A high performance coal gangue lightweight aggregate concrete and preparation method thereof
By adding filler whiskers and alkali slag to light aggregate concrete, the tricalcium aluminate mono ore is preferred to generate minerals such as ettringite, the quality loss problem of light aggregate concrete under freeze-thaw cycle conditions is solved, and the resistance of light aggregate concrete is improved Freeze-thawing and mechanical properties, suitable for high-rise buildings.
Patent Information
- Application Number
- CN202410314966.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-03-19
AI Technical Summary
Existing light aggregate concrete is prone to mass loss under freeze-thaw cycle conditions, resulting in poor structural performance, limiting its promotion and application.
Using high-performance coal gangue light aggregate concrete formula, add filler whiskers and alkali slag, and prefer tricalcium aluminate single ore to generate minerals such as ettringite through moisture storage and reaction, enhancing the skeleton support of concrete and anti-freeze-thawing performance.
It effectively reduces the shrinkage of concrete and improves the resistance to freeze-thaw, delays the drop in humidity, and enhances the mechanical properties of concrete. It is suitable for high-rise and large-span buildings.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of concrete, and more specifically, to a high-performance coal gangue lightweight aggregate concrete and a preparation method thereof. Background Art
[0002] Lightweight aggregate concrete refers to concrete containing graded ceramic sand as aggregate and with an apparent density not exceeding 1950kg / m 3 When lightweight aggregate concrete is used in industrial and civil buildings and other projects, it can reduce the weight of the structure, help improve the efficiency of component transportation and hoisting, and reduce the foundation load. It is suitable for high-rise and large-span buildings. At the same time, the use of lightweight aggregate concrete can also improve the thermal effect of the building structure.
[0003] In the related art, there is a lightweight aggregate concrete, which includes the following components: 120kg water, 290kg cement, 20kg gypsum powder, 16kg water reducer, 80kg fly ash, 120kg sand, 270kg modified ceramsite, the particle size of fly ash is 1200 mesh, and the fineness modulus of sand is 2.2. The preparation method of modified ceramsite includes the following steps: grinding glass to obtain glass powder; mixing glass powder with fly ash, adding pore-forming agent, binder and water, stirring and mixing, and forming inner balls through a ball forming process; stirring and mixing glass powder, fly ash, brucite fiber, binder and water, and forming outer balls wrapped outside the inner balls through a ball forming process, and then drying, then roasting the inner balls and outer balls, and then cooling to room temperature to obtain modified ceramsite.
[0004] With respect to the above-mentioned related technologies, the inventors believe that the lightweight aggregate concrete in the related technologies uses expanded clay as coarse aggregate, and the expanded clay prepared according to the method in the related technologies has poor mechanical properties and has more pores, which can easily lead to internal defects such as shrinkage cracks in the lightweight aggregate concrete. Therefore, the lightweight aggregate concrete in the related technologies is prone to serious quality loss under freeze-thaw cycle conditions, which is not conducive to the promotion and application of lightweight aggregate concrete. Summary of the invention
[0005] The lightweight aggregate concrete in the related art is prone to serious quality loss under freeze-thaw cycle conditions, which is not conducive to the promotion and application of lightweight aggregate concrete. In order to improve this defect, the present application provides a high-performance coal gangue lightweight aggregate concrete and a preparation method thereof.
[0006] In the first aspect, the present application provides a high-performance coal gangue lightweight aggregate concrete, adopting the following technical scheme: a high-performance coal gangue lightweight aggregate concrete, the raw materials of the lightweight aggregate concrete include the following components in parts by weight: 20-42 parts of silicate cement, 4-10 parts of mineral admixtures, 1.2-3.6 parts of filling whiskers, 30-85 parts of graded ceramic sand, 20-28 parts of alkali slag, 10-22 parts of water, and 0.22-0.52 parts of admixtures; the mineral admixture includes tricalcium aluminate monoore, the filling whiskers include calcium sulfate whiskers, the graded ceramic sand includes expanded clay and ceramic sand, the raw materials of the graded ceramic sand include coal gangue, and the admixture includes a water reducer.
[0007] By adopting the above technical scheme, the present application adds filler whiskers and alkali slag to the formula system, and also preferably selects the mineral admixture as tricalcium aluminate monoore. Alkali slag and graded pottery sand both have the ability to store and release water. In the lightweight aggregate concrete of the present application, the graded pottery sand and alkali slag after absorbing water can release water as the humidity inside the concrete decreases, which helps to delay the decrease of the humidity inside the concrete, achieve the internal curing effect, and then reduce the shrinkage of the concrete. Alkali slag contains calcium sulfate and a certain amount of soluble chloride ions. After silicate cement is hydrated, calcium hydroxide can be produced, and the soluble chloride ions in the alkali slag mainly exist in the form of calcium chloride, which can react with calcium hydroxide to form insoluble calcium oxychloride. On the one hand, the tricalcium aluminate in silicate cement and mineral admixtures can react with calcium chloride to produce insoluble hydrated calcium chloroaluminate, and on the other hand, it can also react with calcium sulfate in the alkali slag and calcium sulfate whiskers in the concrete component to produce calcium aluminate. Hydrated calcium chloroaluminate, calcium oxychloride, and ettringite can play a role of skeleton support together, which is conducive to the formation of cement stone structure, and realizes the solidification of soluble chloride ions, overcoming the defect that chloride ions easily aggravate freeze-thaw damage. The expansion generated when ettringite is formed can compensate for the shrinkage of concrete, and in addition, hydrated calcium chloroaluminate and calcium oxychloride are also produced in the pore structure of alkali slag, so it is helpful to overcome the influence of alkali slag on the development of concrete mechanical properties, and it is also possible to make calcium sulfate whiskers more fully combined with cement stone. By adopting the scheme of the present application to prepare lightweight aggregate concrete, on the one hand, it is possible to realize the recycling of waste, on the other hand, it can also play a role in reducing shrinkage, reducing the negative impact of the use of graded pottery sand on the freeze-thaw resistance, overcoming the defect of poor freeze-thaw resistance of ceramsite lightweight aggregate concrete in the related art, and being conducive to the promotion and application of lightweight aggregate concrete.
[0008] Preferably, the ceramsite is prepared according to the following method:
[0009] (1) mixing the sulfur-fixing ash and coal gangue in a weight ratio of (1.7-2.8):1, adding a flux and grinding to obtain a powder, adding water to the powder for aging to obtain an aged material for standby use;
[0010] (2) Granulating the aged material to obtain raw material balls, drying the raw material balls, and then pre-burning them at 400-420°C for 20-25 minutes, heating them to 1150-1200°C, roasting them for 5-7 minutes, cooling them to 680-700°C in the furnace, taking them out and waiting for natural cooling to obtain ceramsite.
[0011] By adopting the above technical scheme, the present application uses sulfur-fixing ash and coal gangue as the main components and adopts a sintering method to prepare ceramsite. The sulfur-fixing ash contains calcium sulfate and free calcium oxide. During the calcination process, calcium sulfate can react with coal gangue to produce intermediate minerals such as calcium sulfoaluminate and anhydrous calcium sulfoaluminate, thereby increasing the activity of coal gangue. Under the activation of calcium sulfate, free calcium oxide can react with coal gangue as a calcium source to form a certain amount of hydraulic cementitious minerals. The formation of hydraulic cementitious minerals enables ceramsite to provide a certain strength during immersion and concrete curing, which helps to reduce the negative impact of ceramsite on the durability of lightweight aggregate concrete and improve the freeze-thaw resistance of lightweight aggregate concrete.
[0012] The expanded clay of the present application uses coal gangue as one of the main components. The finished expanded clay has the property of storing and releasing water. It can release water when the relative humidity inside the concrete decreases to promote the hydration of the surrounding cementitious materials, reduce the downward gradient of the humidity inside the concrete, and play an internal curing effect together with pottery sand and alkali slag, which can effectively reduce the self-shrinkage of the concrete.
[0013] Preferably, the mass fraction of calcium sulfate in the desulfurized ash is 4.3-5.2%, and the mass fraction of free calcium oxide is 2.2-2.6%.
[0014] By adopting the above technical solution, the present application optimizes the mass fraction of calcium sulfate and free calcium oxide in the solid sulfur ash, which helps to fully improve the mechanical properties of ceramsite and improve the freeze-thaw resistance of lightweight aggregate concrete.
[0015] Preferably, the flux is potassium carbonate, and the amount of the flux is 1.2-1.7% of the total weight of the solid sulfur ash and coal gangue.
[0016] By adopting the above technical scheme, the present application preferably uses potassium carbonate as a flux and preferably uses potassium carbonate. The addition of potassium carbonate can increase the total amount of liquid phase produced during the calcination process, so that the ceramsite has better mechanical properties, and on the other hand, it also produces a small amount of pores in the ceramsite. Under the flux dosage conditions of the present application, the generation of pores can prevent stress concentration, help improve the mechanical properties of ceramsite, and improve the freeze-thaw resistance of lightweight aggregate concrete.
[0017] Preferably, the ceramic sand is prepared according to the following method:
[0018] (1) mixing nepheline tailings, silicate cement and fly ash in a weight ratio of (3.8-4.2):(3-4):(1-1.2), and then adding a water retaining agent to obtain a base material for standby use; taking the concentration of the base material as a reference, weighing hydrogen peroxide, water glass and mixing water in a ratio of 4-8%, 17-22% and 7-12% of the total weight of the base material, respectively, and setting them aside;
[0019] (2) Add mixing water into a ball forming machine, add the base material into the ball forming machine after stirring, spray hydrogen peroxide on the surface of the base material, and continue stirring. When the amount of hydrogen peroxide sprayed reaches 30-35% of the total volume of hydrogen peroxide, start spraying water glass into the base material until the water glass and hydrogen peroxide are used up, and continue stirring for a period of time to obtain material balls;
[0020] (3) Screening the obtained balls, curing the screened balls, crushing and drying the balls after curing, re-screening and compounding according to different particle size grades to obtain pottery sand.
[0021] By adopting the above technical scheme, the present application uses nepheline tailings, silicate cement and fly ash as main raw materials, hydrogen peroxide as foaming agent, and water glass as activator to prepare unburned ceramsite, and then obtains pottery sand by crushing, screening and compounding. In the method of the present application, in order to facilitate the balling of the base material, the balling machine is pre-wetted with mixing water, and then hydrogen peroxide is added by spraying, so that hydrogen peroxide is absorbed by the base material in the balling process. Afterwards, the addition of water glass plays a bonding role on the one hand, promotes the balling process, and on the other hand, provides an alkaline environment, so that hydrogen peroxide begins to foam, and finally obtains a ball with certain water absorption performance, and is further processed into pottery sand.
[0022] Preferably, the water retaining agent comprises modified polyacrylonitrile fiber powder, the amount of the modified polyacrylonitrile fiber powder is 1-5% of the weight of the base material, and the modified polyacrylonitrile fiber powder is prepared according to the following method:
[0023] (1) tying and opening polyacrylonitrile fibers to obtain fiber balls for later use; preparing a sodium hydroxide solution with a mass concentration of 8-10% and a hydrochloric acid solution with a mass concentration of 3-4% for later use;
[0024] (2) immersing the fiber balls in a sodium hydroxide solution at a weight ratio of 1:(20-28), heating at 95-98° C. for 60-70 min, and continuously stirring and condensing and refluxing during the heating process;
[0025] (3) After heating, the fiber balls are washed with water, immersed in hydrochloric acid for neutralization, then taken out and washed with water again, dried, and then crushed to obtain modified polyacrylonitrile fiber powder.
[0026] By adopting the above technical solution, the present application uses polyacrylonitrile fiber as raw material, converts the nitrile group into a carboxylate group by treating with an alkaline solution, and then converts the carboxylate group into a carboxyl group by acid washing and water washing, thereby completing the hydrolysis of the nitrile group. By dispersing the hydrolyzed polyacrylonitrile fiber, a fiber powder with certain water absorption and water retention properties can be obtained, which can be used as a water retention agent.
[0027] Preferably, the admixture is formed by mixing a water reducer and triethanolamine in a weight ratio of (20-50):1.
[0028] By adopting the above technical solution, the present application selects triethanolamine as a component of the admixture, and mixes triethanolamine and a water reducer for use. Triethanolamine can promote the formation of ettringite, creating favorable conditions for the reaction of tricalcium aluminate and calcium sulfate to produce ettringite, which helps to improve the freeze-thaw resistance of lightweight aggregate concrete.
[0029] Preferably, the tricalcium aluminate monoore is prepared according to the following method:
[0030] Calcium carbonate and aluminum oxide are mixed in a molar ratio of 3:1, ground and pulverized, and then calcined at 1400-1450° C. until the free calcium oxide content is less than 1%, and then ball milled to obtain tricalcium aluminate monoore.
[0031] By adopting the above technical solution, the present application uses calcium carbonate and aluminum oxide as raw materials, reacts the two under calcination conditions, and obtains tricalcium aluminate single ore.
[0032] Preferably, the mineral admixture is formed by mixing tricalcium aluminate ore and modified steel slag in a weight ratio of (3.2-3.6):1, and the modified steel slag is prepared according to the following method:
[0033] Steel slag, bauxite and limestone are mixed at a calcium-silicon ratio of 2.7-2.8, and raw powder is obtained after ball milling. Manganese dioxide with a weight equivalent to 1-2% of the total weight of the raw powder is added to the raw powder to obtain a composite powder. The composite powder is pressed into a block under a pressure of 1.2-1.7 MPa, and then heated to 1280-1360°C, kept warm for 40-45 minutes, and then quenched in air. Modified steel slag is obtained after crushing and grinding.
[0034] By adopting the above technical scheme, the present application uses limestone to adjust the calcium-silicon ratio of steel slag under high temperature conditions with the participation of manganese dioxide, and adds a certain amount of bauxite as an auxiliary component to obtain modified steel slag. The modified steel slag contains a certain amount of tetracalcium aluminoferrate, and the hydration product of tetracalcium aluminoferrate can react with chloride salt to form hydrated calcium chloroaluminate. Therefore, when it replaces ordinary steel slag as a mineral admixture, it can improve the skeleton support effect of insoluble mineral components, thereby improving the freeze-thaw resistance of lightweight aggregate concrete.
[0035] In a second aspect, the present application provides a method for preparing high-performance coal gangue lightweight aggregate concrete, which adopts the following technical solution.
[0036] A method for preparing high-performance coal gangue lightweight aggregate concrete comprises the following steps:
[0037] (1) mixing ceramsite and pottery sand, and mixing the obtained mixture with a portion of water and stirring to obtain graded pottery sand, which is ready for use; mixing an admixture with the remaining water to obtain an admixture solution, which is ready for use; mixing silicate cement, filling whiskers, mineral admixtures and alkali residue to obtain a dry material, which is ready for use;
[0038] (2) Mixing and stirring the dry material and graded pottery sand, adding the admixture solution during the stirring process, and then continuing to stir to obtain a concrete mixture, and then putting the concrete mixture into a mold for curing. After curing to a specified age, a high-performance coal gangue lightweight aggregate concrete is obtained.
[0039] By adopting the above technical scheme, the present application first prepares graded ceramic sand, dry material and admixture solution respectively, and then performs mixing processing in two steps to obtain a concrete mixture. After the concrete mixture is cured, high-performance coal gangue lightweight aggregate concrete can be obtained.
[0040] In summary, this application has the following beneficial effects:
[0041] 1. Utilization of renewable resources: Coal gangue is the industrial waste with the largest land area and accumulated stock in my country. It contains harmful substances such as heavy metals and sulfides, which usually need to be treated and disposed of. Using it as aggregate for concrete can reduce the demand for traditional aggregates and reduce the exploitation and consumption of natural resources.
[0042] 2. Lightweight: The apparent density of coal gangue ceramsite (about 1600kg / m 3 ) is about 3 / 5 of the ordinary aggregate, and the density of recycled lightweight aggregate concrete (about 1800kg / m 3 ) and ordinary concrete (density about 2400kg / m 3 ) can be reduced by about 25% compared with conventional concrete, which can effectively reduce the dead weight of concrete and save the amount of steel bars.
[0043] 3. Good thermal insulation performance: Since the interior of the gangue expanded clay has a honeycomb porous structure without capillary phenomenon, the thermal conductivity of the gangue lightweight aggregate concrete is greatly reduced compared with that of ordinary concrete, which can greatly improve the self-insulation function of the floor. In this embodiment, the thermal conductivity of the gangue lightweight aggregate concrete is 0.35W / (m·K), which is much lower than the thermal conductivity of ordinary concrete 1.40W / (m·K), and has lower thermal conductivity.
[0044] 4. Anti-shrinkage: Coal gangue ceramsite has a "sponge" core and a "micro-connected pore" shell structure. It has high water absorption and excellent water storage and release properties. It can release moisture when the relative humidity inside the concrete drops to promote the hydration of the surrounding cementitious materials, reduce the downward gradient of the humidity inside the concrete, produce an internal curing effect, and effectively reduce the self-shrinkage of the concrete.
[0045] 5. Self-leveling: The shape of ceramsite particles is similar to a circle, which can significantly improve the flow properties of concrete. It can flow naturally, self-level and self-fill without applying external force, providing convenience for construction and making the construction simple and easy.
[0046] 6. Good sound insulation performance: The weighted standardized impact sound pressure level of the coal gangue lightweight aggregate concrete insulation and sound insulation floor system is about 65dB, which can well meet the impact sound insulation performance requirements of GB 50118 "Civil Building Sound Insulation Code" for high-demand residential bedrooms, living rooms (halls) for separate floor slabs. DETAILED DESCRIPTION
[0047] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.
[0048] Preparation example of ceramsite
[0049] The following is an explanation using Preparation Example 1.
[0050] Preparation Example 1
[0051] In this preparation example, ceramsite is prepared according to the following method:
[0052] (1) The sulfur-fixing ash and coal gangue were mixed in a weight ratio of 1.7:1 (referred to as the ceramsite ratio in Table 2), and then ground after adding flux to obtain a ceramsite with a specific surface area of 350 m 2 / kg of powder, add water equivalent to 10% of the total weight of the powder to the powder, and then let it stand in a dense container for 24 hours to obtain an aged material for standby use; the mass fraction of calcium sulfate in the solid sulfur ash is 3.8%, and the mass fraction of free calcium oxide is 1.9%; the flux is potassium carbonate, and the amount of potassium carbonate is 0.9% of the sum of the weight of the solid sulfur ash and coal gangue;
[0053] (2) The aged material is granulated to obtain raw material balls, which are dried and then pre-fired at 400°C (referred to as the pre-fired temperature in Table 2) for 20 min (referred to as the pre-fired time in Table 2), and then heated to 1150°C (referred to as the roasting temperature in Table 2) at a rate of 30°C / min, roasted for 5 min (referred to as the roasting time in Table 2), and then cooled to 680°C (referred to as the furnace cooling temperature in Table 2) with the furnace, and then taken out and waited to cool naturally to 20°C to obtain ceramsite.
[0054] As shown in Table 1, the differences between Preparation Examples 1-5 are that the ceramsite ratios and some production and processing parameters are different.
[0055] Table 1 Ceramic aggregate ratio, production and processing parameters
[0056]
[0057] Preparation Example 5-9
[0058] As shown in Table 2, the difference between Preparation Examples 5-9 is that the mass fraction of calcium sulfate and the mass fraction of free calcium oxide in the desulfurized ash are different.
[0059] Table 2 Calcium sulfate mass fraction and free calcium oxide mass fraction
[0060] sample Calcium sulfate mass fraction / % Free calcium oxide mass fraction / % Preparation Example 5 3.8 1.9 Preparation Example 6 4.1 2.0 Preparation Example 7 4.3 2.2 Preparation Example 8 4.7 2.4 Preparation Example 9 5.2 2.6
[0061] Preparation Examples 9-13
[0062] As shown in Table 3, the difference between Preparation Examples 9-13 is that the percentage of the amount of flux used in the sum of the weight of the solid sulfur ash and coal gangue (referred to as flux ratio in Table 3) is different.
[0063] Table 3 Flux ratio
[0064] sample Flux ratio / % Preparation Example 9 0.9 Preparation Example 10 1.2 Preparation Example 11 1.4 Preparation Example 12 1.5 Preparation Example 13 1.7
[0065] The preparation example of pottery sand is described below using Preparation Example 14 as an example.
[0066] Preparation Example 14
[0067] Before formally preparing pottery sand, the water retaining agent must be prepared first. The water retaining agent is modified polyacrylonitrile fiber powder. The modified polyacrylonitrile fiber powder is prepared according to the following method:
[0068] (1) The polyacrylonitrile fibers were tied and opened to obtain fiber balls, which were set aside; a sodium hydroxide solution with a mass concentration of 8% (referred to as sodium hydroxide concentration in Table 4) and a hydrochloric acid with a mass concentration of 3% (referred to as hydrochloric acid concentration in Table 4) were prepared and set aside; the fineness of the polyacrylonitrile fibers was 1.67 dtex and the length was 140 mm;
[0069] (2) immersing the fiber balls in a sodium hydroxide solution at a weight ratio of 1:28 (referred to as the immersion ratio in Table 4), heating at 95° C. (referred to as the heating temperature in Table 4) for 6 min (referred to as the heating time in Table 4), and continuously stirring and performing condensation reflux during the heating process;
[0070] (3) After heating, the fiber balls are washed with water, immersed in hydrochloric acid for neutralization, then taken out and washed with water again, dried at 105°C, and then crushed to obtain modified polyacrylonitrile fiber powder with an average length of 1.5 mm.
[0071] After obtaining the water-retaining agent, you can start preparing the pottery sand.
[0072] In this preparation example, pottery sand is prepared according to the following method:
[0073] (1) Mix nepheline tailings, P.O42.5 silicate cement and Class F II fly ash in a weight ratio of 3.8:3:1 (referred to as the mixing ratio in Table 4), and then add a water retaining agent to obtain a base material for use; with the base material concentration as a reference, weigh hydrogen peroxide, water glass and mixing water in a ratio of 4% (referred to as the amount of hydrogen peroxide in Table 4), 17% (referred to as the amount of water glass in Table 4), and 7% (referred to as the amount of mixing water in Table 4) of the total weight of the base material, respectively, and set aside; the composition of the nepheline tailings is calculated by mass fraction of oxides, and the main components are as follows: silicon dioxide 44.21%, aluminum oxide 29.08%, sodium oxide 10.94%, calcium oxide 9.07%, and potassium oxide 4.57%; the water content of water glass is 66%, and the modulus is 3.19; the mass concentration of hydrogen peroxide in hydrogen peroxide is 30%;
[0074] (2) Add mixing water into a ball-forming machine, add the base material into the ball-forming machine after stirring, spray hydrogen peroxide on the surface of the base material, and continue stirring. When the amount of hydrogen peroxide sprayed reaches 30% of the total volume of hydrogen peroxide (referred to as the initial spraying amount of hydrogen peroxide in Table 4), start spraying water glass into the base material until the water glass and hydrogen peroxide are used up, and continue stirring for a period of time to obtain material balls;
[0075] (3) The obtained balls are screened and then cured (according to standard concrete curing conditions for 28 days). After the curing, the balls are crushed and dried, and then re-screened and compounded according to different particle size grades to obtain ceramic sand.
[0076] As shown in Table 4, the difference between Preparation Examples 14-18 lies in the different raw material ratios of the water retaining agent and the ceramic sand, and the production and processing parameters.
[0077] Table 4 Raw material ratios, production and processing parameters of water retaining agent and ceramic sand
[0078]
[0079]
[0080] Preparation Example of Tricalcium Aluminate Monoore
[0081] The following is an explanation using Preparation Example 19 as an example.
[0082] Preparation Example 19
[0083] In this preparation example, tricalcium aluminate monoore was prepared according to the following method:
[0084] Calcium carbonate and aluminum oxide were mixed in a molar ratio of 3:1, ground and calcined at 1400°C until the free calcium oxide content was less than 1%. After ball milling, a specific surface area of 420 m 2 / kg of tricalcium aluminate single mineral.
[0085] As shown in Table 5, the difference between Preparation Examples 19-23 is that the calcination temperatures of tricalcium aluminate monoore are different.
[0086] Table 5 Calcination temperature of tricalcium aluminate single ore
[0087] sample Calcination temperature / % Preparation Example 19 1400 Preparation Example 20 1410 Preparation Example 21 1425 Preparation Example 22 1440 Preparation Example 23 1450
[0088] Preparation example of modified steel slag
[0089] The following is an explanation using Preparation Example 24 as an example.
[0090] Preparation Example 24
[0091] In this preparation example, the modified steel slag is prepared according to the following method:
[0092] Steel slag, bauxite and limestone were mixed at a calcium-silicon molar ratio of 2.7 (referred to as calcium-silicon ratio in Table 6), and the weight ratio of bauxite to steel slag was set to 1:13.8. After ball milling, raw powder was obtained. Manganese dioxide with a weight equivalent to 1-2% of the total weight of the raw powder (referred to as manganese dioxide dosage in Table 6) was added to the raw powder to obtain a composite powder. The composite powder was pressed into a block under a pressure of 1.2 MPa (referred to as molding pressure in Table 6), and then heated to 1280°C (referred to as calcination temperature in Table 6) at a rate of 35°C / min, kept warm for 40 minutes (referred to as holding time in Table 6), and then quenched in room temperature air at 20°C. After crushing and grinding, a block with a specific surface area of 420m 2 / kg of modified steel slag.
[0093] As shown in Table 6, the difference between Preparation Examples 24-28 lies in the different production and processing parameters of the modified steel slag.
[0094] Table 6 Production and processing parameters of modified steel slag
[0095]
[0096] Example
[0097] Examples 1-5
[0098] The following description is given by taking Example 1 as an example.
[0099] Example 1
[0100] This embodiment provides a lightweight aggregate concrete, the raw materials of which include the following components: 20 kg of silicate cement, 4 kg of mineral admixture, 1.2 kg of filler whisker, 30 kg of graded pottery sand, 20 kg of alkali slag, 10 kg of water, and 0.22 kg of admixture. The silicate cement is P.O42.5 silicate cement, and the mineral admixture is a single calcium aluminate ore of Preparation Example 19 and a single calcium aluminate ore with a specific surface area of 420 m 2 / kg of steel slag powder is mixed in a weight ratio of 3.2:1; the filling whiskers are calcium sulfate whiskers with an average length of 150μm and an average diameter of 1.8μm; the graded ceramic sand is prepared by mixing the ceramsite of Preparation Example 1 and the ceramic sand of Preparation Example 14 in a weight ratio of 5:4 and then adding water and stirring, the fineness modulus of the ceramic sand is 2.3, and the ceramsite satisfies a continuous grading of 5-10mm; the average particle size of the alkali slag is 0.32mm, the mass fraction of soluble chloride ions in the alkali slag is 8.2%, the moisture content (mass fraction) of the alkali slag is 32%, and the mass fraction of calcium sulfate in the alkali slag is 12.8%; the admixture is a water reducer with a water reduction rate of 27%.
[0101] In this embodiment, high-performance coal gangue lightweight aggregate concrete is prepared according to the following steps:
[0102] (1) mixing ceramsite and pottery sand, and mixing and stirring the obtained mixture with a portion of water (weighed according to 15% of the total water consumption) to obtain graded pottery sand, which is set aside; mixing an admixture with the remaining water to obtain an admixture solution, which is set aside; mixing silicate cement, filling whiskers, mineral admixtures and alkali slag to obtain dry material, which is set aside;
[0103] (2) The dry material and graded pottery sand are mixed, and after stirring for 120 seconds, an admixture solution is added, and stirring is continued for 120 seconds to obtain a concrete mixture. The concrete mixture is poured into a mold for curing, and high-performance coal gangue lightweight aggregate concrete is obtained after curing to a specified age.
[0104] As shown in Table 7, the differences between Examples 1-5 mainly lie in the different raw material ratios of the concrete mixtures.
[0105] Table 7 Ratio of raw materials for concrete mixture
[0106]
[0107]
[0108] Example 5-17
[0109] As shown in Table 8, the difference between Examples 5-17 is that the preparation examples of ceramsite are different.
[0110] Table 8 Preparation example of ceramsite
[0111]
[0112] Examples 17-21
[0113] As shown in Table 9, the difference between Examples 17-21 is that the preparation examples of ceramic sand are different.
[0114] Table 9 Preparation example of pottery sand
[0115] sample Preparation Example Embodiment 17 Preparation Example 14 Embodiment 18 Preparation Example 15 Embodiment 19 Preparation Example 16 Embodiment 20 Preparation Example 17 Embodiment 21 Preparation Example 18
[0116] Embodiment 22
[0117] The difference between this embodiment and Embodiment 21 is that the admixture is a mixture of a water reducer and triethanolamine in a weight ratio of 50:1.
[0118] As shown in Table 10, the difference between Examples 22-26 is that the weight ratio of the water reducing agent to triethanolamine is different.
[0119] Table 10 Weight ratio of water reducer and triethanolamine
[0120] sample Water reducing agent: triethanolamine Embodiment 22 50:1 Embodiment 23 40:1 Embodiment 24 30:1 Embodiment 25 25:1 Embodiment 26 20:1
[0121] Examples 26-30
[0122] As shown in Table 11, the difference between Examples 26-30 is that the preparation examples of tricalcium aluminate monoore are different.
[0123] Table 11 Preparation example of tricalcium aluminate monoore
[0124] sample Preparation Example Embodiment 26 Preparation Example 19 Embodiment 27 Preparation Example 20 Embodiment 28 Preparation Example 21 Embodiment 29 Preparation Example 22 Embodiment 30 Preparation Example 23
[0125] Embodiment 31
[0126] The difference between this embodiment and Embodiment 30 is that the mineral admixture is formed by mixing tricalcium aluminate ore and the modified steel slag of Preparation Example 24 in a weight ratio of 3.2:1.
[0127] As shown in Table 12, the difference between Examples 31-35 is that the weight ratio of tricalcium aluminate ore and modified steel slag (referred to as mineral admixture ratio in Table 12) is different.
[0128] Table 12 Proportion of mineral admixtures
[0129]
[0130]
[0131] As shown in Table 13, the difference between Examples 35-39 is that the preparation examples of modified steel slag are different.
[0132] Table 13 Preparation example of modified steel slag
[0133] sample Preparation Example Embodiment 35 Preparation Example 24 Embodiment 36 Preparation Example 25 Embodiment 37 Preparation Example 26 Embodiment 38 Preparation Example 27 Embodiment 39 Preparation Example 28
[0134] Comparative Example
[0135] Comparative Example 1
[0136] A lightweight aggregate concrete comprises the following components: 120kg of water, 290kg of cement (P.O42.5), 20kg of gypsum powder, 16kg of water reducing agent, 80kg of fly ash, 120kg of sand, and 270kg of modified ceramsite; the particle size of the fly ash is 1200 meshes, the fineness modulus of the sand is 2.2, and the water reducing agent is sodium lignin sulfonate.
[0137] The preparation method of modified ceramsite comprises the following steps: grinding glass to obtain glass powder with a mesh size of 200; mixing the glass powder with fly ash, adding a pore-forming agent, a binder and water, stirring and mixing, and forming an inner ball through a ball-forming process; stirring and mixing the glass powder, fly ash, brucite fiber, a binder and water, and forming an outer ball wrapped outside the inner ball through a ball-forming process, and then drying, and then roasting the inner ball and the outer ball, and then cooling to room temperature to obtain modified ceramsite; the glass powder, fly ash, and the pore-forming agent are mixed; and the mixture is stirred and mixed. , the weight ratio of binder and water is 1:2:0.5:0.1:0.9, the pore-forming agent is calcium carbonate, the binder is water glass with a modulus of 3.3, and the specification model of brucite fiber is water 5-50 (short fiber); the weight ratio of inner ball to outer ball is 1:0.2; the calcination process of modified ceramsite is: drying at 80℃ for 10h, preheating at 600℃ for 30min, calcining at 700℃ for 20min, and ending calcination after cooling. The maximum particle size of modified ceramsite is 20mm and the minimum particle size is 18mm.
[0138] Comparative Example 2
[0139] The difference between this comparative example and Example 1 is that the tricalcium aluminate ore is replaced by steel slag powder.
[0140] Comparative Example 3
[0141] The difference between this comparative example and Example 1 is that the calcium sulfate whiskers are replaced with gypsum powder with an average particle size of 2.4 μm.
[0142] Performance testing methods
[0143] Lightweight aggregate concrete specimens were prepared according to the description of each embodiment and comparative example, and rapid freeze-thaw tests were carried out on the specimens in accordance with the provisions of Test Method for Long-term Performance and Durability of Ordinary Concrete (GB / T 50082-2009). The specimens were subjected to standard curing after molding, demolded after 28 days, immersed in 18°C water 4 days before the start of the test, and the initial weight of the specimens was checked before the test. Each freeze-thaw cycle was completed within 4 hours. When the specimens were frozen and melted, the center temperature of the specimens was controlled at (-17±2)°C and (8±2)°C, respectively. After 200 freeze-thaw cycles, the specimens were taken out and the weight was checked again.
[0144] The mass loss of the specimen during the freeze-thaw cycle was calculated as a percentage of the original mass of the test, which was recorded as the mass loss rate. Then, based on the mass loss rate of Comparative Example 1, the ratio of the mass loss rate of each embodiment and comparative example to the mass loss rate of Comparative Example 1 was calculated, and the ratio was recorded as the relative loss rate. The results are shown in Table 14.
[0145] Table 14 Relative loss rate
[0146]
[0147]
[0148] Combining Examples 1-5 and Comparative Example 1 and Table 14, it can be seen that the relative examples measured in Examples 1-5 are all lower than Comparative Example 1, indicating that the degree of damage to the samples of Examples 1-5 during the freeze-thaw cycle is relatively low. The scheme of the present application plays a role in reducing shrinkage, reduces the negative impact of the use of graded ceramic sand on the freeze-thaw resistance, overcomes the defect of poor freeze-thaw resistance of ceramsite lightweight aggregate concrete in the related art, and is conducive to the promotion and application of lightweight aggregate concrete.
[0149] Combining Example 1 and Comparative Example 2 with Table 14, it can be seen that when tricalcium aluminate is missing from the components of lightweight aggregate concrete, the measured relative loss rate is higher, indicating that the sample of Comparative Example 2 is more severely damaged after freeze-thaw cycles. Based on this situation, it can be inferred that the lack of tricalcium aluminate affects the formation of hydrated calcium chloroaluminate and ettringite, resulting in the freeze-thaw resistance of lightweight aggregate concrete being affected.
[0150] Combining Example 1 and Comparative Example 3 with Table 14, it can be seen that when calcium sulfate whiskers are missing from the components of lightweight aggregate concrete, even if gypsum powder is added as a substitute, it is difficult to fully improve the freeze-thaw resistance of lightweight aggregate concrete.
[0151] It can be seen from Examples 5-9 and Table 14 that the ceramsite prepared according to the schemes of Preparation Examples 1-5 can be used in the scheme of the present application and enable the lightweight aggregate concrete to have better freeze-thaw resistance.
[0152] It can be seen from Examples 9-13 and Table 14 that when the mass fraction of calcium sulfate in the fixed sulfur ash is 4.3-5.2% and the mass fraction of free calcium oxide is 2.2-2.6%, the mass loss of lightweight aggregate concrete is relatively small, indicating that the ceramsite prepared from the fixed sulfur ash selected within the above range is more helpful to improve the freeze-thaw resistance of lightweight aggregate concrete.
[0153] It can be seen from Examples 13-17 and Table 14 that when the flux is potassium carbonate, limiting the amount of the flux to 1.2-1.7% of the sum of the weight of the solid sulfur ash and coal gangue helps to fully improve the freeze-thaw resistance of lightweight aggregate concrete.
[0154] It can be seen from Examples 17-21 and Table 14 that the pottery sand prepared according to the methods of Preparation Examples 14-18 can be used in the scheme of the present application and can make the lightweight aggregate concrete have better anti-freeze-thaw performance.
[0155] It can be seen from Example 21, Examples 22-26 and Table 14 that the addition of triethanolamine reduces the mass loss of lightweight aggregate concrete, which means that the freeze-thaw resistance is improved. Based on this, it can be considered that since triethanolamine can promote the formation of ettringite, it is beneficial for tricalcium aluminate to react with calcium sulfate in the alkali slag and calcium sulfate whiskers in the concrete component to produce ettringite, thereby improving the freeze-thaw resistance of lightweight aggregate concrete.
[0156] It can be seen from Examples 26-30 and Table 14 that the tricalcium aluminate single ore prepared according to the methods of Preparation Examples 19-23 can be used in the scheme of the present application and can make the lightweight aggregate concrete have better anti-freeze-thaw properties.
[0157] It can be seen from Example 30, Examples 31-35 and Table 14 that the use of modified steel slag instead of steel slag powder can improve the freeze-thaw resistance of lightweight aggregate concrete.
[0158] It can be seen from Examples 35-39 and Table 14 that the modified steel slag prepared according to the methods of Preparation Examples 24-28 can be used in the scheme of the present application and can make the lightweight aggregate concrete have better freeze-thaw resistance.
[0159] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high performance coal gangue lightweight aggregate concrete, characterized in that: The raw materials of the lightweight aggregate concrete include the following components in parts by weight: 20-42 parts of silicate cement, 4-10 parts of mineral admixtures, 1.2-3.6 parts of filling whiskers, 30-85 parts of graded pottery sand, 20-28 parts of alkali slag, 10-22 parts of water, and 0.22-0.52 parts of admixtures; the mineral admixtures include tricalcium aluminate, the filling whiskers include calcium sulfate whiskers, the graded pottery sand includes ceramsite and pottery sand, the raw materials of the graded pottery sand include coal gangue, and the admixture includes a water reducer; the ceramsite is prepared according to the following method: (1) mixing the sulfur-fixing ash and coal gangue in a weight ratio of (1.7-2.8):1, adding a flux and grinding to obtain a powder, adding water to the powder for aging to obtain an aged material for standby use; (2) Granulate the aged material to obtain raw material balls, dry the raw material balls, and then pre-burn them at 400-420°C for 20-25 minutes, then heat them to 1150-1200°C, bake them for 5-7 minutes, cool them to 680-700°C in the furnace, then take them out and wait for them to cool down naturally to obtain expanded clay.
2. The high performance coal gangue lightweight aggregate concrete according to claim 1, characterized in that: The mass fraction of calcium sulfate in the desulfurized ash is 4.3-5.2%, and the mass fraction of free calcium oxide is 2.2-2.6%.
3. The high performance coal gangue lightweight aggregate concrete according to claim 1, characterized in that: The flux is potassium carbonate, and the amount of the flux is 1.2-1.7% of the total weight of the solid sulfur ash and coal gangue.
4. The high performance coal gangue lightweight aggregate concrete according to claim 1, characterized in that: The ceramic sand is prepared according to the following method: (1) Mix nepheline tailings, silicate cement and fly ash in a weight ratio of (3.8-4.2):(3-4):(1-1.2), and then add a water retaining agent to obtain a base material for later use; based on the concentration of the base material, weigh hydrogen peroxide, water glass and mixing water in a ratio of 4-8%, 17-22% and 7-12% of the total weight of the base material, respectively, and set aside; (2) Add mixing water into the ball forming machine, add the base material into the ball forming machine after stirring, then spray hydrogen peroxide on the surface of the base material and continue stirring. When the amount of hydrogen peroxide sprayed reaches 30-35% of the total volume of hydrogen peroxide, start spraying water glass into the base material until the water glass and hydrogen peroxide are used up. Continue stirring for a period of time to obtain material balls; (3) Screening the obtained balls, curing the screened balls, crushing and drying the balls after curing, re-screening and compounding according to different particle size grades to obtain ceramic sand.
5. The high performance coal gangue lightweight aggregate concrete according to claim 4, characterized in that: The water retaining agent comprises modified polyacrylonitrile fiber powder, the dosage of the modified polyacrylonitrile fiber powder is 1-5% of the weight of the base material, and the modified polyacrylonitrile fiber powder is prepared according to the following method: (1) ligating and opening polyacrylonitrile fibers to obtain fiber balls for later use; preparing a sodium hydroxide solution with a mass concentration of 8-10% and a hydrochloric acid solution with a mass concentration of 3-4% for later use; (2) immersing the fiber balls in a sodium hydroxide solution at a weight ratio of 1:(20-28), heating at 95-98° C. for 60-70 min, and continuously stirring and condensing and refluxing during the heating process; (3) After the heating is completed, the fiber balls are washed with water, and the washed fiber balls are immersed in hydrochloric acid for neutralization. The fiber balls are then taken out and washed with water again, the fiber balls are dried, and then the fiber balls are crushed to obtain modified polyacrylonitrile fiber powder.
6. The high performance coal gangue lightweight aggregate concrete according to claim 1, characterized in that: The admixture is prepared by mixing a water reducer and triethanolamine in a weight ratio of (20-50):
1.
7. The high performance coal gangue lightweight aggregate concrete according to claim 1, characterized in that: The tricalcium aluminate single ore is prepared according to the following method: Calcium carbonate and aluminum oxide are mixed in a molar ratio of 3:1, ground and calcined at 1400-1450°C until the free calcium oxide content is less than 1%, and then ball milled to obtain tricalcium aluminate monoore.
8. The high performance coal gangue lightweight aggregate concrete according to claim 7, characterized in that: The mineral admixture is prepared by mixing tricalcium aluminate ore and modified steel slag in a weight ratio of (3.2-3.6):1, and the modified steel slag is prepared according to the following method: Steel slag, bauxite and limestone are mixed at a calcium-silicon ratio of 2.7-2.8, and raw powder is obtained after ball milling. Manganese dioxide with a weight equivalent to 1-2% of the total weight of the raw powder is added to the raw powder to obtain a composite powder. The composite powder is pressed into a block under a pressure of 1.2-1.7 MPa, and then heated to 1280-1360°C, kept warm for 40-45 minutes, and then quenched in air. Modified steel slag is obtained after crushing and grinding.
9. The method for preparing high-performance coal gangue lightweight aggregate concrete according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) Mixing ceramsite and ceramic sand, and mixing the obtained mixture with a portion of water and stirring to obtain graded ceramic sand, which is set aside; mixing an admixture with the remaining water to obtain an admixture solution, which is set aside; mixing silicate cement, filler whiskers, mineral admixtures and alkali slag to obtain dry material, which is set aside; (2) Mixing and stirring the dry material and graded pottery sand, adding the admixture solution during the stirring process, and then continuing to stir to obtain a concrete mixture, and then putting the concrete mixture into a mold for curing. After curing to a specified age, a high-performance coal gangue lightweight aggregate concrete is obtained.