount of micro-alloying elements during the production process, and the cost reduction is limited. At the same time, the controlled rolling and controlled cooling process has limited effect on improving the core of large-size round steel.

Method used

Using a production process that includes rolling and cooling steps, through water cooling before the final rolling, the surface temperature of the round steel drops sharply, and internal two-phase zone rolling is achieved during the last rolling, combining multiple stages Through water cooling and fine heating procedures, the steel temperature and rolling speed are controlled to avoid the use of micro-alloying elements.

Benefits of technology

It achieves uniform distribution of internal and external mechanical properties of large-size round steel, reduces production costs, improves the strength and toughness ratio of round steel by refining the grain size, and improves the nucleation effect of the internal structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118237397B
    Figure CN118237397B
Patent Text Reader

Abstract

The invention relates to the field of metallurgical technology, and in particular to a production process for hot-rolled round steel for hydraulic supports. The production process comprises a rolling step and a cooling step. In the rolling step, the round steel is rolled by at least 6 rolling mills arranged alternately. The cooling step comprises at least one water-penetrating cooling of the round steel before the last rolling, so that the surface temperature of the round steel before entering the last rolling is 600-700°C. When the round steel passes through the last rolling, a part of the inner area is rolled in a two-phase region, and at least three water-penetrating cooling is further comprised after rolling. The production process for hot-rolled round steel for hydraulic supports provided by the invention realizes uniform distribution of internal and external mechanical properties of large-size round steels without adding microalloy precipitation strengthening elements through a controlled rolling and controlled cooling process, thereby reducing the production cost of the hot-rolled round steels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a production process for hot-rolled round steel for hydraulic supports. Background Art

[0002] The common steel grade used in mine hydraulic supports is 27SiMn. The traditional manufacturing process performs overall quenching and tempering treatment on round steel to make it have a higher strength and toughness match. The traditional quenching and tempering process is not only costly and inefficient, but also causes huge pollution to the environment. At present, the replacement of non-quenched and tempered steel is the development direction of the machinery industry. However, general non-quenched and tempered steel often uses precipitation strengthening phase to achieve high strength and toughness of steel. The application of a large number of micro-alloying elements is inevitable, and the cost reduction is limited; the Chinese patent with application number CN202010795993.1 proposes a fine-grained high-carbon steel and its rolling production method. The patent proposes a method of controlling the heating temperature, deformation degree and cold cutting speed, that is, controlling rolling and cooling to achieve the effect of grain refinement. However, the final rolling temperature in the patent is above 800°C, and the final rolling temperature in the industry is also controlled above 800°C, which has limited improvement effect on the core of large-sized round steel. Summary of the invention

[0003] In view of this, the purpose of the present invention is to propose a production process for hot-rolled round steel for hydraulic supports, so as to solve the problems that the existing non-quenched and tempered steel requires a large amount of micro-alloying elements, the cost reduction is limited, and the existing controlled rolling and controlled cooling method has limited improvement effect on the core of the round steel.

[0004] Based on the above purpose, the present invention proposes a production process for hot-rolled round steel for hydraulic support, the composition and mass percentage of the hot-rolled round steel are: C: 0.28-0.30%, Si: 1.27-1.35%, Mn: 1.25-1.36%, P ≤0.015%, S: 0-0.005%, Cr: 0.15-0.2%, H: ≤1.5ppm, O: ≤40ppm, N: ≤100ppm, and the balance is Fe and unavoidable impurities;

[0005] The production process includes a rolling step and a cooling step. In the rolling step, the round steel is rolled by at least 6 rolling mills arranged alternately. The cooling step includes at least one water-penetrating cooling of the round steel before the last rolling. After the water-penetrating cooling, the surface temperature of the round steel drops sharply, so that the surface temperature of the round steel before entering the last rolling is 600-700°C. When the round steel passes through the last rolling, part of the internal area is rolled in the two-phase region, so that the core of the round steel is fully deformed. It also includes at least three water-penetrating cooling after rolling.

[0006] Optionally, in the cooling step, the round steel is subjected to strong cooling in a water cooling before the final rolling, and the round steel after rolling is subjected to four stages of alternating strong and weak water cooling.

[0007] Optionally, in the rolling step, the temperature of the steel entering the rolling step is controlled to be 810-850° C., and the rolling speed is controlled to be ≤0.5 m / s.

[0008] Optionally, a heating step is further included before the rolling step, in which the preheating section temperature is <900°C, the target temperature is 860°C, and the time is >1.0h; the heating section I temperature is 900-1100°C, the target temperature is 1000°C, and the time is ≥1.0h; the heating section II temperature is 1180-1260°C, the target temperature is 1230°C, and the time is ≥2h; the soaking section temperature is 1200-1260°C, the target temperature is 1240°C, the time is ≥3h, and the total heating time is ≥6.0h.

[0009] Optionally, the method further includes a smelting step before the heating step, wherein the smelting step includes electric furnace smelting, LF refining, and VD vacuum treatment, and a continuous casting step is also included after the smelting step.

[0010] Optionally, in the LF refining step, the white slag making time is ≥20 min, and the smelting time is ≥35 min; and the auxiliary material used is 100-140 kg of silicon carbide.

[0011] Optionally, in the VD vacuum treatment step, the VD high vacuum degree is ≤67Pa, the high vacuum holding time is ≥10min, and the soft blowing time is ≥15min; wire feeding is performed after the vacuum is completed, and the wire feeding sequence is: aluminum wire-calcium silicon wire; the length of the calcium silicon wire is 55-90m.

[0012] Optionally, in the continuous casting step, electromagnetic stirring is used, and the position and parameters of the electromagnetic stirring are: crystallizer electromagnetic stirring: 260A / 2Hz, casting strand electromagnetic stirring: 150A / 8Hz, end electromagnetic stirring: 1200A / 8Hz, and the continuous casting pulling speed is 0.39m / min.

[0013] Beneficial effects of the present invention: The production process for hot-rolled round steel of hydraulic supports provided by the present invention allows the round steel to pass through a water cooling process before the final rolling, so that the surface temperature of the round steel drops sharply, so that the internal part of the round steel is rolled in the two-phase region during the final rolling process, and the surface temperature of the round steel is reduced. During the final rolling process, the core of the round steel can be fully deformed to store high deformation energy. In the subsequent water cooling process, high supercooling and high deformation energy conditions are created to promote nucleation, further refine the internal structure of the round steel, and make the internal part of the round steel have a better strength and toughness ratio.

[0014] The production process for hot-rolled round steel of hydraulic supports provided by the present invention realizes uniform distribution of internal and external mechanical properties of large-sized round steel without adding micro-alloy precipitation strengthening elements through controlled rolling and controlled cooling processes, thereby reducing the production cost of hot-rolled round steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 A picture showing the grain size of hot-rolled round steel for hydraulic support produced by the production process of the present invention;

[0017] Figure 2 A picture showing the grain size of the subcutaneous 1 / 3R of the hot-rolled round steel for hydraulic support produced by the production process of the present invention;

[0018] Figure 3 A picture showing the grain size of the subcutaneous 1 / 2R of the hot-rolled round steel for hydraulic support produced by the production process of the present invention;

[0019] Figure 4 A picture showing the grain size of the center of the hot-rolled round steel used for hydraulic support produced by the production process of the present invention;

[0020] Figure 5 This is a picture showing the grain size under the skin of round steel produced in the comparative example;

[0021] Figure 6 This is a picture showing the grain size of the round steel produced in the comparative example at 1 / 3R below the skin;

[0022] Figure 7 This is a picture showing the grain size of the 1 / 2R subcutaneous round steel produced in the comparative example;

[0023] Figure 8 This is a picture showing the grain size at the center of the round steel produced as a comparative example. DETAILED DESCRIPTION

[0024] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. Example 1

[0025] A production process for hot-rolled round steel for hydraulic supports, comprising the following steps:

[0026] Smelting steps: smelting in electric furnace, then refining in LF refining furnace, and then VD vacuum treatment. The process requirements of LF refining stage are: adding 600kg lime to make white slag, and adding 200kg cleaning agent, white slag making time 22min, smelting time 37min, auxiliary material dosage: silicon carbide 100kg. Control target carbon content 0.16% ≥ C ≥ 0.06%, end point temperature ≥ 1610℃;

[0027] The process requirements of VD vacuum treatment are: VD high vacuum degree 65Pa, high vacuum holding time 13min, soft blowing time 15min; after the vacuum is finished, wire feeding is carried out, and the wire feeding sequence is: aluminum wire-silicon calcium wire; the length of the silicon calcium wire is 55m;

[0028] Continuous casting steps: During the cooling stage, the first cooling water is water pipe cooling with a water flow rate of 4500L / min, and the second cooling water is water mist cooling, with 25L / min in one zone and 48L / min in the second zone; during the crystallization and solidification stage, electromagnetic stirring is adopted, and the position and parameters of electromagnetic stirring are: crystallizer electromagnetic stirring: 260A / 2Hz, casting strand electromagnetic stirring: 150A / 8Hz, end electromagnetic stirring: 1200A / 8Hz, and the continuous casting pulling speed is 0.39m / min.

[0029] Heating steps: the continuous casting billet is heated in four stages, the preheating stage temperature is 890°C, the time is 1.5h; the heating stage I temperature is 920°C, the time is 1.5h; the heating stage II temperature is 1250°C, the time is 3h, and the soaking stage temperature is 1260°C, the time is 3h;

[0030] Rolling step: the heated continuous casting billet is passed through the billet opening machine to obtain an intermediate billet with a specification of 305mm×315mm. The intermediate billet is hydraulically sheared at the head and tail, and the continuous rolling temperature is controlled to 840℃ through the cooling control equipment. It is rolled through 6 interactively arranged rolling mills to obtain φ160mm round steel. The specific layout of the 6 interactively arranged rolling mills is: horizontal rolling mill-vertical rolling mill-horizontal rolling mill-vertical rolling mill-horizontal rolling mill-horizontal rolling mill, and the rolling speed is 0.5m / s. A section of water cooling is set before the last rolling. After the water cooling, the temperature of the round steel is 680℃. The cooled round steel is rolled by the last horizontal rolling mill. After the last rolling, 4 sections of water cooling are set. After 4 sections of water cooling, the surface temperature of the round steel is 600℃. The water flow parameters of the 5 sections of water cooling are shown in Table 1.

[0031] Table 1

[0032]

[0033] Round steel cooling: The round steel is collected on the cooling bed for air cooling and finally pit cooling;

[0034] Preparation of round steel finished products: straighten the cooled round steel, then perform stress relief annealing, and obtain the finished round steel products after finishing. Perform flaw detection on the finished round steel products, and the qualified finished round steel products will be put into storage. Example 2

[0035] A production process for hot-rolled round steel for hydraulic supports, comprising the following steps:

[0036] Smelting steps: smelting in electric furnace, then refining in LF refining furnace, and then VD vacuum treatment. The process requirements of LF refining stage are: adding 600kg lime to make white slag, and adding 200kg cleaning agent, white slag making time 25min, smelting time 40min, auxiliary material dosage: silicon carbide 100kg. Control target carbon content 0.16% ≥ C ≥ 0.06%, end point temperature ≥ 1610℃;

[0037] The process requirements of VD vacuum treatment are: VD high vacuum degree 65Pa, high vacuum holding time 13min, soft blowing time 15min; after the vacuum is finished, wire feeding is carried out, and the wire feeding sequence is: aluminum wire-silicon calcium wire; the length of the silicon calcium wire is 55m;

[0038] Continuous casting steps: During the cooling stage, the first cooling water is water pipe cooling with a water flow rate of 4500L / min, and the second cooling water is water mist cooling, with 25L / min in one zone and 48L / min in the second zone; during the crystallization and solidification stage, electromagnetic stirring is adopted, and the position and parameters of electromagnetic stirring are: crystallizer electromagnetic stirring: 260A / 2Hz, casting strand electromagnetic stirring: 150A / 8Hz, end electromagnetic stirring: 1200A / 8Hz, and the continuous casting pulling speed is 0.39m / min.

[0039] Heating steps: the continuous casting billet is heated in four stages, the preheating stage temperature is 880°C, the time is 2h; the heating stage I temperature is 1060°C, the time is 1.5h; the heating stage II temperature is 1200°C, the time is 3h, and the soaking stage temperature is 1260°C, the time is 3h;

[0040] Rolling steps: After the heated continuous casting billet is passed through the billet opening machine, an intermediate billet with a specification of 305mm×315mm is obtained. The intermediate billet is hydraulically sheared at the head and tail, and the continuous rolling temperature is controlled to 810℃ through the cooling control equipment. It is rolled through 6 interactively arranged rolling mills to obtain φ160mm round steel. The specific layout of the 6 interactively arranged rolling mills is: horizontal rolling mill-vertical rolling mill-horizontal rolling mill-vertical rolling mill-horizontal rolling mill-horizontal rolling mill, and the rolling speed is 0.5m / s. A section of water cooling is set before the last rolling. After the water cooling, the temperature of the round steel is 620℃. The cooled round steel is rolled by the last horizontal rolling mill. After the last rolling, 4 sections of water cooling are set. After 4 sections of water cooling, the surface temperature of the round steel is 580℃. The water flow parameters of the 5 sections of water cooling are shown in Table 2.

[0041] Table 2

[0042]

[0043] Round steel cooling: The round steel is collected on the cooling bed for air cooling and finally pit cooling;

[0044] Preparation of round steel finished products: straighten the cooled round steel, then perform stress relief annealing, and obtain the finished round steel products after finishing. Perform flaw detection on the finished round steel products, and the qualified finished round steel products will be put into storage. Example 3

[0045] A hot-rolled round steel for a hydraulic support, whose composition and mass percentage are: C: 0.28%, Si: 1.33%, Mn: 1.36%, P: 0.013%, S: 0.003%, Cr: 0.17%, H: 1.0ppm, O: 20ppm, N: 50ppm, and the rest are Fe and unavoidable impurities. Example 4

[0046] A hot-rolled round steel for a hydraulic support, whose composition and mass percentage are: C: 0.29%, Si: 1.33%, Mn: 1.31%, P: 0.010%, S: 0.001%, Cr: 0.166%, H: 1.1ppm, O: 12ppm, N: 40ppm, and the rest are Fe and unavoidable impurities. Example 5

[0047] A hot-rolled round steel for a hydraulic support, whose composition and mass percentage are: C: 0.288%, Si: 1.33%, Mn: 1.33%, P: 0.008%, S: 0.002%, Cr: 0.17%, H: 1.1ppm, O: 10ppm, N: 31ppm, and the rest are Fe and unavoidable impurities.

[0048] Comparative Example

[0049] A 27SiMn heat treatment process comprises the following steps:

[0050] Round steel heating: Place the round steel in a heating furnace and heat it to 950°C for 1.5 hours;

[0051] Insulation: Keep the heated 27SiMn round steel at high temperature for a period of time to make its internal structure undergo phase change. The insulation time is generally 1 hour;

[0052] Cooling: Take the 27SiMn round steel out from the high temperature and cool it quickly by water quenching.

[0053] The mechanical properties of the round steel produced by the production process proposed by the present invention and the round steel produced by the production process in the comparative example were tested, as shown in Table 3:

[0054] Table 3 Mechanical properties test results of the present invention and comparative examples

[0055]

[0056] The test data of the above mechanical properties are measured using the standards and methods of GB / T228.1-2010 "Tensile test for metallic materials" and GB / T229-2010 "Charpy pendulum impact test method for metallic materials".

[0057] It can be seen from the above table that the round steel produced by the production process proposed by the present invention has higher strength and better toughness;

[0058] The metallographic structures of the round steel produced by the production process proposed by the present invention and the round steel produced by the comparative example are tested, and the subcutaneous, subcutaneous 1 / 3R, subcutaneous 1 / 2R and central positions of the two are tested respectively. Figure 1-Figure 4 is the test result of the round steel produced by the production process proposed by the present invention, Figure 5-Figure 8 The comparison results of the grain size in Table 4 are obtained for the comparative example. The grain size is determined according to GB / T6394-2017 "Method for Determination of Average Grain Size of Metals"

[0059] Table 4 Grain size test results of the present invention and comparative examples

[0060]

[0061] By comparison, it can be seen that the grain size of the round steel produced by the production process proposed by the present invention is finer.

[0062] It should be understood by those skilled in the art that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the above aspects of the present invention, which are not provided in detail for the sake of simplicity.

[0063] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A production process for hot-rolled round steel for hydraulic supports, characterized in that: The composition and mass percentage of the hot-rolled round steel are: C: 0.28-0.30%, Si: 1.27-1.35%, Mn: 1.25-1.36%, P ≤0.015%, S: 0-0.005%, Cr: 0.15-0.2%, H: ≤1.5ppm, O: ≤40ppm, N: ≤100ppm, and the balance is Fe and unavoidable impurities; The production process includes a rolling step and a cooling step. In the rolling step, the round steel is rolled by at least 6 rolling mills arranged alternately. The cooling step includes at least one water-penetrating cooling of the round steel before the last rolling. After the water-penetrating cooling, the surface temperature of the round steel drops sharply, so that the surface temperature of the round steel before entering the last rolling is 600-700°C. When the round steel passes through the last rolling, a part of the internal area is rolled in the two-phase region, so that the core of the round steel is fully deformed. It also includes at least three water-penetrating cooling after rolling.

2. The production process for hot-rolled round steel for hydraulic support according to claim 1 is characterized in that: In the cooling step, the round steel is subjected to strong cooling in the water cooling before the last rolling, and the round steel after rolling is subjected to four stages of alternating strong and weak water cooling.

3. The production process for hot-rolled round steel for hydraulic support according to claim 1 is characterized in that: In the rolling step, the temperature of the steel entering the rolling step is controlled to be 810-850° C., and the rolling speed is controlled to be ≤0.5 m / s.

4. The production process for hot-rolled round steel for hydraulic support according to claim 1 is characterized in that: It also includes a heating step before the rolling step, in which the preheating section temperature is <900°C, the target temperature is 860°C, and the time is >1.0h; the heating section I temperature is 900-1100°C, the target temperature is 1000°C, and the time is ≥1.0h; the heating section II temperature is 1180-1260°C, the target temperature is 1230°C, and the time is ≥2h; the soaking section temperature is 1200-1260°C, the target temperature is 1240°C, the time is ≥3h, and the total heating time is ≥6.0h.

5. The production process for hot-rolled round steel for hydraulic support according to claim 4 is characterized in that: It also includes a smelting step before the heating step, wherein the smelting step includes electric furnace smelting, LF refining, and VD vacuum treatment, and a continuous casting step is also included after the smelting step.

6. The production process for hot-rolled round steel for hydraulic support according to claim 5, characterized in that: In the LF refining step, the white slag making time is ≥20 min, and the smelting time is ≥35 min; and the auxiliary material used is 100-140 kg of silicon carbide.

7. The production process for hot-rolled round steel for hydraulic support according to claim 5, characterized in that: In the VD vacuum treatment step, the VD high vacuum degree is ≤67Pa, the high vacuum holding time is ≥10min, and the soft blowing time is ≥15min; after the vacuum is finished, wire feeding is performed, and the wire feeding sequence is: aluminum wire-silicon calcium wire; wherein the length of the silicon calcium wire is 55-90m.

8. The production process for hot-rolled round steel for hydraulic support according to claim 5, characterized in that: In the continuous casting step, electromagnetic stirring is used during the crystallization and solidification stages. The position and parameters of the electromagnetic stirring are: crystallizer electromagnetic stirring: 260A / 2Hz, casting strand electromagnetic stirring: 150A / 8Hz, end electromagnetic stirring: 1200A / 8Hz, and the continuous casting pulling speed is 0.39m / min.

Citation Information

Patent Citations

  • Fine-grain high-carbon steel and rolling production method thereof

    CN112080687A

  • Production process for non-quenched and tempered steel

    CN104043660A

  • Steel wire rod for high-strength boron-contained and annealing-free fastening piece and preparation method thereof

    CN105543678A

  • Preparation method of hot-rolled steel coil rod for 10.9-level high-strength bolt

    CN106929623A

  • Preparation method of ultra-fine-grain anti-seismic steel bar

    CN111004979A