Method for preparing unbleached recycled nylon chips using colored nylon waste yarn
By combining chemical stripping and high-temperature stripping treatment with the suction and fine filtration of a melt extruder, the problem of the difficulty in recycling colored nylon waste yarn is solved, and high-quality natural white recycled nylon chips are produced, which are suitable for spinning high-quality recycled nylon fibers.
Patent Information
- Application Number
- CN202410371835.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-03-29
AI Technical Summary
Existing technologies are difficult to effectively recycle colored nylon waste yarn, resulting in a decline in the performance of recycled nylon fibers and limitations in color processing. Furthermore, chemical recycling methods are energy-intensive and involve complex processes.
Chemical stripping was performed using a stripping solution composed of sodium hydroxide pretreatment, benzyl alcohol, biochar granules, and sodium dithionite. Combined with the suction and fine filtration devices of a melt extruder, oil, dyes, and impurities on the surface of colored nylon waste yarn were removed to prepare unbleached recycled nylon chips.
It achieves efficient separation of dyes and nylon, removes surface oils and impurities, reduces production energy consumption, and improves the quality and utilization rate of recycled nylon chips, making it suitable for spinning high-quality recycled nylon fibers.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of recycled nylon technology, specifically relating to a method for preparing unbleached recycled nylon chips using colored nylon waste yarn. Background Technology
[0002] In recent years, the government has further increased its support for green, low-carbon, and circular industries closely related to the recycling and utilization of renewable resources, greatly promoting the industry's transformation, upgrading, and high-quality development. "Increasing the proportion of recycled raw materials used in product green design" has been made a key requirement, and the government has proposed improving standards and regulations for recycled raw materials and strengthening target management of recycled materials. Against this backdrop, recycled nylon fiber has become a hot topic in the recycled chemical fiber market.
[0003] Currently, nylon recycling mainly involves chemical and physical methods. Among them, chemical methods include research directions such as green solvent dissolution / reprecipitation technology, subcritical / supercritical fluid depolymerization technology, solid superacid catalytic depolymerization technology, and depolymerization in ionic liquids. However, chemical recycling processes are energy-intensive, complex, and costly. Therefore, physical recycling has become an important direction for the industry's development.
[0004] Patent document CN111876871A discloses a method for producing recycled nylon environmentally friendly air-coated yarn. After removing impurities from waste nylon yarn or nylon fabric through physical and chemical processes, the yarn is melted at high temperature to obtain recycled polyamide melt. This polyamide melt is then mixed with conventional nylon 66 and conventional polyester in a ratio of 3–5:2:0.3–0.5, melted, extruded, granulated, and sliced to obtain recycled polyamide chips. The melting temperature is 260–285°C. Patent document CN114248364A provides a method for implementing a recycled nylon 6 chip production system. Waste nylon 6 yarn is mixed, quantitatively fed, and transported to an auxiliary screw extruder for pressure stabilization and cooling. Finally, it is melted and cut to obtain recycled nylon chips, eliminating the need for raw material degreasing, reducing processes, and lowering costs.
[0005] Currently, the recycling of nylon waste mainly utilizes unbleached nylon fibers, while the recycling of colored nylon waste is still limited. This is primarily because various pigments and additives are added during the processing of colored nylon products, making the recycling of waste nylon fibers more difficult. For example, these additives reduce the intrinsic viscosity of recycled nylon, thus affecting its strength and other properties; pigments also limit the color processing of subsequent products. However, colored nylon waste accounts for the vast majority of nylon waste. Therefore, the decolorization, cleaning, and regeneration of colored waste nylon is of greater practical significance. The industrial-scale production process of recycled colored nylon waste into spinning chips remains a blank area in the chemical fiber industry. Summary of the Invention
[0006] In view of this, the present invention provides a method for the batch and continuous production of recycled natural white nylon chips from colored nylon waste yarn. The product obtained by this method has good uniformity and stability and can be used to spin high-quality recycled nylon fibers.
[0007] A method for preparing unbleached recycled nylon chips using colored nylon waste yarn includes the following steps:
[0008] (1) The colored nylon waste yarn was pretreated by immersing it in an aqueous sodium hydroxide solution;
[0009] (2) Immerse the pretreated nylon waste yarn in the stripping solution and strip it under stirring. Then, dehydrate, wash and dry it in sequence.
[0010] (3) Using a melt extruder equipped with a suction device and a fine filter device, the dried nylon waste yarn is melted, drawn into strips, and cut to obtain the white recycled nylon chips.
[0011] In step (1) above:
[0012] The aforementioned colored nylon waste yarn is colored nylon 6 waste yarn.
[0013] The purpose of using sodium hydroxide aqueous solution for pretreatment is to prepare for subsequent stripping treatment, and at the same time remove oil and tannic acid from the surface of nylon waste yarn.
[0014] Preferably, in the pretreatment, the mass-to-volume ratio of nylon waste filament to sodium hydroxide aqueous solution is 1:(20-40) g / mL. More preferably, it is 1:(25-35) g / mL. Even more preferably, it is 1:30 g / mL.
[0015] As a preferred option, colored nylon waste yarn is first cut by a cutting machine before pretreatment, with a cutting length of 1-5 mm.
[0016] Preferably, the concentration of sodium hydroxide in the aqueous solution is 1–5 g / L.
[0017] Preferably, the pretreatment temperature is 80–95℃ and the time is 45–90 min.
[0018] In step (2) above:
[0019] Preferably, the stripping solution is prepared by dissolving a stripping agent composed of benzyl alcohol, biochar particles, and sodium dithionite in water. Benzyl alcohol, as an oil solvent, has a plasticizing effect on nylon fibers and a solubilizing effect on the dyes on the fibers, significantly improving the stripping effect. The main function of the biochar particles is to adsorb the dye molecules stripped from the fibers, preventing re-dyeing of the fibers and addressing issues such as difficult wastewater treatment. The main function of sodium dithionite is to destroy the groups in the color-developing system of the dye molecules, thereby causing the nylon to fade.
[0020] As a further preferred embodiment, the concentration of benzyl alcohol in the stripping solution is 0.1–1 ml / L;
[0021] The concentration of biochar particles is 10–50 g / L;
[0022] The concentration of sodium dithionite is 1–3 g / L.
[0023] Preferably, in the stripping process, the mass-to-volume ratio of nylon waste yarn to stripping solution is 1:(10-30) g / mL. More preferably, it is 1:(15-25) g / mL. Even more preferably, it is 1:20 g / mL.
[0024] Preferably, the temperature for the color stripping treatment is 100–120°C, and the time is 30–60 min.
[0025] Preferably, the drying temperature is 100–120℃ and the drying time is 60–120 min.
[0026] In step (3) above:
[0027] Preferably, the melting temperature is 225–270°C and the screw speed is 300–650 rpm. More preferably, the melting temperature is 250–270°C.
[0028] Preferably, the suction negative pressure is 0.08–0.1 MPa, and the filtration accuracy is 3–10 μm. More preferably, the filtration accuracy is 3–5 μm.
[0029] The aforementioned melt extruder equipped with a suction device and a fine filtration device has a suction device installed near the discharge port and a fine filtration device installed at the discharge port. The suction device is used to extract and partially remove residual moisture and high-temperature decomposed dye monomers from the nylon waste filament melt during the melting stage; the fine filtration device is used to further remove solid additives and dye impurities from the nylon waste filament melt, improving the quality of the product chips.
[0030] The present invention discloses a method for preparing natural white recycled nylon chips from colored nylon waste yarn. The colored nylon waste yarn is cut, pretreated, and stripped of its color to become light-colored or natural white nylon. At the same time, the surface oil of the nylon waste yarn is removed. Then, it is melt-granulated to further decompose the dye molecules at high temperature. The residual moisture and dye molecules decomposed at high temperature in the melt are removed by using the suction and fine filtration functions of the melt extruder, and additives and dye impurities are filtered out, finally obtaining high-quality natural white recycled nylon chips.
[0031] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0032] This invention discloses a method for preparing unbleached recycled nylon chips from colored nylon waste filaments. Through dual treatment of chemical and high-temperature stripping of the colored nylon waste filaments, efficient separation of dye and nylon is achieved. Simultaneously, pretreatment, suction, and fine filtration effectively remove surface oils, additives, and dye impurities from the nylon waste filaments, ensuring the performance of the resulting recycled nylon chips. Furthermore, no additional degreasing or impurity removal processes are required, reducing production energy consumption and improving the quality of the nylon chips. The unbleached recycled nylon chips obtained by this method have a viscosity of 2.5–2.55; ash content of 0.31–0.43%; whiteness of 96–99%; and moisture content of 400–600 ppm. They can be used for spinning high-quality recycled nylon fibers. This preparation method effectively improves the recycling rate of colored waste nylon (nylon waste filaments), overcomes the limitation that colored waste nylon cannot be recycled and granulated, and broadens the raw material sources for recycled nylon chips. Detailed Implementation
[0033] Example 1:
[0034] 1. The collected colored nylon 6 waste yarn is first processed by a cutting machine and cut into 5 mm nylon waste yarn short fibers.
[0035] 2. Pretreatment: Place the waste nylon short fibers in a high-temperature and high-pressure reactor, add an appropriate amount of water (the mass-volume ratio of waste nylon short fibers to water is 1:30 g / mL), add sodium hydroxide (the mass-volume ratio of water to sodium hydroxide is 5 g / L), raise the temperature to 95℃, and treat for 90 minutes to remove surface oil and tannic acid.
[0036] 3. Stripping treatment: Prepare a stripping solution by dissolving benzyl alcohol, biochar granules, and sodium dithionite in water, wherein the concentration of benzyl alcohol is 1 ml / L; the concentration of biochar granules is 50 g / L; and the concentration of sodium dithionite is 3 g / L. Put the pretreated nylon waste yarn into the stripping solution (the mass-volume ratio of nylon waste yarn to stripping solution is 1:20 g / mL), stir, heat to 120℃, strip for 60 min, and then dehydrate and wash with water.
[0037] 4. Dry the stripped nylon waste yarn at 120℃ for 120 minutes.
[0038] 5. Using a melt extruder equipped with a suction device and a fine filtration device, the dried nylon waste filaments are fed into the melt extruder via a feeder. After melting, they are drawn into strands and cut to obtain natural white recycled nylon chips. The melting temperature is 270℃, the screw speed is 650 rpm, the suction negative pressure is 0.1 MPa, and the filtration accuracy is 3 microns.
[0039] The suction device is located near the discharge port of the extruder to suction and partially remove residual moisture and high-temperature decomposed dye monomers from the melt discharged from the discharge port; the fine filter device is installed at the discharge port of the extruder to further remove additives and dye impurities, thereby improving the quality of nylon chips.
[0040] Tests showed that the high-quality unbleached recycled nylon chips obtained in this embodiment had a viscosity of 2.52, an ash content of 0.31%, a whiteness of 99%, and a moisture content of 400 ppm; they can be used for spinning high-quality recycled nylon fibers.
[0041] Example 2:
[0042] 1. The collected colored nylon 6 waste yarn is first processed by a cutting machine and cut into 5 mm nylon waste yarn short fibers.
[0043] 2. Pretreatment: Place the waste nylon short fibers in a high-temperature and high-pressure reactor, add an appropriate amount of water (the mass-volume ratio of waste nylon short fibers to water is 1:30 g / mL), add sodium hydroxide first (the mass-volume ratio of water to sodium hydroxide is 1 g / L), raise the temperature to 80℃, and treat for 45 minutes to remove surface oil and tannic acid.
[0044] 3. Stripping treatment: Prepare a stripping solution by dissolving benzyl alcohol, biochar granules, and sodium dithionite in water. The concentration of benzyl alcohol is 0.1 ml / L, the concentration of biochar granules is 10 g / L, and the concentration of sodium dithionite is 1 g / L. Put the pretreated nylon waste yarn into the stripping solution (the mass-volume ratio of nylon waste yarn to stripping solution is 1:20 g / mL), stir, heat to 100℃, strip for 30 min, and then dehydrate and wash with water.
[0045] 4. Dry the stripped nylon waste yarn at 100℃ for 60 minutes.
[0046] 5. Using a melt extruder equipped with a suction device and a fine filtration device, the dried nylon waste filaments are fed into the melt extruder via a feeder. After melting, they are drawn into strands and cut to obtain natural white recycled nylon chips. The melting temperature is 270℃, the screw speed is 300 rpm, the suction negative pressure is 0.08 MPa, and the filtration accuracy is 3 microns.
[0047] The suction device is located near the discharge port of the extruder to suction and partially remove residual moisture and high-temperature decomposed dye monomers from the melt discharged from the discharge port; the fine filter device is installed at the discharge port of the extruder to further remove additives and dye impurities, thereby improving the quality of nylon chips.
[0048] Tests showed that the high-quality off-white recycled nylon chips obtained in this embodiment had a viscosity of 2.53, an ash content of 0.4%, a whiteness of 96%, and a moisture content of 400 ppm; they can be used for spinning high-quality recycled nylon fibers.
[0049] Example 3
[0050] 1. The collected colored nylon 6 waste yarn is first processed by a cutting machine and cut into 5 mm nylon waste yarn short fibers.
[0051] 2. Pretreatment: Place the waste nylon short fibers in a high-temperature and high-pressure reactor, add an appropriate amount of water (the mass-volume ratio of waste nylon short fibers to water is 1:30 g / mL), add sodium hydroxide first (the mass-volume ratio of water to sodium hydroxide is 2.5 g / L), raise the temperature to 95℃, and treat for 90 minutes to remove surface oil and tannic acid.
[0052] 3. Stripping treatment: Prepare a stripping solution by dissolving benzyl alcohol, biochar granules, and sodium dithionite in water, wherein the concentration of benzyl alcohol is 0.5 ml / L; the concentration of biochar granules is 25 g / L; and the concentration of sodium dithionite is 2 g / L. Put the pretreated nylon waste yarn into the stripping solution (the mass-volume ratio of nylon waste yarn to stripping solution is 1:20 g / mL), stir, heat to 120℃, strip for 60 min, and then dehydrate and wash with water.
[0053] 4. Dry the stripped nylon waste yarn at 120℃ for 120 minutes.
[0054] 5. Using a melt extruder equipped with a suction device and a fine filtration device, the dried nylon waste filaments are fed into the melt extruder via a feeder, melted, drawn into strands, and cut to obtain natural white recycled nylon chips. The melting temperature is 260℃, the screw speed is 500 rpm, the suction negative pressure is 0.09 MPa, and the filtration accuracy is 3 microns.
[0055] The suction device is located near the discharge port to suction and partially remove residual moisture and high-temperature decomposed dye monomers from the melt discharged from the discharge port; the fine filter device is installed at the discharge port of the extruder to further remove additives and dye impurities, thereby improving the quality of nylon chips.
[0056] Tests showed that the high-quality off-white recycled nylon chips obtained in this embodiment had a viscosity of 2.5, an ash content of 0.31%, a whiteness of 98%, and a moisture content of 400 ppm; they can be used for spinning high-quality recycled nylon fibers.
[0057] Comparative Example
[0058] 1. The collected colored nylon 6 waste yarn is first processed by a cutting machine and cut into 5 mm nylon waste yarn short fibers.
[0059] 2. Using a melt extruder equipped with a suction device and a fine filtration device, waste nylon short fibers are fed into the melt extruder via a feeder. After melting, they are drawn into strands and cut to obtain natural white recycled nylon chips. The melting temperature is 270℃, the screw speed is 650 rpm, the suction negative pressure is 0.1 MPa, and the filtration accuracy is 3 microns.
[0060] The suction device is located near the discharge port to suction and partially remove residual moisture and high-temperature decomposed dye monomers from the melt discharged from the discharge port; the fine filter device is installed at the discharge port of the extruder to further remove additives and dye impurities, thereby improving the quality of nylon chips.
[0061] Tests showed that the recycled nylon chips prepared in this comparative example had uneven color, large viscosity deviation, and a whiteness value of less than 50%, making them unsuitable for spinning recycled nylon fibers.
Claims
1. A method for preparing unbleached recycled nylon chips using colored nylon waste yarn, characterized in that, Includes the following steps: (1) The colored nylon waste yarn is pretreated by immersing it in an aqueous sodium hydroxide solution; (2) Immerse the pretreated nylon waste yarn in the stripping solution and strip it under stirring. Then, dehydrate, wash and dry it in sequence. (3) Using a melt extruder equipped with a suction device and a fine filter device, the dried nylon waste yarn is melted, drawn into strips, and cut to obtain the natural white recycled nylon chips; The concentration of sodium hydroxide in aqueous solution is 1~5 g / L; The stripping solution is prepared by dissolving a stripping agent composed of benzyl alcohol, biochar particles, and sodium dithionite in water; The concentration of benzyl alcohol in the stripping solution is 0.1~1 ml / L; The concentration of biochar particles is 10~50 g / L; The concentration of sodium dithionite is 1~3 g / L.
2. The method for preparing unbleached recycled nylon chips using colored nylon waste yarn according to claim 1, characterized in that, The pretreatment temperature is 80~95℃ and the time is 45~90min.
3. The method for preparing unbleached recycled nylon chips using colored nylon waste yarn according to claim 1, characterized in that, In the stripping process, the mass-to-volume ratio of nylon waste yarn to stripping solution is 1:(10~30)g / mL.
4. The method for preparing unbleached recycled nylon chips using colored nylon waste yarn according to claim 1, characterized in that, The temperature for the color stripping process is 100~120℃, and the time is 30~60min.
5. The method for preparing unbleached recycled nylon chips using colored nylon waste yarn according to claim 1, characterized in that, In step (3), the melting temperature is 225~270℃ and the screw speed is 300~650 rpm; The suction negative pressure is 0.08~0.1MPa, and the filtration accuracy is 3~10μm.
6. The method for preparing unbleached recycled nylon chips using colored nylon waste yarn according to claim 1, characterized in that, In the pretreatment, the mass-to-volume ratio of nylon waste filaments to sodium hydroxide aqueous solution is 1:(20~40) g / mL.
7. The method for preparing unbleached recycled nylon chips using colored nylon waste yarn according to claim 1, characterized in that, In step (1), before the colored nylon waste yarn is pretreated, it is first cut by a cutting machine with a cutting length of 1~5mm.
8. The method for preparing unbleached recycled nylon chips using colored nylon waste yarn according to claim 1, characterized in that, In step (2), the drying temperature is 100~120℃ and the drying time is 60~120min.
Citation Information
Patent Citations
Polyamide regenerated environment-friendly air covered yarns
CN111876871A
Implementation method of regenerated chinlon 6 slice production system
CN114248364A
Method for preparing regenerated plastic particles by using waste cloth and regenerated plastic particles
CN106346634A
Method for dyeing aramid 1414 fibers
CN112359614A
Method and device for producing engineering plastic grade slices by using waste brocade-spandex fabric garments
CN113977802A