A ground silicon nitride ceramic sheet

Through ball milling mixing method and microwave sintering process, combined with multiple double-sided grinding and back-burning, the problem of brittleness and warpage of silicon nitride ceramic tiles is solved, and its applicability and performance in semiconductors are improved.

CN118239787BActive Publication Date: 2024-10-25江苏富乐华功率半导体研究院有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410331645.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-22
Publication Date
2024-10-25
Estimated Expiration
2044-03-22

AI Technical Summary

Technical Problem

The brittleness and warpage problems of silicon nitride ceramic tiles limit its application in semiconductors. Traditional grinding methods lead to uneven thickness of the ceramic tiles, affecting bonding and reliability.

Method used

The ball milling mixing method is used to add toughening materials of chopped carbon fiber and silicon carbide whiskers, modified by silane coupling agent, combined with microwave sintering process, and multiple double-sided grinding and back-burning are performed to improve the toughness and compactness of the ceramic.

Benefits of technology

It significantly improves the toughness and thermal conductivity of silicon nitride ceramic tiles, reduces brittleness and warpage, and enhances its applicability in the semiconductor field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004753699290000101
    Figure BDA0004753699290000101
Patent Text Reader

Abstract

The present invention relates to the field of semiconductor technology, specifically a kind of ground silicon nitride ceramic sheet. The preparation of the silicon nitride ceramic sheet includes the following preparation steps: step one: α-silicon nitride, modified toughening material, and sintering aid are added to a solvent, ball milling is mixed evenly, and a dispersion is obtained; step two: (1) the dispersion is centrifuged, the precipitate is filtered out, and after drying, grinding, and sieving, a powder is obtained; (2) the powder is placed in a mold, pressed and formed, and after being kept warm for a period of time, a silicon nitride ceramic body is obtained; step three: the silicon nitride ceramic body is subjected to microwave sintering to obtain silicon nitride ceramics; step four: silicon nitride ceramics are subjected to double-sided grinding, back-firing, and secondary double-sided grinding in sequence to obtain silicon nitride ceramic sheets. The silicon nitride ceramic sheet has few surface defects, uniform thickness, low warpage, high thermal conductivity, and large peel strength, and has a wider application in the semiconductor field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductors, in particular to a ground silicon nitride ceramic sheet. Background Art

[0002] In recent years, with the widespread application of high-power semiconductor devices, silicon nitride ceramic substrates (silicon nitride ceramic substrates are made of silicon nitride ceramic sheets and copper sheets) have a broad market as insulating substrate materials with high thermal conductivity and excellent mechanical properties. However, silicon nitride ceramic sheets have the defect of high intrinsic brittleness, which greatly limits their application in semiconductors; therefore, how to improve the toughness and reliability of silicon nitride ceramic sheets has become a key issue that needs to be solved urgently.

[0003] The strengthening and toughening of ceramics is essentially to reduce internal crack defects and improve the ability to resist crack propagation. The most direct method is second-phase toughening, which includes introducing reinforcing phases such as fibers, whiskers and particles into the matrix. Fibers, whiskers and particles are easy to agglomerate, resulting in low interfacial bonding between the ceramic matrix, which ultimately affects the mechanical properties and toughening effect of silicon nitride ceramic materials.

[0004] At the same time, considering the traditional grinding method of silicon nitride ceramic sheets, it is easy to cause the warping of silicon nitride ceramic sheets to exceed the standard value, making the thickness of the ceramic sheets uneven, which greatly affects the bonding between the copper sheets and the silicon nitride ceramic sheets, and ultimately leads to reduced peeling strength and thermal shock performance of the copper-clad substrate and increased thermal resistance, thereby reducing the reliability of semiconductor packages.

[0005] In summary, it is extremely necessary to obtain a silicon nitride ceramic wafer with less brittleness and to improve the surface state of the silicon nitride ceramic wafer to obtain a silicon nitride ceramic wafer with less warping and higher reliability, thereby improving its application in the semiconductor industry. Summary of the invention

[0006] The object of the present invention is to provide a ground silicon nitride ceramic sheet to solve the problems raised in the above background technology.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] A ground silicon nitride ceramic sheet, the preparation of which comprises the following preparation steps:

[0009] Step 1: Add α-silicon nitride, modified toughening material and sintering aid into the solvent, and mix by ball milling at a speed of 100 to 500 r / min for 24 to 72 hours to obtain a dispersion;

[0010] Step 2: (1) centrifuging the dispersion, filtering out the precipitate, heating it to 80-100° C. for drying, grinding and sieving to obtain a powder; (2) placing the powder in a mold, pressing it under a pressure of 100-200 MPa, and keeping it at 400-600° C. for 1-3 hours to obtain a silicon nitride ceramic body;

[0011] Step 3: placing the silicon nitride ceramic body on the auxiliary heating device, and placing it in the heat preservation device in the microwave sintering furnace to microwave sinter into porcelain, so as to obtain silicon nitride ceramics;

[0012] Step 4: The silicon nitride ceramic is subjected to double-sided grinding, re-firing, and double-sided grinding for a second time in sequence to obtain a silicon nitride ceramic sheet.

[0013] Furthermore, the mass ratio of the α-silicon nitride, the modified toughening material and the sintering aid is 100:(10-25):(5-20).

[0014] Furthermore, the preparation method of the modified toughening material is as follows: (1) soaking the toughening material in a 25-35wt% hydrofluoric acid solution for 24-48 hours, filtering, washing, and drying to obtain an acid-treated toughening material; (2) soaking the acid-treated toughening material in a 25-35wt% hydrogen peroxide solution for 1-2 hours, filtering, washing, and drying to obtain a carboxylated toughening material; (3) adding the carboxylated toughening material and thionyl chloride into a reaction container, stirring at 20-30°C and a speed of 500-600 r / min. After reacting for 10 to 30 minutes, the temperature is raised to 50 to 60° C., and the reaction is continued with stirring for 12 to 24 hours. The reaction is terminated, and finally, excess thionyl chloride is removed by rotary evaporation to obtain an acyl chloride toughening material; (4) The acyl chloride toughening material, a silane coupling agent with a hydroxyl group, and toluene are added to a reaction container, and stirred in a nitrogen atmosphere at 40 to 50° C. at a speed of 500 to 600 r / min for 10 to 20 minutes, and then refluxed for 3 to 6 hours to terminate the reaction. After filtering, washing, and drying, a modified toughening material is obtained.

[0015] Furthermore, the toughening material is composed of chopped carbon fibers and silicon carbide whiskers mixed in a mass ratio of 5:1, wherein the aspect ratio of the chopped carbon fibers is 100:1, and the aspect ratio of the silicon carbide whiskers is 20:1.

[0016] Furthermore, the mass ratio of the toughening material to the hydrofluoric acid solution is 1:(15-20).

[0017] Furthermore, the mass ratio of the acid-treated toughening material to the hydrogen peroxide is 1:(15-20).

[0018] Furthermore, the mass ratio of the carboxylated toughening material to thionyl chloride is 1:20.

[0019] Furthermore, the mass ratio of the acyl chloride toughening material, the silane coupling agent with hydroxyl group and toluene is 1:(0.05-0.1):20.

[0020] Furthermore, the hydroxyl-containing silane coupling agent includes, but is not limited to, a combination of one or more of 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane, 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, and tert-butyldimethylhydroxyethoxysilane.

[0021] Considering that silicon nitride ceramics are polycrystalline materials composed of covalent bonds, have strong bond energy, lack a slip system inside that can cause the material to deform, that is, it is difficult to undergo elastic deformation and plastic deformation. In addition, there are inevitable defects on the surface and inside of the ceramic material. Under the action of external loads, stress is easily concentrated at the crack source, causing brittle fracture of silicon nitride ceramics, which will undoubtedly limit the application of silicon nitride ceramics in semiconductors. Therefore, the scheme adds a toughening material composed of chopped carbon fibers and silicon carbide whiskers to the raw materials, so that the concentrated stress at the crack source of the ceramic matrix can be partially eliminated through the action of this material, so as to improve the material's resistance to crack propagation and prevent the propagation of cracks in the ceramic matrix, thereby achieving a toughening effect, reducing the brittleness of the prepared silicon nitride ceramics. On the other hand, considering that short carbon fibers and silicon carbide whiskers are easily agglomerated and unevenly dispersed when added to solvents, the interfacial bonding force of the sintered ceramics is low, affecting the mechanical properties and toughening effect of silicon nitride ceramics. Therefore, short carbon fibers and silicon carbide whiskers are modified by silane coupling agents to promote their dispersion and avoid agglomeration. At the same time, siloxane groups can be hydrolyzed into silanols, dehydrated and condensed with hydroxyl groups on the surfaces of silicon nitride and sintering aids, and connected with each component through chemical bonds, thereby enhancing the bonding force of each component and improving the density of silicon nitride ceramics to a certain extent, so as to obtain silicon nitride ceramics with better toughness and improve the brittle defect of silicon nitride ceramics. In addition, short carbon fibers and silicon carbide whiskers also have a positive effect on the thermal conductivity of silicon nitride.

[0022] Furthermore, the sintering aid is obtained by mixing the first sintering aid and the second sintering aid in a mass ratio of (4-8):(3-6).

[0023] Furthermore, the first sintering aid includes but is not limited to a combination of one or more of aluminum oxide, yttrium oxide, lanthanum oxide, and magnesium oxide; the second sintering aid includes but is not limited to a combination of one or more of boron oxide, lithium oxide, and zinc oxide.

[0024] Furthermore, the first sintering aid is obtained by mixing aluminum oxide, yttrium oxide, lanthanum oxide, and magnesium oxide in a mass ratio of 3:2:2:1; and the second sintering aid is obtained by mixing boron oxide, lithium oxide, and zinc oxide in a mass ratio of 1:1:2.

[0025] In the scheme, the sintering aid is composed of a first sintering aid and a second sintering aid. The first sintering aid is made of alumina and Re2O3 type rare earth oxides (yttrium oxide, lanthanum oxide), which have a small ionic radius. Therefore, while promoting sintering, it can also promote the growth of silicon nitride ceramic grains to improve the plasticity of silicon nitride ceramics and reduce its brittleness. At the same time, magnesium oxide is further added, which can cooperate with yttrium oxide and lanthanum oxide to promote ceramic densification and phase change. Since the microwave sintering method is used to sinter silicon nitride ceramics in this scheme, the second sintering aid is made of aluminum oxide with excellent The material composition with different microwave absorption properties can enhance the microwave absorption capacity of the silicon nitride ceramic body, make the temperature change of each part of the silicon nitride ceramic body more uniform when heated, can effectively avoid the defects caused by local overheating of the ceramic, and ensure the comprehensive performance of the sintered silicon nitride ceramic; under the synergistic effect of the first sintering aid and the second sintering aid, the sintering temperature is greatly reduced, and dense sintering can be achieved at 1500-1600°C, and the performance of the silicon nitride ceramic is improved, its brittleness is reduced, and its thermal conductivity is enhanced, which greatly expands the applicability of silicon nitride ceramics.

[0026] Furthermore, the solvent is obtained by mixing deionized water and polyvinyl alcohol in a mass ratio of 4:1.

[0027] Furthermore, after drying, the powder contains 5-10% solvent, and the polyvinyl alcohol contained in the remaining solvent can be used as a binder to stick the powder together. After heat preservation treatment and removal of the solvent, silicon nitride ceramics with better density can be obtained.

[0028] Furthermore, the powder, after grinding, has D 50 The particle size is 0.5~1μm.

[0029] In the scheme, a microwave sintering process is used to sinter the silicon nitride ceramic green body into porcelain to obtain silicon nitride ceramics; from the perspective of energy saving and environmental protection, microwave sintering can reduce the activation energy and sintering time required for sintering, and compared with traditional sintering, it can save energy by about 50 to 80%, greatly improving energy utilization efficiency; from the perspective of the ceramic itself, microwave sintering can make the material evenly heated inside and outside, which can inhibit the abnormal growth of ceramic grains, thereby improving the density and grain uniformity of silicon nitride ceramics, and ultimately obtaining silicon nitride ceramics with better mechanical properties to compensate for the subsequent strength loss caused by grinding and re-firing of silicon nitride ceramic pieces.

[0030] Furthermore, the parameters of the microwave sintering are as follows: microwave frequency is 2.45 GHz, nitrogen is used as protective gas, the gas pressure in the sintering chamber is 0.1-0.5 MPa, the heating rate is 10-20°C / min, the sintering temperature is 1500-1600°C, and the insulation time is 10-40 min; after the insulation is completed, the furnace is cooled to room temperature to obtain silicon nitride ceramics.

[0031] Furthermore, the specific process of step four is as follows: (1) the silicon nitride ceramic is double-sided ground once using a 400-1000 mesh sander, and both sides are ground to the same thickness to obtain ground ceramic; (2) the ground ceramic is placed in a microwave sintering furnace, and the microwave sintering parameters are set: the microwave frequency is 2.45 GHz, nitrogen is used as the protective gas, the gas pressure in the sintering chamber is 0.1-0.5 MPa, the heating rate is 1-5°C / min, the sintering temperature is 1100-1500°C, and the insulation time is 10-30 min; after the insulation is completed, the furnace is cooled to room temperature to obtain a re-fired ceramic; (3) the re-fired ceramic is double-sided ground again using a 400-1000 mesh sander, and both sides are ground to the same thickness to obtain a silicon nitride ceramic sheet.

[0032] Furthermore, the thickness of the grinding ceramic is 0.36-0.38 mm; the thickness of the silicon nitride ceramic sheet is 0.32 mm.

[0033] Furthermore, the total thickness lost after the first double-sided grinding and the second double-sided grinding is ≥80 μm.

[0034] In the scheme, in order to further reduce the defects of silicon nitride ceramic sheets and make them uniform in thickness, the prepared silicon nitride ceramics were subjected to three steps of primary grinding, re-firing and secondary grinding; the total thickness lost by the two grindings was ≥80μm, because only this thickness can remove the white spots on the surface; the purpose of the two grindings in the scheme is: the thinning amount of a small amount of multiple grindings is small, the warping will not increase significantly, and it is beneficial to control the thickness of the ground silicon nitride ceramic sheets to make them more uniform and cause less damage to the surface of the silicon nitride ceramic sheets; the purpose of re-firing is to eliminate the microcracks caused by the first grinding, because if the re-firing temperature is too high and the heating rate is too fast, the silicon nitride ceramic grains will grow too large, thereby causing its strength to drop sharply, so the sintering temperature needs to be controlled at 1100-1500℃; the second grinding can also remove the surface defects caused by re-firing; finally, silicon nitride ceramic sheets with few surface defects, uniform thickness, low warping, high thermal conductivity and high peeling strength are obtained.

[0035] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: (1) by adding toughening materials, the toughness of silicon nitride ceramics is improved, and by modifying the toughening materials, the dispersion of the toughening materials in the ceramics is promoted, and the bonding force of the components is enhanced, and the compactness of silicon nitride ceramics can be improved to a certain extent, so as to obtain silicon nitride ceramics with better toughness and improve the defect of large brittleness of silicon nitride ceramics; (2) two sintering aids are prepared to synergistically promote the orderly growth of silicon nitride ceramic grains, so as to improve the plasticity of silicon nitride ceramics and further improve the brittleness of silicon nitride ceramics; (3) the polyvinyl alcohol in the solvent has a bonding effect, which can tightly bind the components in the silicon nitride ceramic body. Combined together, the density of silicon nitride ceramics is promoted; (4) the scheme adopts microwave sintering process for sintering, which is energy-saving and environmentally friendly, and can inhibit the abnormal growth of ceramic grains, thereby improving the density and grain uniformity of silicon nitride ceramics, and finally obtaining silicon nitride ceramics with better mechanical properties to compensate for the subsequent strength loss caused by grinding and re-firing of silicon nitride ceramic pieces; (5) the scheme conducts double-sided grinding, re-firing, and double-sided grinding of silicon nitride ceramics once. By grinding in small amounts and multiple times, the thickness of silicon nitride ceramic pieces is controlled, and finally silicon nitride ceramic pieces with fewer surface defects, uniform thickness, low warpage, high thermal conductivity, and high peeling strength are obtained, which have a wider range of applications in the semiconductor field. DETAILED DESCRIPTION

[0036] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.

[0037] In this embodiment, it should be noted that the purchase manufacturers of all raw materials involved in the present invention are not subject to any special restrictions, and exemplary examples include: α-silicon nitride with a purity of 99.9%, CAS number: 12033-89-5, item number: B-Si3N4-800N, model: 20nm, purchased from Ningbo Yutian Materials Technology Co., Ltd.; short carbon fiber with an aspect ratio of 100:1 and a carbon content of >98%, purchased from Shenzhen Feige Fiber Materials Co., Ltd.; silicon carbide whiskers with a purity of 99% and an aspect ratio of 20:1, purchased from Guangzhou Hongwu Materials Technology Co., Ltd.; anhydrous hydrofluoric acid with a purity of 99.99 %, item number: 2023-8-26, purchased from Shandong Xingshi Chemical Sales Co., Ltd.; dichlorothionyl with a purity of 99% was purchased from Wuhan Beiguofeng Chemical Co., Ltd.; 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane with a purity of 99% was purchased from Hubei Yongkuo Technology Co., Ltd.; aluminum oxide, yttrium oxide, lanthanum oxide, magnesium oxide, boron oxide, lithium oxide, and zinc oxide with a purity of 99.9% were purchased from Yumu (Ningbo) New Materials Co., Ltd.; polyvinyl alcohol with a purity of 99.99% was purchased from Shanghai Yuanye Biotechnology Co., Ltd.; In addition, it should be noted that in the following implementation manner, parts are parts by mass.

[0038] Example 1: A ground silicon nitride ceramic wafer:

[0039] Step 1: (1) Preparation of modified toughening material: 1) Soaking 20 parts of toughening material (chopped carbon fiber and silicon carbide whisker mixed in a mass ratio of 5:1) in 320 parts of 30wt% hydrofluoric acid solution for 30h, filtering, washing and drying to obtain acid-treated toughening material; 2) Soaking 20 parts of acid-treated toughening material in 320 parts of 30wt% hydrogen peroxide for 1h, filtering, washing and drying to obtain carboxyl toughening material; 3) Adding 20 parts of carboxyl toughening material and 400 parts of thionyl chloride into a reaction vessel, at 25°C, at 55°C, 0r / min, stirring and reacting for 25min, then heating to 55°C, continuing stirring and reacting for 18h, terminating the reaction, and finally removing excess thionyl chloride by rotary evaporation to obtain an acyl chloride toughening material; 4) adding 20 parts of the acyl chloride toughening material, 1.6 parts of 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane, and 400 parts of toluene into a reaction container, stirring and reacting at 45°C and 550r / min for 15min in a nitrogen atmosphere, and then refluxing for 5h, terminating the reaction, filtering, washing, and drying to obtain a modified toughening material;

[0040] (2) Alumina, yttrium oxide, lanthanum oxide, and magnesium oxide are mixed uniformly in a mass ratio of 3:2:2:1 to obtain a first sintering aid; boron oxide, lithium oxide, and zinc oxide are mixed uniformly in a mass ratio of 1:1:2 to obtain a second sintering aid; the first sintering aid and the second sintering aid are mixed uniformly in a mass ratio of 2:1 to obtain a sintering aid;

[0041] (3) adding 100 parts of α-silicon nitride, 20 parts of modified toughening material, and 15 parts of sintering aid to 200 parts of 20 wt% polyvinyl alcohol solution, and ball milling at a speed of 300 r / min for 48 hours to obtain a dispersion;

[0042] Step 2: (1) Centrifuge the dispersion, filter out the precipitate, heat it to 90°C to dry it, grind it, and sieve it to obtain D 50 Powder with particle size of 0.5μm;

[0043] (2) placing the powder in a mold, pressing it under a pressure of 150 MPa, and keeping it at 500° C. for 2 h to obtain a silicon nitride ceramic body;

[0044] Step 3: Place the silicon nitride ceramic body on the silicon carbide sheet auxiliary heating device and place it in the heat preservation device in the microwave sintering furnace. At a microwave frequency of 2.45 GHz, use nitrogen as the protective gas, control the gas pressure in the sintering chamber to be 0.3 MPa, heat up to 1550°C at a heating rate of 15°C / min, keep warm for 30 minutes, and finally cool the furnace to obtain a 400 μm thick silicon nitride ceramic;

[0045] Step 4: (1) Grind the silicon nitride ceramic on both sides with a 1000-mesh sander, grind each side to 15 μm, and grind both sides to the same thickness to obtain ground ceramic; (2) Place the ground ceramic in a microwave sintering furnace, set the microwave sintering parameters: microwave frequency is 2.45 GHz, nitrogen is used as the protective gas, the air pressure in the sintering chamber is 0.3 MPa, heat up to 1300°C at a heating rate of 2°C / min, and keep warm for 20 minutes; after the insulation is completed, the furnace is cooled to room temperature to obtain re-fired ceramic; (3) Grind the re-fired ceramic again with a 1000-mesh sander, grind both sides to the same thickness, and obtain a 320 μm thick silicon nitride ceramic sheet.

[0046] Example 2: A ground silicon nitride ceramic wafer:

[0047] Step 1: (1) Preparation of modified toughening material: 1) Soaking 20 parts of toughening material (chopped carbon fiber and silicon carbide whisker mixed in a mass ratio of 5:1) in 300 parts of 25wt% hydrofluoric acid solution for 24 hours, filtering, washing and drying to obtain an acid-treated toughening material; 2) Soaking 20 parts of the acid-treated toughening material in 300 parts of 25wt% hydrogen peroxide for 1 hour, filtering, washing and drying to obtain a carboxylated toughening material; 3) Adding 20 parts of the carboxylated toughening material and 400 parts of thionyl chloride into a reaction vessel, at 25°C for 5 minutes, After stirring at a speed of 50 r / min for 25 minutes, the temperature was raised to 55°C, and the stirring reaction was continued for 18 hours, the reaction was terminated, and finally the excess dithionyl chloride was removed by rotary evaporation to obtain an acyl chloride toughening material; 4) 20 parts of the acyl chloride toughening material, 1 part of 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane, and 400 parts of toluene were added to a reaction container, stirred at 45°C and 550 r / min for 15 minutes in a nitrogen atmosphere, and then refluxed for 5 hours to terminate the reaction, filtered, washed, and dried to obtain a modified toughening material;

[0048] (2) Alumina, yttrium oxide, lanthanum oxide, and magnesium oxide are mixed uniformly in a mass ratio of 3:2:2:1 to obtain a first sintering aid; boron oxide, lithium oxide, and zinc oxide are mixed uniformly in a mass ratio of 1:1:2 to obtain a second sintering aid; the first sintering aid and the second sintering aid are mixed uniformly in a mass ratio of 2:1 to obtain a sintering aid;

[0049] (3) adding 100 parts of α-silicon nitride, 10 parts of modified toughening material, and 15 parts of sintering aid to 200 parts of 20 wt % polyvinyl alcohol solution, and mixing by ball milling at a speed of 300 r / min for 48 hours to obtain a dispersion;

[0050] Step 2: (1) Centrifuge the dispersion, filter out the precipitate, heat it to 90°C to dry it, grind it, and sieve it to obtain D 50 Powder with particle size of 0.5μm;

[0051] (2) placing the powder in a mold, pressing it under a pressure of 150 MPa, and keeping it at 500° C. for 2 h to obtain a silicon nitride ceramic body;

[0052] Step 3: Place the silicon nitride ceramic body on the silicon carbide sheet auxiliary heating device and place it in the heat preservation device in the microwave sintering furnace. At a microwave frequency of 2.45 GHz, use nitrogen as the protective gas, control the gas pressure in the sintering chamber to be 0.3 MPa, heat up to 1550°C at a heating rate of 15°C / min, keep warm for 30 minutes, and finally cool the furnace to obtain a 400 μm thick silicon nitride ceramic;

[0053] Step 4: (1) Grind the silicon nitride ceramic on both sides with a 400-mesh sander, grind each side to 15 μm, and grind both sides to the same thickness to obtain ground ceramic; (2) Place the ground ceramic in a microwave sintering furnace, set the microwave sintering parameters: microwave frequency is 2.45 GHz, nitrogen is used as the protective gas, the air pressure in the sintering chamber is 0.3 MPa, heat up to 1300°C at a heating rate of 2°C / min, and keep warm for 20 minutes; after the insulation is completed, the furnace is cooled to room temperature to obtain re-fired ceramic; (3) Grind the re-fired ceramic again with a 400-mesh sander, grind both sides to the same thickness, and obtain a 320 μm thick silicon nitride ceramic sheet.

[0054] Example 3: A ground silicon nitride ceramic wafer:

[0055] Step 1: (1) Preparation of modified toughening material: 1) Soaking 20 parts of toughening material (chopped carbon fiber and silicon carbide whisker mixed in a mass ratio of 5:1) in 320 parts of 30wt% hydrofluoric acid solution for 48 hours, filtering, washing and drying to obtain acid-treated toughening material; 2) Soaking 20 parts of acid-treated toughening material in 320 parts of 30wt% hydrogen peroxide for 2 hours, filtering, washing and drying to obtain carboxyl toughening material; 3) Adding 20 parts of carboxyl toughening material and 400 parts of thionyl chloride into a reaction vessel, at 25°C, at 55°C, 0r / min, stirring and reacting for 25min, then heating to 55°C, continuing stirring and reacting for 18h, terminating the reaction, and finally removing excess thionyl chloride by rotary evaporation to obtain an acyl chloride toughening material; 4) adding 20 parts of the acyl chloride toughening material, 1.6 parts of 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane, and 400 parts of toluene into a reaction container, stirring and reacting at 45°C and 550r / min for 15min in a nitrogen atmosphere, and then refluxing for 5h, terminating the reaction, filtering, washing, and drying to obtain a modified toughening material;

[0056] (2) Alumina, yttrium oxide, lanthanum oxide, and magnesium oxide are mixed uniformly in a mass ratio of 3:2:2:1 to obtain a first sintering aid; boron oxide, lithium oxide, and zinc oxide are mixed uniformly in a mass ratio of 1:1:2 to obtain a second sintering aid; the first sintering aid and the second sintering aid are mixed uniformly in a mass ratio of 2:1 to obtain a sintering aid;

[0057] (3) adding 100 parts of α-silicon nitride, 25 parts of modified toughening material, and 15 parts of sintering aid to 200 parts of 20 wt % polyvinyl alcohol solution, and mixing by ball milling at a speed of 300 r / min for 48 hours to obtain a dispersion;

[0058] Step 2: (1) Centrifuge the dispersion, filter out the precipitate, heat it to 90°C to dry it, grind it, and sieve it to obtain D50 Powder with particle size of 0.5μm;

[0059] (2) placing the powder in a mold, pressing it under a pressure of 150 MPa, and keeping it at 500° C. for 2 h to obtain a silicon nitride ceramic body;

[0060] Step 3: Place the silicon nitride ceramic body on the silicon carbide sheet auxiliary heating device and place it in the heat preservation device in the microwave sintering furnace. At a microwave frequency of 2.45 GHz, use nitrogen as the protective gas, control the gas pressure in the sintering chamber to be 0.3 MPa, heat up to 1550°C at a heating rate of 15°C / min, keep warm for 30 minutes, and finally cool the furnace to obtain a 400 μm thick silicon nitride ceramic;

[0061] Step 4: (1) Grind the silicon nitride ceramic on both sides with a 1000-mesh sander, grind each side to 15 μm, and grind both sides to the same thickness to obtain ground ceramic; (2) Place the ground ceramic in a microwave sintering furnace, set the microwave sintering parameters: microwave frequency is 2.45 GHz, nitrogen is used as the protective gas, the air pressure in the sintering chamber is 0.3 MPa, heat up to 1300°C at a heating rate of 2°C / min, and keep warm for 20 minutes; after the insulation is completed, the furnace is cooled to room temperature to obtain re-fired ceramic; (3) Grind the re-fired ceramic again with a 1000-mesh sander, grind both sides to the same thickness, and obtain a 320 μm thick silicon nitride ceramic sheet.

[0062] Based on Example 1, a control experiment was carried out, specifically Comparative Examples 1 to 5, as described below:

[0063] Comparative Example 1: The following adjustments were made to Comparative Example 1: the toughening material was directly added without modification, and the other processes remained unchanged, specifically:

[0064] (1) Alumina, yttrium oxide, lanthanum oxide, and magnesium oxide are mixed uniformly in a mass ratio of 3:2:2:1 to obtain a first sintering aid; boron oxide, lithium oxide, and zinc oxide are mixed uniformly in a mass ratio of 1:1:2 to obtain a second sintering aid; the first sintering aid and the second sintering aid are mixed uniformly in a mass ratio of 2:1 to obtain a sintering aid;

[0065] (2) adding 100 parts of α-silicon nitride, 20 parts of a toughening material (chopped carbon fiber and silicon carbide whisker mixed in a mass ratio of 5:1), and 15 parts of a sintering aid to 200 parts of a 20 wt % polyvinyl alcohol solution, and ball milling at a speed of 300 r / min for 48 h to obtain a dispersion;

[0066] Comparative Example 2: The following adjustments were made to Comparative Example 2: no toughening material was added, and the remaining processes remained unchanged, specifically:

[0067] (1) Alumina, yttrium oxide, lanthanum oxide, and magnesium oxide are mixed uniformly in a mass ratio of 3:2:2:1 to obtain a first sintering aid; boron oxide, lithium oxide, and zinc oxide are mixed uniformly in a mass ratio of 1:1:2 to obtain a second sintering aid; the first sintering aid and the second sintering aid are mixed uniformly in a mass ratio of 2:1 to obtain a sintering aid;

[0068] (2) adding 100 parts of α-silicon nitride and 15 parts of a sintering aid to 200 parts of a 20 wt % polyvinyl alcohol solution, and ball milling at a speed of 300 r / min for 48 hours to obtain a dispersion;

[0069] Comparative Example 3: The comparative example 3 is adjusted as follows: the conventional sintering method is used for sintering, and other processes remain unchanged, specifically:

[0070] Step 3: Place the silicon nitride ceramic body into a sintering furnace, heat it to 1550°C at a heating rate of 15°C / min, keep it warm for 30 hours, and finally cool it in the furnace to obtain a 400μm thick silicon nitride ceramic;

[0071] Step 4: (1) Grind the silicon nitride ceramic on both sides once with a 400-mesh sander, grind each side to 15 μm, and grind both sides to the same thickness to obtain ground ceramic; (2) Place the ground ceramic in a sintering furnace, heat it to 1300°C at a heating rate of 2°C / min, and keep it warm for 24 hours; after the insulation is completed, cool the furnace to room temperature to obtain a re-fired ceramic; (3) Grind the re-fired ceramic again with a 400-mesh sander, grind both sides to the same thickness, and obtain a 320 μm thick silicon nitride ceramic sheet.

[0072] Comparative Example 4: Comparative Example 4 is adjusted as follows: the silicon nitride ceramic is ground only once, and no re-firing is performed. Other processes remain unchanged, specifically:

[0073] Step 4: (1) Grind the silicon nitride ceramic on both sides once using a 400-mesh sander, grinding each side by 40 μm, and grinding both sides to the same thickness to obtain a 320 μm thick silicon nitride ceramic sheet.

[0074] Comparative Example 5: The following is an adjustment in Comparative Example 5: the silicon nitride ceramic is not ground, and other processes remain unchanged.

[0075] Testing experiment: The performance of the silicon nitride ceramic sheets prepared in Examples 1 to 3 and Comparative Examples 1 to 5 was tested, specifically:

[0076] (1) Density test:

[0077] (2) According to the test method in GB / T4741-1999 "Test Method for Flexural Strength of Ceramic Materials", the flexural strength of silicon nitride ceramics was tested;

[0078] (3) According to the test method in GB / T 39862-2021 "Testing of thermal conductivity of high thermal conductivity ceramics", the thermal conductivity of silicon nitride ceramics was tested; the specific test results are shown in Table 1 below:

[0079] Table 1

[0080]

[0081] Analysis of results: From the data in Table 1 above, it can be seen that the addition and modification of the toughening material (chopped carbon fiber and silicon carbide whisker) in the present invention has a positive effect on the performance of silicon nitride ceramics. Comparative Examples 1 and 2 show that the density, flexural strength and thermal conductivity are significantly improved; Comparative Example 3 shows that the scheme uses microwave sintering to slightly improve the relevant properties of silicon nitride; Comparative Example 4 shows that the scheme uses a small amount of multiple grinding, plus re-firing to eliminate cracks, and the obtained ceramic piece has better performance; Comparative Example 5, combined with Comparative Example 2, it can be seen that grinding has a great negative impact on the flexural strength of silicon nitride ceramics, but the toughening material can significantly compensate for the loss of flexural strength caused by grinding, and a small amount of multiple grinding plus re-firing also promotes the density and thermal conductivity of silicon nitride ceramics.

[0082] In summary, the silicon nitride ceramic sheet prepared by the present invention has better bending strength (i.e. better toughness and less brittleness), higher density and thermal conductivity, and is more widely applicable in semiconductors.

[0083] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.

Claims

1. A ground silicon nitride ceramic wafer, characterized in that: The preparation of the silicon nitride ceramic sheet comprises the following preparation steps: Step 1: Add α-silicon nitride, modified toughening material and sintering aid into the solvent, and mix by ball milling at a speed of 100-500 r / min for 24-72 hours to obtain a dispersion; Step 2: (1) centrifuging the dispersion, filtering out the precipitate, heating it to 80-100°C for drying, grinding it, and sieving it to obtain a powder; (2) placing the powder in a mold, pressing it under a pressure of 100-200 MPa, and keeping it at 400-600°C for 1-3 hours to obtain a silicon nitride ceramic body; Step 3: Sintering the silicon nitride ceramic body by microwave to obtain silicon nitride ceramic; Step 4: (1) Grind the silicon nitride ceramic on both sides once with a 400-1000 mesh sander, grind both sides to the same thickness, and obtain ground ceramic; (2) Place the ground ceramic in a microwave sintering furnace, set the microwave sintering parameters: microwave frequency is 2.45 GHz, nitrogen is used as the protective gas, the gas pressure in the sintering chamber is 0.1-0.5 MPa, the heating rate is 1-5 °C / min, the sintering temperature is 1100-1500 °C, and the insulation time is 10-30 min; after the insulation is completed, the furnace is cooled to room temperature to obtain a re-fired ceramic; (3) Grind the re-fired ceramic again with a 400-1000 mesh sander, grind both sides to the same thickness, and obtain a silicon nitride ceramic sheet; The preparation method of the modified toughening material is as follows: (1) soaking the toughening material in a 25-35wt% hydrofluoric acid solution for 24-48 hours, filtering, washing and drying to obtain an acid-treated toughening material; (2) soaking the acid-treated toughening material in a 25-35wt% hydrogen peroxide solution for 1-2 hours, filtering, washing and drying to obtain a carboxyl toughening material; (3) adding the carboxyl toughening material and thionyl chloride into a reaction container, stirring the reaction at 20-30°C and a speed of 500-600 r / min for 1 hour. After 0-30 minutes, the temperature is raised to 50-60°C, and the reaction is continued with stirring for 12-24 hours. The reaction is terminated, and finally the excess thionyl chloride is removed by rotary evaporation to obtain an acyl chloride toughening material; (4) the acyl chloride toughening material, the silane coupling agent with a hydroxyl group, and toluene are added to a reaction container, and the reaction is stirred at 40-50°C and a speed of 500-600 r / min for 10-20 minutes in a nitrogen atmosphere, and then refluxed for 3-6 hours to terminate the reaction. After filtering, washing, and drying, a modified toughening material is obtained; The toughening material is a toughening material composed of chopped carbon fibers and silicon carbide whiskers in a mass ratio of 5:1; the aspect ratio of the chopped carbon fibers is 100:1, and the aspect ratio of the silicon carbide whiskers is 20:1; the mass ratio of the toughening material and the hydrofluoric acid solution is 1:(15-20); the mass ratio of the acid-treated toughening material and hydrogen peroxide is 1:(15-20); the mass ratio of the carboxyl toughening material and dichlorothionyl is 1:20; the mass ratio of the acyl chloride toughening material, the hydroxyl-containing silane coupling agent, and toluene is 1:(0.05-0.1):20; the hydroxyl-containing silane coupling agent includes a combination of one or more of 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane, 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, and tert-butyldimethylhydroxyethoxysilane; The sintering aid is obtained by mixing a first sintering aid and a second sintering aid in a mass ratio of (4-8):(3-6); wherein the first sintering aid is obtained by mixing aluminum oxide, yttrium oxide, lanthanum oxide, and magnesium oxide in a mass ratio of 3:2:2:1; and the second sintering aid is obtained by mixing boron oxide, lithium oxide, and zinc oxide in a mass ratio of 1:1:2; The mass ratio of the α-silicon nitride, the modified toughening material and the sintering aid is 100:(10-25):(5-20); The thickness of the ground ceramic is 0.36-0.38 mm; the thickness of the silicon nitride ceramic piece is 0.32 mm; and the total thickness lost after the first double-sided grinding and the second double-sided grinding is ≥80 μm.

2. A ground silicon nitride ceramic sheet according to claim 1, characterized in that: The solvent is obtained by mixing deionized water and polyvinyl alcohol in a mass ratio of 4:

1.

3. A ground silicon nitride ceramic sheet according to claim 1, characterized in that: The parameters of the microwave sintering are as follows: microwave frequency is 2.45 GHz, nitrogen is used as protective gas, the gas pressure in the sintering chamber is 0.1-0.5 MPa, the heating rate is 10-20° C. / min, the sintering temperature is 1500-1600° C., and the holding time is 10-40 min.

4. A ground silicon nitride ceramic sheet according to claim 1, characterized in that: The powder, after drying, contains 5 to 10% solvent; after grinding, its D 50 The particle size is 0.5~1μm.