Semi-continuous casting pipe crystallizer and pipe manufacturing method
Through the dual cooling system of semi-continuous cast pipe crystallizer, the problems of complex and high cost of traditional copper tube manufacturing processes are solved, and efficient production and strength improvement of large-diameter copper tubes are achieved.
Patent Information
- Application Number
- CN202311240251.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-09-22
AI Technical Summary
Traditional copper tube manufacturing methods are complex and expensive, making it difficult to produce copper tubes with large diameters and good strength.
The semi-continuous cast pipe crystallizer is adopted to achieve rapid solidification and strength improvement of copper raw materials through a dual cooling system of cooling medium and cooling water, simplify the manufacturing process and reduce costs.
The ability to produce large diameter copper pipes is realized, the manufacturing cost is reduced, and the strength and manufacturing efficiency of the pipes are improved.
Smart Images

Figure CN118287640B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal pipe manufacturing, and in particular to a semi-continuous casting pipe crystallizer and a pipe manufacturing method. Background Art
[0002] Copper has excellent thermal conductivity, and copper pipes can be used as heat transfer materials in air conditioners, chemical equipment, power plants, etc. Copper pipes have better corrosion resistance than iron, so they can also be used as water pipes, gas pipes, etc.
[0003] At present, the manufacturing methods of copper tubes are mainly divided into extrusion-tube rolling-stretching method, oblique rolling piercing-tube rolling-stretching method, and coil welding method. The above copper tube manufacturing methods all include the hole making process, and the size of the hole is changed by stretching to obtain a copper tube of the target size.
[0004] Among them, the core process of the extrusion-rolling-stretching method includes drilling holes in copper ingots, heating copper ingots, and stretching copper ingots. Copper ingots need to be melted in advance and then cast and cooled in molds. This process is relatively complicated, with many process steps, high energy consumption during the production process, high production costs, and it is difficult to produce long copper tubes with large diameters (more than 200 mm). Generally, the length of the copper tubes produced is short. This is also the mainstream production method for other metal tubes, such as seamless steel tubes, aluminum alloy tubes, etc.
[0005] The oblique rolling piercing-tube rolling-stretching method has gradually faded out of actual production due to the existence of the piercing process, high requirements on equipment, high energy consumption and high production costs.
[0006] The production process of the coil welding method is to roll the copper plate into a tube and then weld it at the joint. The copper tube produced by this method will have a weld on its body. The presence of the weld may greatly increase the risk of cracking of the copper tube, and its strength is difficult to guarantee.
[0007] Therefore, it is urgent to provide a production device and method with simple manufacturing process, low cost, and the ability to produce copper tubes with large diameter (more than 200 mm) and good strength. Summary of the invention
[0008] The purpose of the present invention is to solve the problems of traditional copper tube manufacturing methods, such as complex manufacturing process, high manufacturing cost, and difficulty in producing copper tubes with large diameter (over 200 mm) and good strength, and to provide a semi-continuous casting tube crystallizer and tube manufacturing method, which can effectively solve the above technical problems.
[0009] The object of the present invention is achieved through the following technical scheme: a semi-continuous casting pipe crystallizer, comprising an upper end plate and a melt cavity, a cooling inner core is provided on the upper end plate, the cooling inner core is located in the middle of the melt cavity, an annular cooling crystallization cavity is formed between the cooling inner core and the melt cavity, and a diversion gate corresponding to the cooling crystallization cavity is provided on the upper end plate;
[0010] The cooling core is provided with a cooling medium cavity, a cooling medium passage for introducing cooling medium into the cooling medium cavity, and a first cooling medium outlet guide hole for discharging cooling medium in the cooling medium cavity;
[0011] A cooling water cavity is arranged in the melt cavity, one end of the cooling water cavity is a cooling water inlet end, and the other end of the cooling water cavity is a cooling water outlet end.
[0012] Preferably, a lower end plate is provided at the lower end of the melt cavity, and a second cooling medium outlet guide hole corresponding to the cooling water outlet end is provided on the lower end plate.
[0013] Preferably, the first cooling medium outlet guide hole is aligned with the inner surface of the pipe, and the second cooling medium outlet guide hole is aligned with the outer surface of the pipe;
[0014] The cooling medium in the cooling medium cavity passes through the first cooling medium outlet guide hole and is sprayed toward the inner surface of the pipe; the cooling water in the cooling water cavity passes through the second cooling medium outlet guide hole and is sprayed toward the outer surface of the pipe.
[0015] Preferably, a cooling medium inlet corresponding to the cooling medium passage is provided on the upper end plate.
[0016] Preferably, the cooling water cavity is a cylindrical cavity, and the cooling water cavity is arranged in a circular array inside the melt cavity.
[0017] Preferably, the cooling core is made of pure copper or copper alloy, and the outer side of the cooling core is coated with an insulating layer, and the insulating layer is made of oxidation-resistant graphite, silicon nitride or silicon carbide.
[0018] Preferably, the cooling medium introduced into the cooling core is one of water, water mist, nitrogen, gaseous carbon dioxide, argon, liquid carbon dioxide, liquid nitrogen, and liquid ammonia.
[0019] A method for manufacturing a pipe comprises the following specific steps:
[0020] The cooling medium is introduced into the cooling medium cavity through the cooling medium passage, and the cooling medium in the cooling medium cavity is discharged from the first cooling medium outlet guide hole; the cooling medium is introduced into the cooling water cavity through the cooling water inlet end, and the cooling medium in the cooling water cavity is discharged through the second cooling medium outlet guide hole;
[0021] The copper raw material is completely melted to form a melt, and the melt is poured into a cooling crystallization cavity through a diversion gate at the upper end of a semi-continuous casting tube crystallizer. The semi-continuous casting tube crystallizer cools the melt once, and the outer surface of the melt exchanges heat with the melt cavity and is cooled and solidified to form an outer solidified shell of the tube, and the inner surface of the melt exchanges heat with the cooling inner core and is cooled and solidified to form an inner solidified shell of the tube;
[0022] The melt after primary cooling in the semi-continuous casting pipe crystallizer forms a semi-solidified pipe, which is discharged from the lower end of the cooling crystallization chamber at a certain speed. The cooling medium discharged from the first cooling medium outlet guide hole is sprayed onto the inner surface of the semi-solidified pipe and the inner surface is secondary cooled; the cooling medium discharged from the second cooling medium outlet guide hole is sprayed onto the outer surface of the semi-solidified pipe and the outer surface is secondary cooled.
[0023] Preferably, cooling water is used as the cooling medium in the melt cavity, and the manufacturing speed V of the pipe is calculated by the following formula:
[0024] The pipe discharge speed V1 is calculated based on the cooling condition of the outer surface of the pipe. The calculation formula of the pipe discharge speed V1 is as follows:
[0025] V1=KP1(100-T 入水 )R 冷 *h*C 水 / (M*B 21 *C s L);
[0026] The pipe discharge speed V2 is calculated based on the condensation condition on the inner surface of the pipe. The calculation formula of the pipe discharge speed V2 is as follows:
[0027] V2=P2M 冷 / (MB 22 );
[0028] Among them, K is the comprehensive proportional coefficient, P1 is the pressure of cooling water entering the cooling water cavity, P2 is the pressure of cooling medium entering the cooling medium cavity, T 入水 is the temperature of cooling water before it enters the cooling water chamber, R 冷 is the radius of the second cooling medium outlet guide hole, C s is the solid phase heat capacity of the pipe material, h is the height of the semi-continuous casting pipe crystallizer, C 水 is the specific heat capacity of cooling water, M is the material parameter of the pipe, M 冷 is the cooling medium parameter, L is the minimum distance between the cooling water cavity and the melt, B 21 is the first condensation shell parameter, B 22 is the second condensation shell parameter;
[0029] The manufacturing speed V of the pipe is selected as the smaller value between the pipe discharging speed V1 and the pipe discharging speed V2.
[0030] As a preference, the first shell parameter B 21 The calculation formula is as follows:
[0031] B 21 =R a -(R a -X a ) 2 / R a ;
[0032] Second condensation shell parameter B 22 The calculation formula is as follows:
[0033] B 22 =R b +X b -R b 2 / (R b +X b );
[0034] Among them, R a is the outer diameter of the pipe, R b is the inner diameter of the pipe, X a is the thickness of the outer shell, X b is the thickness of the inner shell.
[0035] Preferably, the value of the comprehensive proportionality coefficient K is 0.0045.
[0036] The beneficial effects of the present invention are:
[0037] 1. The present invention has a simple manufacturing process, low manufacturing cost, can produce metal pipes with large diameters (more than 200 mm), and the manufactured metal pipes have good strength.
[0038] 2. When manufacturing the pipe, the present invention calculates the manufacturing speed of the pipe based on the size parameters of the pipe, the cooling medium parameters and other data, determines the optimal manufacturing speed of the pipe, and improves the manufacturing efficiency while ensuring that the pipe is fully cooled. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a top view of the semi-continuous casting pipe crystallizer.
[0040] Figure 2 This is a cross-sectional view of a semi-continuous casting pipe crystallizer.
[0041] Figure 3 Schematic diagram of metal tube manufacturing by semi-continuous casting tube crystallizer.
[0042] Figure 4 Schematic diagram of the production of metal tubes using a semi-continuous casting tube crystallizer.
[0043] In the figure: 1. upper end plate, 2. transfer gate, 3. cooling medium inlet, 4. fixing bolt, 5. cooling inner core, 6. cooling medium passage, 7. cooling medium cavity, 8. first cooling medium outlet guide hole, 9. melt cavity, 10. cooling water cavity, 11. cooling water inlet end, 12. lower end plate, 13. second cooling medium outlet guide hole, 14. cooling crystallization cavity. DETAILED DESCRIPTION
[0044] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0045] Those skilled in the art should understand that, in the disclosure of the present invention, the orientation or position relationship indicated by the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are based on the orientation or position relationship shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the above terms should not be understood as limiting the present invention.
[0046] It is to be understood that the term "one" should be understood as "at least one" or "one or more", that is, in one embodiment, the number of an element may be one, while in another embodiment, the number of the element may be multiple, and the term "one" should not be understood as a limitation on the quantity.
[0047] like Figures 1 to 4 As shown, a semi-continuous casting pipe crystallizer includes an upper end plate 1, a melt cavity 9, and a lower end plate 12. The upper end plate 1 is fixedly connected to the upper end of the melt cavity 9 by fixing bolts 4. A cooling inner core 5 is provided on the upper end plate 1, and the cooling inner core 5 is located at the lower side of the upper end plate 1. The cooling inner core 5 is located in the middle of the melt cavity 9. An annular cooling crystallization cavity 14 is formed between the cooling inner core 5 and the melt cavity 9. The upper end plate 1 is provided with a diversion gate 2 corresponding to the cooling crystallization cavity 14.
[0048] The cooling core 5 is provided with a cooling medium cavity 7, a cooling medium passage 6 for introducing cooling medium into the cooling medium cavity 7, and a first cooling medium outlet guide hole 8 for discharging cooling medium from the cooling medium cavity 7. The upper end plate 1 is provided with a cooling medium inlet 3 corresponding to the cooling medium passage 6, and the cooling medium inlet 3 is connected to the cooling medium passage 6.
[0049] A plurality of cooling water cavities 10 are provided in the melt cavity 9, one end of the cooling water cavity 10 is a cooling water inlet end 11, and the other end of the cooling water cavity 10 is a cooling water outlet end. The cooling water inlet end 11 passes through the side of the melt cavity 9. In the present invention, the cooling water cavity 10 is a cylindrical cavity, and a plurality of cooling water cavities 10 are arranged in a circular array inside the melt cavity 9. The lower end plate 12 is annular, and the lower end plate 12 is fixedly arranged at the lower end of the melt cavity 9. The lower end plate 12 is provided with a second cooling medium outlet guide hole corresponding to the cooling water outlet end and used to discharge the cooling water in the cooling water cavity 10.
[0050] In one embodiment, the first cooling medium outlet guide hole 8 is aligned with the inner surface of the pipe, and the second cooling medium outlet guide hole 13 is aligned with the outer surface of the pipe. The cooling medium in the cooling medium cavity 7 passes through the first cooling medium outlet guide hole 8 and is sprayed toward the inner surface of the pipe; the cooling water in the cooling water cavity 10 passes through the second cooling medium outlet guide hole 13 and is sprayed toward the outer surface of the pipe, and secondary cooling of the pipe is achieved in the above manner.
[0051] In another embodiment, when secondary cooling of the pipe is not required, the setting direction of the first cooling medium outlet guide hole and the second cooling medium outlet guide hole may not be aligned with the inner and outer surfaces of the pipe, so that the cooling medium and cooling water will not be sprayed onto the inner and outer surfaces of the pipe, thereby eliminating secondary cooling of the pipe.
[0052] The sizes of the cooling core 5 and the melt cavity 9 can be determined according to the size of the metal pipe to be processed.
[0053] The thermal conductivity of the cooling core material should be higher than 100W / mK. The cooling core material can be pure copper, copper alloy or graphite. The surface of the cooling core is coated with an insulating layer. The insulating layer material is anti-oxidation graphite, silicon nitride or silicon carbide. In actual use, the internal material of the cooling core can be selected according to actual needs.
[0054] In the present invention, the cooling medium in the melt cavity is cooling water, and the cooling medium introduced into the cooling core can be a gas cooling medium, a liquid cooling medium, a mixed cooling medium or a phase change cooling medium, wherein the liquid cooling medium can be water, the gas cooling medium can be nitrogen, gaseous carbon dioxide, argon, the mixed cooling medium can be water mist (i.e. a mixture of water and air), and the phase change cooling medium can be liquid carbon dioxide, liquid nitrogen, liquid ammonia.
[0055] The semi-continuous casting tube crystallizer can be used for manufacturing copper tubes, and can also be used for manufacturing tubes of other materials, such as iron tubes. The metal tube manufactured by the present invention can be either a round tube or a square tube.
[0056] A method for manufacturing a pipe, using the semi-continuous casting pipe crystallizer described above to manufacture the pipe, wherein the melt cavity 9 of the semi-continuous casting pipe crystallizer is cylindrical, the cooling inner core 5 is cylindrical, and copper is used as the raw material to manufacture a round copper pipe. In the manufacturing method, the first cooling medium outlet guide hole is aligned with the inner surface of the pipe, and the second cooling medium outlet guide hole is aligned with the outer surface of the pipe. The manufacturing method includes the following specific steps:
[0057] The cooling medium is introduced into the cooling medium cavity 7 through the cooling medium passage 6, and the cooling medium in the cooling medium cavity 7 is discharged from the first cooling medium outlet guide hole 8; the cooling medium is introduced into the cooling water cavity 10 through the cooling water inlet end 11, and the cooling medium in the cooling water cavity 10 is discharged through the second cooling medium outlet guide hole 13;
[0058] The copper raw material is completely melted to form a melt, and the melt is poured into the cooling crystallization cavity 14 through the transfer gate 2 at the upper end of the semi-continuous casting pipe crystallizer. The semi-continuous casting pipe crystallizer cools the melt once, and the outer surface of the melt exchanges heat with the melt cavity 9 and is cooled and solidified to form an outer solidified shell of the pipe. The inner surface of the melt exchanges heat with the cooling inner core 5 and is cooled and solidified to form an inner solidified shell of the pipe.
[0059] After the melt is cooled once in the semi-continuous casting tube crystallizer, it forms a semi-solidified tube. The semi-solidified tube is discharged from the lower end of the cooling crystallization chamber 14 at a certain speed. The cooling medium discharged from the first cooling medium outlet guide hole 8 is sprayed onto the inner surface of the semi-solidified tube and performs secondary cooling on the inner surface. The cooling medium discharged from the second cooling medium outlet guide hole 13 is sprayed onto the outer surface of the semi-solidified tube and performs secondary cooling on the outer surface. After secondary cooling, the semi-solidified tube finally forms a copper tube product.
[0060] Among them, the cooling medium in the melt cavity is cooling water, and the manufacturing speed V of the pipe (copper pipe) is calculated by the following formula:
[0061] The pipe discharge speed V1 is calculated based on the cooling condition of the outer surface of the pipe. The calculation formula of the pipe discharge speed V1 is as follows:
[0062] V1=KP1(100-T 入水 )R 冷 *h*C 水 / (M*B 21 *C s L);
[0063] The pipe discharge speed V2 is calculated based on the condensation condition on the inner surface of the pipe. The calculation formula of the pipe discharge speed V2 is as follows:
[0064] V2=P2M 冷 / (MB 22 );
[0065] Among them, K is the comprehensive proportional coefficient, P1 is the pressure of cooling water entering the cooling water cavity, P2 is the pressure of cooling medium entering the cooling medium cavity, T 入水 is the temperature of cooling water before it enters the cooling water chamber, R 冷 is the radius of the second cooling medium outlet guide hole, C s is the solid phase heat capacity of the pipe material, h is the height of the semi-continuous casting pipe crystallizer, C 水 is the specific heat capacity of cooling water, M is the material parameter of the pipe, M 冷 is the cooling medium parameter, L is the minimum distance between the cooling water cavity and the melt, B 21 is the first condensation shell parameter, B 22 is the second condensation shell parameter;
[0066] The manufacturing speed V of the pipe is selected as the smaller value between the pipe discharging speed V1 and the pipe discharging speed V2.
[0067] In the above formula, the first shell parameter B 21 The calculation formula is as follows:
[0068] B 21 =R a -(R a -X a ) 2 / R a ;
[0069] Second condensation shell parameter B 22 The calculation formula is as follows:
[0070] B 22 =R b +X b -R b 2 / (R b +X b );
[0071] Among them, R a is the outer diameter of the pipe, R b is the inner diameter of the pipe, X a is the thickness of the outer shell, X b is the thickness of the inner shell.
[0072] Among them, the calculation formula of the pipe discharge speed V1 is derived as follows:
[0073] The entire copper tube manufacturing process was subjected to thermal analysis, and the following formula was obtained based on the law of heat conservation:
[0074] △Q=Q 进 -Q 出 =Q 冷 ;
[0075] △Q is the heat change value, Q 进 is the initial heat of the melt when it enters the crystallizer, Q 出 is the heat of the melt when it leaves the crystallizer, Q 冷 The heat removed by the cooling medium.
[0076] Assume that the melting point of the melt is T r , the latent heat of phase change is H 相变 , the liquid phase heat capacity of the pipe is C l The average heat capacity of the melt from liquid phase to solid phase is C S The temperature of the melt before entering the crystallizer is T1, T1>T r The outer surface temperature of the tube after leaving the crystallizer is T 2a , the thickness of the outer shell is X a , the phase change enthalpy is H, and the inner surface temperature of the tube after leaving the crystallizer is T 2b , the inner shell thickness is X b The metal tube manufacturing speed is V. The outer diameter of the tube is R a , the inner diameter of the pipe is R b . R m It is the radius of the highest temperature zone in the melt in the cooling crystallization cavity. The temperature change value at each position of the tube (copper tube) cross section is a function of the radius and is also affected by the cooling factor. The temperature T at each position of the tube (copper tube) cross section can be approximately calculated by the following formula:
[0077] T=T m -(T m -T 2a )*(RR m ) / (R a -R m ).
[0078] This patent adopts double cooling crystallization of cooling inner core and melt cavity. For the outer surface of copper tube, the heat calculation is as follows:
[0079]
[0080] Among them, the flow rate of cooling water is proportional to the water pressure P, and the flow rate of cooling water V 水 =KP1,K 水 is the proportionality coefficient between water pressure and flow velocity.
[0081] Q 冷 =K 水 *P1*(T 出水 -T 入水 )*S*C 水 / L;
[0082] S=2πR 冷 *h*N;
[0083] In the above formula, T 出水 -T 入水 is the temperature difference between the water inlet and the water outlet, S is the surface area of the cooling water cavity in the melt cavity, R 冷 is the radius of the cooling water cavity; h is the height of the crystallizer, and the height of the cooling water cavity is approximately the same as the height of the crystallizer h; L is the minimum distance between the cooling water cavity and the melt, C 水 is the specific heat capacity of cooling water, and N is the number of cooling water cavities.
[0084] The number of cooling water chambers N depends on the outer diameter R of the pipe. a The number of cooling water chambers N and the outer diameter of the pipe R a The following function formula is satisfied:
[0085] N=2πR a / 0.3;
[0086] Substituting the above formula into the equation, we get S = 40 / 3*π 2 h 冷 *R a ;
[0087] For the crystallizer, the crystallizer dissipates heat through air and cooling water, and absorbs heat from the melt. When the temperature is stable, the heat absorbed and released by the crystallizer are equal. That is, Q 冷 =△Q. Since the thermal conductivity of the contact surface between copper and air is relatively large and the heat capacity of air is very small, it can be ignored in this equation and is therefore not included in the discussion.
[0088] Next, we simplify the formula. The heat capacity of the melt is approximately unchanged before and after condensation, so it can be considered that C s =C l , so the following formula is obtained:
[0089]
[0090] When the melt is cooled in the crystallizer, the cooling target of the inner and outer surfaces of the tube is to form an inner and outer shell of a certain thickness. There may still be melt inside the tube, that is, the maximum temperature T in the tube. m Higher than the melting point of the pipe (copper).
[0091] Q 冷 Simplified to K△T*S. And because Q 冷 =△Q, let H 相变 *ρ / Cs=MSimplifying the equation, we get:
[0092] P1K 水 (T 出水 -T 入水 )*40 / 3*π*h*R 冷 *R a *C 水 / (C s LV)=
[0093] 2 / 3*(T m -T 2a )(R a 2 +R m 2 +R a *R m )-(T m -T 2a )*R m *(R a +R m )+(R a 2 -(R a -X a ) 2 )M;
[0094] After sorting, we get:
[0095] V=40πK 水 P1(T 出水 -T 入水 )R 冷 *h*C 水 /
[0096] C s L*((2R a -R m 2 / R a -R m )*(T m -T2a )+(R a -(R a -X a ) 2 / Ra)*M);
[0097] Let B 11 =2R a -R m 2 / R a -R m , B 21 =R a -(R a -X a ) 2 / R a , substituting it into the above formula, we get:
[0098] V=40πK 水 P1(T 出水 -T 入水 )R 冷 *h*C 水 / (((T m -T 2a )*B 11 +M*B 21 )*C s L);
[0099] The V calculated by this formula is the pipe discharge speed V1.
[0100] Among them B 11 is the first cooling parameter. 21 is the first shell parameter. M is the material parameter of the pipe, H 相变 *ρ / Cs=M, when the material of the pipe is fixed, the latent heat of phase change H 相变 , specific heat capacity Cs and density ρ are also fixed, that is, M is fixed.
[0101] In the cooling water cavity, heat exchange is divided into two parts. First, the heat is transferred from the melt to the water on the surface of the cooling water cavity. The water on the pipe surface is heated and then transferred to the water inside the cooling water cavity. When the water temperature rises, the heat transfer between the cooling water wall and the pipe will be reduced. Therefore, when the inlet water temperature is higher, the outlet water temperature will also be higher, but the higher degree is lower than the inlet water temperature.
[0102] Due to △T 水 =T 出水 -T 入水 ;
[0103] When the casting conditions remain unchanged, T 出水 It is T 入水 function, so △T 水 Also T入水 Function of T 入水 The smaller the △T 水 In order to simplify the equation, set the temperature proportionality coefficient K T , according to experience △T 水 =K T *(100-T 入水 ), and replace the coefficient 40πK in the equation T K 水 Combined into a comprehensive proportional coefficient K, substitute it into the equation and simplify it to get the following formula:
[0104] V1=KP(100-T 入水 )R 冷 *h*C 水 / (((T m -T 2a )*B 11 +M*B 21 )*C s L).
[0105] In actual production experience, (T m -T 2a )*B1 is much smaller than M*B 21 The value of this item is, therefore (T m -T 2a )*B 11 This term can be ignored in the formula, so the above formula can be further simplified to obtain the simplified calculation formula:
[0106] V1=KP1(100-T 入水 )R 冷 *h*C 水 / (M*B 21 *C s L).
[0107] When water is used as the cooling medium, the value of the comprehensive proportional coefficient K is determined to be 0.0045.
[0108] The calculation formula of pipe discharge speed V2 is derived as follows:
[0109] When cooling the inner surface of the pipe, the main cooling method is to directly contact the inner surface of the melt with the cooling water sprayed from the first cooling medium outlet guide hole. At this time, the heat equation is:
[0110] Q 冷 =△Q;
[0111]
[0112] Here, the phase change and reaction enthalpy change are both represented by H. When the gas pressure component remains unchanged, the heat taken away is proportional to the contact area. In the copper tube, the contact area is proportional to the radius of the copper tube. All proportional coefficients are concentrated on the proportional coefficient K.
[0113] make Then we can get:
[0114] (T m -T 2b )*B 12 +M*B 22 =P2M 冷 / (C s V);
[0115] After adjusting the formula, we get:
[0116] V=P2M 冷 / (C s *((T m -T 2b )*B 12 +M*B 22 ));
[0117] The V calculated in this formula is the pipe discharge speed V2.
[0118] In the above formula, M = H 相变 *ρ / C s , B 12 =2R m -R b 2 / R m -R b , B 22 =R b +X b -R b 2 / (R b +X b );
[0119] B 12 is the second cooling parameter, B 22 is the second condensation shell parameter.
[0120] M 冷 is the item related to the cooling medium, M 冷 The calculation formula of is the same as that of M. When the cooling medium is fixed, M 冷 The value of is fixed. 冷 When we need to adjust M 冷When adjusting the cooling medium, it can be adjusted from the perspective of specific heat capacity and phase change. For example, if the cooling medium is water mist, increasing the proportion of water in the water mist can increase the heat carried away by the water phase change and increase the specific heat capacity of the mixture. If the cooling medium contains graphite powder, it is necessary to consider the heat released by the oxidation of graphite powder. At this time, increasing the proportion of graphite powder will reduce the cooling capacity.
[0121] Considering the actual application process, C s *((T m -T 2b )*B 12 The value of this item is much smaller than M*B 22 The value of this term, therefore C s *((T m -T 2b )*B 12 This term can be ignored in the formula, and the final simplification of the formula is:
[0122] V2=P2M 冷 / (MB 22 ).
[0123] Specific example 1:
[0124] Manufacturing round copper tubes, the inner diameter of the copper tube is 0.6 meters, the outer diameter of the copper tube is 0.2 meters, the height of the crystallizer is 0.275 meters, the minimum distance L between the cooling water cavity and the melt is 0.15 meters, the diameter of the cooling water cavity is 0.03 meters, the inlet temperature of the cooling water is 30℃ (303.15K), the water enters from the top and exits from the bottom. The pouring temperature of the copper liquid is 1150℃, and the pressure P1 of the cooling water is 5*10 5 Pa. The cooling medium in the cooling core is water mist, and the injection pressure P2 is 3.5*10 5 pa, water mist concentration is 5g / L, H 相变 =209000J / kg, C s =390J / (kg·℃), the density of the pipe is ρ=8.92*10 3 kg / m 3 , M=478000.
[0125] Required outer shell thickness X a = 0.1906 m, calculated B 21 =R a -(R a -X a ) 2 / R a =0.3206, after substituting it into the calculation formula of the pipe discharge speed V1, we get V1=2.62m / h.
[0126] Required inner shell thickness X b= 0.0953 m, calculated B 22 =R b +X b -R b 2 / (R b +X b )=0.1598, and after substituting it into the calculation formula of the pipe discharge speed V2, it is calculated that V2=2.69m / h.
[0127] Therefore, the final copper tube manufacturing speed V is selected as 2.62m / h.
[0128] Specific example 2:
[0129] The size of the crystallizer and the cooling medium conditions are consistent with those of Specific Example 1, and a round copper tube with an outer diameter of 0.5 m and an inner diameter of 0.3 m is manufactured.
[0130] Required outer shell thickness X a =0.0953 meters, and B2=0.1724 is calculated. After substituting it into the calculation formula of the pipe discharge speed V1, it is calculated that V1=3.9m / h.
[0131] Required inner shell thickness X b = 0.0477 m, calculated B 22 =0.08886, and after substituting it into the calculation formula of the pipe discharge speed V2, it is calculated that V2 = 4.85m / h.
[0132] Therefore, the final copper tube manufacturing speed V is selected as 3.9m / h.
[0133] Specific example 3:
[0134] When the material of the pipe is changed from copper to iron, the thermal conductivity of iron is significantly slower than that of copper, and its melting point is higher. Since the heat released is mainly latent heat, according to the formula:
[0135] V=KP1T 入水 R 冷 *h*C 水 / (M*B 21 *C s L)
[0136] The thermal conductivity of iron is only one-fifth of that of copper, which greatly reduces K. If other conditions remain unchanged, the casting speed will drop significantly. In order to ensure the casting speed, the following adjustments can be made:
[0137] 1. Increasing the cooling water pressure P will increase the water flow rate and also increase the K value;
[0138] 2. Reduce the distance L between the cooling water and the melt;
[0139] 3. Increase the crystallizer height h.
[0140] For cooling the inner core, according to the formula V = P2M 冷 / (MB 22 ), due to the poor thermal conductivity of iron, the efficiency of the cooling medium will be reduced. We can increase the cooling effect by increasing the pressure of the input cooling medium to increase the casting speed.
[0141] According to the formula
[0142] We can also increase M by increasing the heat capacity of the cooling medium or increasing the phase change heat absorption. 冷 The simplest way is to increase the proportion of water in the mist; crushed ice can also be mixed to further increase the phase change absorption heat to increase M 冷 , ultimately increasing the casting speed.
[0143] The present invention has the following advantages:
[0144] 1. The present invention has a simple manufacturing process, low manufacturing cost, can produce metal pipes with large diameters (above 400 mm), and the manufactured metal pipes have good strength.
[0145] 2. When manufacturing the pipe, the present invention calculates the manufacturing speed of the pipe based on the size parameters of the pipe, the cooling medium parameters and other data, determines the optimal manufacturing speed of the pipe, and improves the manufacturing efficiency while ensuring that the pipe is fully cooled.
[0146] The present invention is not limited to the above-mentioned optimal implementation mode. Anyone can derive other various forms of products under the inspiration of the present invention. However, no matter what changes are made in the shape or structure, all technical solutions that are the same or similar to those of the present application fall within the protection scope of the present invention.
Claims
1. A method for manufacturing a pipe, characterized in that: The semi-continuous casting tube crystallizer is used to complete the manufacturing, and the semi-continuous casting tube crystallizer includes an upper end plate and a melt cavity. The upper end plate is connected to a cooling inner core, and the cooling inner core is located in the middle of the melt cavity. An annular cooling crystallization cavity is formed between the cooling inner core and the melt cavity, and a diversion gate corresponding to the cooling crystallization cavity is provided on the upper end plate; The cooling core is provided with a cooling medium cavity, a cooling medium passage for introducing cooling medium into the cooling medium cavity, and a first cooling medium outlet guide hole for discharging cooling medium in the cooling medium cavity; A cooling water cavity is provided in the melt cavity, one end of the cooling water cavity is a cooling water inlet end, and the other end of the cooling water cavity is a cooling water outlet end; A lower end plate is provided at the lower end of the melt cavity, and a second cooling medium outlet guide hole corresponding to the cooling water outlet end is provided on the lower end plate; the first cooling medium outlet guide hole is aligned with the inner surface of the pipe, and the second cooling medium outlet guide hole is aligned with the outer surface of the pipe; The cooling medium in the cooling medium cavity passes through the first cooling medium outlet guide hole and is sprayed toward the inner surface of the pipe; the cooling water in the cooling water cavity passes through the second cooling medium outlet guide hole and is sprayed toward the outer surface of the pipe; The pipe manufacturing method comprises the following specific steps: The cooling medium is introduced into the cooling medium cavity through the cooling medium passage, and the cooling medium in the cooling medium cavity is discharged from the first cooling medium outlet guide hole; the cooling medium is introduced into the cooling water cavity through the cooling water inlet end, and the cooling medium in the cooling water cavity is discharged through the second cooling medium outlet guide hole; The copper raw material is completely melted to form a melt, and the melt is poured into a cooling crystallization cavity through a diversion gate at the upper end of a semi-continuous casting tube crystallizer. The semi-continuous casting tube crystallizer cools the melt once, and the outer surface of the melt exchanges heat with the melt cavity and is cooled and solidified to form an outer solidified shell of the tube, and the inner surface of the melt exchanges heat with the cooling inner core and is cooled and solidified to form an inner solidified shell of the tube; After the melt is cooled once in the semi-continuous casting tube crystallizer, it forms a semi-solidified tube. The semi-solidified tube is pulled out from the lower end of the cooling crystallization chamber at a certain speed. The cooling medium discharged from the first cooling medium outlet guide hole is sprayed onto the inner surface of the semi-solidified tube and the inner surface is cooled for a second time. The cooling medium discharged from the second cooling medium outlet guide hole is sprayed onto the outer surface of the semi-solidified tube and the outer surface is cooled for a second time. Cooling water is used as the cooling medium in the melt cavity, and the manufacturing speed V of the pipe is calculated by the following formula: The pipe discharge speed V1 is calculated based on the cooling condition of the outer surface of the pipe. The calculation formula of the pipe discharge speed V1 is as follows: ; The pipe discharge speed V2 is calculated based on the condensation condition on the inner surface of the pipe. The calculation formula of the pipe discharge speed V2 is as follows: <h2 style=";text-align:left;direction:ltr">V2=P2M<h2 style=";text-align:left;direction:ltr"> 冷 <h2 style=";text-align:left;direction:ltr"> / (MB<h2 style=";text-align:left;direction:ltr"> 22 <h2 style=";text-align:left;direction:ltr"> ); Among them, K is the comprehensive proportional coefficient, P1 is the pressure of cooling water entering the cooling water cavity, P2 is the pressure of cooling medium entering the cooling medium cavity, T 入水 is the temperature of cooling water before it enters the cooling water chamber, R 冷 is the radius of the second cooling medium outlet guide hole, C s is the average heat capacity of the melt cooling from liquid phase to solid phase, h is the height of the semi-continuous casting pipe crystallizer, C 水 is the specific heat capacity of cooling water, M is the material parameter of the pipe, M 冷 is the cooling medium parameter, L is the minimum distance between the cooling water cavity and the melt, B 21 is the first condensation shell parameter, B 22 is the second condensation shell parameter; First condensation shell parameter B 21 The calculation formula is as follows: B 21 =R a -(R a -X a ) 2 / R a ; Second condensation shell parameter B 22 The calculation formula is as follows: B 22 =R b +X b -R b 2 / (R b +X b ); Among them, R a is the outer diameter of the pipe, R b is the inner diameter of the pipe, X a is the thickness of the outer shell, X b is the thickness of the inner shell; The manufacturing speed V of the pipe is selected as the smaller value between the pipe discharging speed V1 and the pipe discharging speed V2.
2. A method for manufacturing a pipe according to claim 1, characterized in that: The upper end plate is provided with a cooling medium inlet corresponding to the cooling medium passage.
3. A method for manufacturing a pipe according to claim 1, characterized in that: The cooling water cavity is a cylindrical cavity, and the cooling water cavity is arranged inside the melt cavity in a circular array.
4. A method for manufacturing a pipe according to claim 1, characterized in that: The material of the cooling inner core is pure copper or copper alloy, the surface of the cooling inner core is coated with an insulating layer, and the material of the insulating layer is anti-oxidation graphite, silicon nitride or silicon carbide.