A method for manufacturing a flexible perovskite photovoltaic module with high flatness
Through the lamination technology of electrostatic adsorption protective film and thermoplastic solid film, the problem of difficult to ensure the flatness of flexible perovskite photovoltaic modules during the manufacturing process is solved, and high-quality and efficient module production is achieved.
Patent Information
- Application Number
- CN202410680922.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-29
AI Technical Summary
During the manufacturing process, flexible perovskite photovoltaic modules are difficult to maintain flatness due to the flexibility and ductility of the substrate, resulting in bubbles, defects and uneven coating problems in the process, affecting the quality of the component.
The lamination technology of flexible substrates and thermoplastic solid films using electrostatic adsorption protective films is ensured to have a smooth bond between the flexible substrate and the rigid substrate through the combination of pre-pressed parts and high-temperature cloth, and a soft and hard bond is formed by lamination. , ensure the consistency of the perovskite film layer.
It effectively avoids the flatness problem of flexible substrates, improves the quality and production efficiency of perovskite photovoltaic modules, and ensures the uniformity of the functional layer and the elasticity of the product.
Smart Images

Figure CN118251104B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photovoltaic technology, and in particular to a method for manufacturing a flexible perovskite photovoltaic module with high flatness. Background Art
[0002] Flexible perovskite photovoltaic modules are prepared on flexible substrate materials. Commonly used materials are generally PET, PEN, polyimide (PI), etc. Because of the softness of the materials and their certain ductility, it is very difficult to directly adopt roll-to-roll continuous production. Directly cutting the flexible substrate materials into independent units in the preparation and processing of perovskite film layers has serious problems, such as the fixation of substrate materials before the process: to prevent it from moving and offset, vacuum adsorption is usually used, but because of the flexibility of the material, there will be obvious deformation at the vacuum adsorption hole, which will affect the corresponding process, such as vacuum coating, laser scribing, perovskite film slit coating or spin coating. At present, the industry usually fixes the flexible substrate material on the rigid substrate material, and then carries out the perovskite photovoltaic preparation process (vacuum coating, laser scribing, perovskite coating, etc.). For this reason, the flexible substrate material is usually fixed on the rigid substrate (glass and other materials) by gluing. Common methods include: fixing it around with tape, applying glue on the surface of the rigid substrate and then gluing the flexible substrate material.
[0003] Chinese patent CN116406216A discloses a method of fixing by adhesive tape. However, since the substrate is relatively large and flexible, it may sag or bulge in the middle due to its ductility, and the flatness of the surface of the flexible substrate cannot be guaranteed.
[0004] By applying glue on the surface of a rigid substrate and then pasting the flexible substrate material, bubbles will exist in the solution. Especially in large-area preparation, the bubble problem is more prominent and cannot be fundamentally solved. The presence of bubbles and other conditions makes it impossible to guarantee the flatness of the surface of the flexible substrate material.
[0005] The inability to ensure the flatness of the flexible substrate surface will lead to the inability to proceed normally with related processes. For example, the laser scribing in Chinese patent CN117750849A may not be able to cut through the lines. Slit coating will have a large number of defects because the consistency of the distance between the coating head and the substrate cannot be guaranteed. Spin coating cannot obtain a uniform perovskite film layer.
[0006] Therefore, it is necessary to design a new manufacturing method to avoid the above problems. Summary of the invention
[0007] The main purpose of the present invention is to provide a method for manufacturing a flexible perovskite photovoltaic module with high flatness, which can ensure the flatness of the flexible substrate after bonding with the rigid substrate, ensure the consistency of the perovskite film layer in subsequent manufacturing, and improve the quality of the flexible perovskite photovoltaic module.
[0008] The present invention achieves the above-mentioned purpose through the following technical solution: a method for manufacturing a flexible perovskite photovoltaic module with high flatness, the steps comprising:
[0009] S1. Soft board filming: Use electrostatic adsorption to stick a layer of protective film on both sides of the flexible substrate to form a soft board with film;
[0010] S2, pre-lamination of soft and hard boards: stacking one rigid substrate, one thermoplastic solid adhesive film, two soft boards with films, another thermoplastic solid adhesive film and another rigid substrate in this order, and then fixing the outer surface edges of the two rigid substrates with adhesive tape to form a pre-pressed part, wherein the protective film in contact with the thermoplastic solid adhesive film is defined as the A-side protective film, and the protective film on the other side is defined as the B-side protective film, and the length and width of the rigid substrate are smaller than the length and width of the flexible substrate;
[0011] S3, lamination: a support bar with a height greater than the thickness of the pre-pressed part is arranged around the side of the pre-pressed part, and a high-temperature cloth is arranged on the upper and lower surfaces of the pre-pressed part, and the range of the high-temperature cloth exceeds the range of the support bar. The range of the support bar is laminated by a silicone plate, and the thermoplastic solid adhesive film is melted by heating to bond the rigid substrate and the A-side protective film together;
[0012] S4, disassembling the board: taking out the pre-pressed part, tearing off the tape, and cutting off the excess part of the film-coated soft board beyond the edge of the rigid substrate to obtain two soft-hard combinations, wherein the soft-hard combinations are composed of the rigid substrate, the thermoplastic solid adhesive film, the A-side protective film, the flexible substrate and the B-side protective film;
[0013] S5, functional layer manufacturing: peeling off the B-side protective film of the soft-hard combination body, manufacturing various functional layers of the photovoltaic module on the B-side of the flexible substrate, and obtaining a flexible perovskite photovoltaic module with a rigid substrate;
[0014] S6, peeling: tearing off the flexible perovskite photovoltaic module from the A-side protective film, leaving the A-side protective film on the rigid substrate.
[0015] Specifically, the material of the thermoplastic solid adhesive film is selected from POE, PVB, EVA or EPE.
[0016] Specifically, the size of the rigid substrate is 1 mm larger than the size of the thermoplastic solid adhesive film, and the size of the flexible substrate is 1 mm larger than the size of the rigid substrate.
[0017] Specifically, in step S4, the lamination pressure is 100 kPa, the lamination time is 20-30 min, the lamination temperature is 90-160° C., and the number of lamination process stages is 1-10.
[0018] The beneficial effects of the technical solution of the present invention are:
[0019] The present invention first pastes a protective film on both sides of the flexible substrate to form a film-coated soft board, then sandwiches two thermoplastic solid adhesive films and two film-coated soft boards between two rigid substrates, and fixes them as pre-pressed parts with adhesive tapes. The pre-pressed parts are then surrounded by support strips and two high-temperature cloths and heated and laminated, so that the rigid substrate and the A-side protective film are adhered together, and two soft-hard combinations are formed after the boards are removed. After the B-side protective film is peeled off, various functional layers are plated on the flexible substrate, and finally the flexible perovskite photovoltaic module is torn off from the A-side protective film. The flatness of the flexible substrate on the rigid substrate is ensured by a special lamination method, and the two soft-hard combinations are manufactured quickly at the same time, which can not only ensure product quality, but also improve production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a three-dimensional diagram of a pre-pressed part;
[0021] Figure 2 is a stack-up diagram of the pre-pressed part;
[0022] Figure 3 This is the lamination schematic diagram;
[0023] Figure 4 It is a stacking diagram of a hard-soft combination;
[0024] Figure 5 A stackup diagram of a flexible perovskite photovoltaic module with a rigid substrate;
[0025] Figure 6 A diagram of the stacking of flexible perovskite photovoltaic modules.
[0026] The markings in the figure are:
[0027] 1-flexible substrate, 2a-A surface protection film, 2b-B surface protection film, 3-rigid substrate, 4-thermoplastic solid adhesive film, 5-adhesive tape, 6-support strip, 7-high temperature cloth, 8-silicone plate, 9-functional layer. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below with reference to specific embodiments.
[0029] Example:
[0030] The following steps are used to passivate the nickel oxide hole transport layer of large-area perovskite cells:
[0031] S1. Soft board filming: A layer of protective film (A side protective film 2a, B side protective film 2b) is pasted on both sides AB of the flexible substrate 1 by electrostatic adsorption to form a film-coated soft board.
[0032] The A-side protective film 2a and the B-side protective film 2b can be fully laminated to the flexible substrate 1, and bubbles between the surfaces can be easily exhausted, thereby protecting the surface of the flexible substrate 1 and avoiding scratches or contamination.
[0033] S2. Pre-lamination of soft and hard boards: stack a rigid substrate 3, a thermoplastic solid adhesive film 4, two soft boards with films, another thermoplastic solid adhesive film 4 and another rigid substrate 3 in this order, and then fix the outer surface edges of the two rigid substrates 3 with tape 5 to form a pre-pressed part, wherein the protective film in contact with the thermoplastic solid adhesive film 4 is defined as the A-side protective film 2a, and the protective film on the other side is defined as the B-side protective film 2b, and the length and width of the rigid substrate 3 are smaller than the length and width of the flexible substrate 1.
[0034] Thermoplastic solid adhesive film 4 is an adhesive film that melts and becomes sticky after heating, and solidifies after cooling to connect the materials on both sides together. It is an elastic solid at room temperature. In order to keep the flexible substrate 1 flat during the functional layer manufacturing 9, the rigid substrate 3 must support the outside of the flexible substrate 1, so the two need to be temporarily bonded. It is also necessary to reduce the wrinkles caused by the thermal expansion and contraction of the flexible substrate 1 material, so the rigid substrate 3 and the A-side protective film 2a need to be connected together with an adhesive film, because the rigid substrate 3 is less affected by heat and can be basically regarded as unchanged. When the two rigid substrates 3 press the two flexible substrates 1 together, the two flexible substrates 1 will remain flat. The tape 5 here can prevent the pre-pressed parts from disintegrating during lamination.
[0035] In this embodiment, the size of the rigid substrate 3 is 1 mm larger than the size of the thermoplastic solid adhesive film 4, and the size of the flexible substrate 1 is 1 mm larger than the size of the rigid substrate 3. Because the edge of the flexible substrate 1 is the range that needs to be trimmed, and the retained portion of the flexible substrate 1 corresponds to the range of the rigid substrate 3, the size of the flexible substrate 1 is appropriately larger than that of the rigid substrate 3. When the thermoplastic solid adhesive film 4 is squeezed during melting, the thickness decreases, and the corresponding range will increase and then cover the gap between the flexible substrate 1 and the rigid substrate 3, and a part of it will leak to the outside of the rigid substrate 3, which needs to be removed. Therefore, the size of the thermoplastic solid adhesive film 4 only needs to be appropriately smaller than the rigid substrate 3. Any more will be a waste, which can save material costs.
[0036] S3, lamination: a support bar 6 with a height greater than the thickness of the pre-pressed part is arranged around the side of the pre-pressed part, and a high temperature cloth 7 is arranged on the upper and lower surfaces of the pre-pressed part, and the range of the high temperature cloth 7 exceeds the range of the support bar 6. The range of the support bar 6 is laminated by the silicone plate 8, and the thermoplastic solid adhesive film 4 is heated to melt and the rigid substrate 3 and the A-side protective film 2a are bonded together. Step S4 lamination pressure is 100kPa, lamination time is 20-30min, lamination temperature is 90-160℃, and the number of lamination process stages is 1-10.
[0037] The silicone plate 8 is a flat plate with elasticity, used as the upper and lower pressing plates in the laminator, thereby sandwiching the pre-pressed part in the middle. Because the surface of the silicone plate 8 is flat, the two clamped rigid substrates 3 will be in a parallel relationship under ideal conditions. Although the two flexible substrates 1 are separated by two layers of B-surface protective films 2b, they will remain flat because they are closely attached to each other. In the process of being pressed and heated, the thermoplastic solid adhesive film 4 will first melt into a fluid, and form an adhesive layer of uniform thickness under appropriate pressure. If the support strip 6 is not used, the silicone plate 8 will form an oblique force at the position where it contacts the rigid substrate 3 due to the concave deformation. This oblique force will make the pressure near the edge of the rigid substrate 3 greater, so the thermoplastic solid film 4 and the flexible substrate 1 at this position will be pressed thinner than the middle position, which is not conducive to product quality; the support strip 6 can make this oblique force act on the outside of the support strip 6 instead of on the rigid substrate 3, so the surface of the entire rigid substrate 3 is only subjected to downward pressure, ensuring that the thickness of the thermoplastic solid film 4 and the flexible substrate 1 is uniform, thereby improving product quality. The high-temperature cloth 7 can prevent the silicone plate 8 from sticking to the rigid substrate 3, making it easier to separate the silicone plate 8 from the pre-pressed part when opening the mold, and also avoiding the risk of the rigid substrate 3 being fragmented and cracked and puncturing the silicone plate 8.
[0038] S5, dismantling the board: take out the pre-pressed part, tear off the tape 5, and cut off the excess part of the film-coated soft board that exceeds the edge of the rigid substrate 3 to obtain two soft-hard combinations, which are composed of a rigid substrate 3, a thermoplastic solid adhesive film 4, an A-side protective film 2a, a flexible substrate 1 and a B-side protective film 2b.
[0039] Lamination only makes the rigid substrate 3 and the A-side protective film 2a adhere together through the thermoplastic solid adhesive film 4, while the two B-side protective films 2b will not adhere to each other. Therefore, after the pre-pressed parts are disassembled, two soft-hard combinations with symmetrical positions can be formed.
[0040] S6, functional layer manufacturing: peel off the B-side protective film 2b of the soft-hard combination, and manufacture various functional layers 9 of the photovoltaic module on the B-side of the flexible substrate 1 to obtain a flexible perovskite photovoltaic module with a rigid substrate 3.
[0041] After lamination, the B-side protective film 2b has completed the protection of the flexible substrate 1, and the B-side of the flexible substrate 1 needs to manufacture the functional layer 9 of the photovoltaic module, so it must be torn off first. The manufacturing steps of the functional layer 9 include coating, laser scribing, perovskite coating, etc. The rigid substrate 3 can keep the flexible substrate 1 flat in this step, and each soft-hard combination is manufactured by the same method. Functional layer 9.
[0042] S7, peeling: tearing off the flexible perovskite photovoltaic module from the A-side protective film 2a, leaving the A-side protective film 2a on the rigid substrate 3.
[0043] The rigid substrate 3 and the A-side protective film 2a are not part of the flexible perovskite photovoltaic module, so after the functional layer 9 is plated, the rigid substrate 3 and the A-side protective film 2a need to be removed. The flexible substrate 1 will maintain good elasticity after being plated with the functional layer 9, so the flexible substrate 1 can be peeled off.
[0044] The present invention ensures the flatness of the flexible substrate 1 on the rigid substrate 3 through a special lamination method, and manufactures two soft-hard combinations quickly, which can ensure product quality and improve production efficiency.
[0045] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for manufacturing a high-flatness flexible perovskite photovoltaic module, characterized in that the steps include: S1. Soft board filming: Use electrostatic adsorption to stick a layer of protective film on both sides of the flexible substrate to form a soft board with film; S2, pre-lamination of soft and hard boards: stacking one rigid substrate, one thermoplastic solid adhesive film, two soft boards with films, another thermoplastic solid adhesive film and another rigid substrate in this order, and then fixing the outer surface edges of the two rigid substrates with adhesive tape to form a pre-pressed part, wherein the protective film in contact with the thermoplastic solid adhesive film is defined as the A-side protective film, and the protective film on the other side is defined as the B-side protective film, and the length and width of the rigid substrate are smaller than the length and width of the flexible substrate; S3, lamination: a support bar with a height greater than the thickness of the pre-pressed part is arranged around the side of the pre-pressed part, and a high-temperature cloth is arranged on the upper and lower surfaces of the pre-pressed part, and the range of the high-temperature cloth exceeds the range of the support bar. The range of the support bar is laminated by a silicone plate, and the thermoplastic solid adhesive film is melted by heating to bond the rigid substrate and the A-side protective film together; S4, disassembling the board: taking out the pre-pressed part, tearing off the tape, and cutting off the excess part of the film-coated soft board beyond the edge of the rigid substrate to obtain two soft-hard combinations, wherein the soft-hard combinations are composed of the rigid substrate, the thermoplastic solid adhesive film, the A-side protective film, the flexible substrate and the B-side protective film; S5, functional layer manufacturing: peeling off the B-side protective film of the soft-hard combination body, manufacturing various functional layers of the photovoltaic module on the B-side of the flexible substrate, and obtaining a flexible perovskite photovoltaic module with a rigid substrate; S6, peeling: tearing off the flexible perovskite photovoltaic module from the A-side protective film, leaving the A-side protective film on the rigid substrate.
2. The method for manufacturing a high-flatness flexible perovskite photovoltaic module according to claim 1, characterized in that: The material of the thermoplastic solid adhesive film is selected from POE, PVB, EVA or EPE.
3. The method for manufacturing a high-flatness flexible perovskite photovoltaic module according to claim 1, characterized in that: The size of the rigid substrate is 1 mm larger than that of the thermoplastic solid adhesive film, and the size of the flexible substrate is 1 mm larger than that of the rigid substrate.
4. The method for manufacturing a high-flatness flexible perovskite photovoltaic module according to claim 1, characterized in that: The lamination pressure in step S4 is 100 kPa, the lamination time is 20-30 min, the lamination temperature is 90-160° C., and the number of lamination process stages is 1-10.