A method for regulating chiral perovskite to produce circularly polarized luminescence through pressure
Patent Information
- Application Number
- CN202410408265.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-04-07
AI Technical Summary
[0003]然而,纯铟基手性钙钛矿的荧光强度太低,因此无法实现圆偏振发光性能
[0004] The purpose of the present invention is to provide a method for producing circularly polarized luminescence by regulating chiral perovskite through pressure, and obtain a chiral perovskite single crystal through a cooling crystallization method. The single crystal has a symmetrical circular dichroism spectrum, that is, chiral properties, but the fluorescence properties are weak and do not have circular polarization Luminescence performance: under high pressure, the chiral spatial structure and electronic structure of the single crystal are controlled, so that the single crystal has both chiral and fluorescent properties, thus showing symmetrical circularly polarized luminescence characteristics, with a luminescence region of 380-740nm. Asymmetry factor g lum Up to 5.0×10 -3 , which is of great significance to the study of circularly polarized luminescence properties.
Smart Images

Figure CN118290271B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of chiral perovskite material synthesis, and in particular to a method for regulating chiral perovskite to produce circularly polarized luminescence through pressure. Background Art
[0002] Circularly polarized luminescent materials are widely used in optical data storage, 3D display, optical anti-counterfeiting and other aspects, and have attracted more and more attention. Metal halide perovskite materials have the characteristics of flexible crystal structure, long carrier diffusion length, high dielectric constant, adjustable band gap, large light absorption coefficient and strong spin-orbit coupling, so they have been proved to be a promising optoelectronic material. 0D perovskite retains the photophysical properties of a single metal halide octahedron or metal halide cluster. Compared with 3D, 2D and 1D perovskites, 0D perovskites have higher stability and are more conducive to commercial applications. Traditionally studied lead-based perovskites contain heavy metal lead, which pollutes the environment and limits their further research and application. Indium-based metal halide perovskite has the advantages of wide emission, non-toxicity and strong stability, and is a non-lead green and friendly material.
[0003] However, the fluorescence intensity of pure indium-based chiral perovskite is too low, so circularly polarized luminescence performance cannot be achieved. The invention patent with publication number CN116715638A and patent name "Antimony-doped chiral dual-ligand indium-based hybrid halide perovskite material and its preparation method and application" adopts an antimony metal doping strategy to prepare chiral hybrid perovskite and achieve circularly polarized luminescence performance, but increases the types of raw materials and increases the cost. High pressure is another important experimental adjustment variable different from parameters such as temperature and concentration. Pressure research has important theoretical and practical significance in the field of materials. The technology of using diamond anvil high-pressure device and ruby for pressure calibration has promoted the steady development of high-pressure science. Using hydrostatic pressure to systematically study the changes in the structure and optical properties of chiral perovskite materials, explore the influence of pressure on fluorescence properties, and provide direct evidence for revealing the structure-activity relationship of material structure to properties. Therefore, extending the hydrostatic pressure effect to indium-based chiral perovskites with weak fluorescence, studying their fluorescence behavior and potential circularly polarized luminescence properties under pressure response, is of great significance for the study of circularly polarized luminescence. Summary of the invention
[0004] The purpose of the present invention is to provide a method for regulating chiral perovskite to produce circularly polarized luminescence by pressure, and obtain a chiral perovskite single crystal by a cooling crystallization method. The single crystal has a symmetrical circular dichroism spectrum, that is, chiral properties, but weak fluorescence properties, and does not have circularly polarized luminescence performance. Under high pressure, the chiral spatial structure and electronic structure of the single crystal are regulated, so that the single crystal has both chirality and fluorescence properties, thereby showing symmetrical circularly polarized luminescence characteristics, the luminescent region is 380-740nm, and the asymmetry factor g is 2.5~8.lum Up to 5.0×10 -3 , which is of great significance to the study of circularly polarized luminescence properties.
[0005] To achieve the above object, the present invention provides a method for regulating chiral perovskite to produce circularly polarized luminescence by pressure, comprising the following steps:
[0006] S1. Preparation of chiral perovskite single crystals;
[0007] S2. Preparation before high-pressure experiment: Use diamond anvil to pre-press the steel sheet, load an appropriate amount of chiral perovskite single crystal sample into the sample cavity, load ruby, drip pressure-transmitting medium silicone oil, buckle the upper and lower diamond anvil surfaces, and complete the sample loading;
[0008] S3. Calibrate the pressure: Use the spectral method to calibrate the pressure. First, aim the laser at the ruby, record the position of the ruby's fluorescence peak, and then determine the internal hydrostatic pressure of the sample chamber based on the position of the fluorescence peak.
[0009] S4. Conduct fluorescence and circularly polarized light tests: Place the pressurized sample in the light path of a fluorescence spectrometer or a circularly polarized fluorescence spectrometer for testing.
[0010] Preferably, the S1 specifically comprises the following steps:
[0011] 1) Prepare chiral ammonium salt; react chiral amine with HBr in ethanol, put RR-DACH and ethanol into a round-bottom flask and mix them evenly, place in an ice-water bath, add HBr aqueous solution into a dropping funnel and add it dropwise into the round-bottom flask, continue to react in an ice-water bath after the addition is complete, remove water and ethanol solution by rotary evaporation after the reaction is complete, wash and dry the crude salt;
[0012] 2) Synthesis of chiral perovskite single crystals: InBr3 and chiral ammonium salt are placed in a polytetrafluoroethylene lining of a reactor in a certain proportion, and then HBr aqueous solution is added as a reaction solvent. The sealed hydrothermal reactor is reacted at high temperature, and then cooled to room temperature at a constant rate. The mixture is allowed to stand and evaporate for 1 to 2 days, and large pieces of colorless and transparent crystals are precipitated to obtain chiral perovskite single crystals.
[0013] Preferably, in the preparation of the chiral ammonium salt, the chiral amine is left-handed cyclohexanediamine SS-DACH or right-handed cyclohexanediamine RR-DACH, and the mass fraction of the HBr aqueous solution is 13-38%.
[0014] The structural formula of chiral amine is:
[0015] Preferably, in the synthesized chiral perovskite single crystal, the ratio of InBr3 to chiral ammonium salt is 1:(0.5-6), and the addition ratio of HBr is 10-16 mL of HBr for every 4 mmol of InBr3; the high temperature reaction temperature is 90-130°C, the reaction time is 8-16 h, and the cooling rate is 2-10°C / h.
[0016] Preferably, in S2, after the pre-pressing of the steel sheet is completed, a laser puncher is used to punch holes in the indentations, and the diameter of the holes is 150 μm.
[0017] Preferably, in S3, locking is performed after each pressure calibration.
[0018] Preferably, in S4, the locked anvil is placed on an optical test light path, and the laser, diamond anvil pressure chamber and detector are ensured to be in a straight line. After adjusting the parameters of fluorescence and circularly polarized fluorescence tests, the test is performed;
[0019] In S1 to S4, chiral amine cyclohexanediamine (SS-DACH, RR-DACH) is reacted with HBr in ethanol to obtain the bromate of the chiral amine, which is reacted with InBr3 in HBr, and a chiral perovskite single crystal is obtained by cooling crystallization. This single crystal has a symmetrical circular dichroism spectrum, i.e., chiral properties, but weak fluorescence properties, and therefore does not have circularly polarized luminescence performance. Under high pressure, the chiral spatial structure and electronic structure of the single crystal are regulated, and the material exhibits bright cold white fluorescence. Due to the strong chirality and fluorescence properties at the same time, the chiral perovskite exhibits symmetrical circularly polarized luminescence characteristics, and the luminescence region is 380-740nm.
[0020] Therefore, the present invention provides a method for regulating the production of circularly polarized luminescence by chiral perovskite through pressure. The temperature drop crystallization method is simple to operate to synthesize perovskite single crystals. The obtained crystals have regular morphology and stable properties. The crystals have only weak fluorescence and therefore no circularly polarized fluorescence performance. Under the action of hydrostatic pressure, the chiral spatial structure in the perovskite changes, and the energy band structure changes at the same time, so that the crystal is transformed from an indirect band gap structure to a direct band gap structure, which is conducive to the radiation recombination of electrons, thereby enhancing the fluorescence intensity. As the pressure increases further, the crystal changes to a non-static state, and the chiral structure is gradually destroyed, resulting in a CPL signal and g lum The value decreases.
[0021] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Circularly polarized fluorescence spectra of (RR-DACH)2InBr7 under different pressures according to Example 1 of the present invention;
[0023] Figure 2 This is the circularly polarized fluorescence spectrum of (SS-DACH)2InBr7 under different pressures in Example 2 of the present invention. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.
[0025] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0026] Example 1
[0027] This example is used to prepare chiral perovskite (RR-DACH)2InBr7, which produces an enhanced CPL signal under pressure regulation.
[0028] Preparation of chiral ammonium salt: 5 mL of RR-DACH and 30 mL of ethanol were placed in a round-bottom flask and mixed evenly. The round-bottom flask was placed in an ice-water bath. 10 mL of HBr aqueous solution (13-38% wt) was added to the dropping funnel and added dropwise to the round-bottom flask. After the addition was completed, the reaction was continued in the ice-water bath for 4 h. After the reaction was completed, the solvent was removed by rotary evaporation. The obtained crude salt RR-DACH·HBr was washed with ether 3-5 times and then dried in a vacuum drying oven at 60°C for use.
[0029] Preparation of chiral perovskite: 4 mmol InBr3 and 16 mmol RR-DACH·HBr salt were weighed and placed in the polytetrafluoroethylene lining of the reactor, and then 6 mL HBr aqueous solution was added as the reaction solvent. The sealed hydrothermal reactor was reacted at 130°C for 8 h, and the temperature was lowered at a rate of 2°C / h, and large pieces of colorless and transparent crystals precipitated.
[0030] Fluorescence and circularly polarized light testing under pressure control: First, use a diamond anvil to pre-press the T301 steel sheet, then use a laser puncher to punch holes in the indentation with a diameter of 150μm; fill an appropriate amount of crystal into the sample cavity, and snap the upper and lower diamond anvil surfaces together to complete the sample loading. Place the anvil in the test light path to calibrate the pressure, lock the pressure after each calibration, and place the diamond anvil in the fluorescence and circularly polarized light test light path for testing.
[0031] Through testing, the chiral perovskite prepared under pressure regulation has a PLQY of 50.16%, and the CPL signal first increases and then weakens. lum The value can reach 5.0×10-3 .
[0032] like Figure 1 As shown, the fluorescence of (RR-DACH)2InBr7 increases when the hydrostatic pressure reaches 2 GPa. When the pressure reaches 4 GPa, the fluorescence intensity reaches the maximum, and then gradually decreases with the increase of pressure. When the pressure increases to 8 GPa, the fluorescence is too weak to be visible to the naked eye.
[0033] During the application of hydrostatic pressure, circularly polarized light signals were gradually detected due to the enhancement of fluorescence, and the circularly polarized light signals also showed a trend of first strengthening and then weakening with the increase of pressure. The highest asymmetry factor g was obtained at 4 GPa pressure. lum , up to 5.0×10 -3 .
[0034] Example 2
[0035] This example is used to prepare chiral perovskite (SS-DACH)2InBr7, which produces an enhanced CPL signal under pressure regulation.
[0036] Preparation of chiral ammonium salt: 6 g of SS-DACH (0.06 mmol) and 35 mL of ethanol were placed in a round-bottom flask and mixed evenly. The round-bottom flask was placed in an ice-water bath. 10 mL of HBr aqueous solution (13-38% wt) was added to the dropping funnel and added dropwise to the round-bottom flask. After the addition was completed, the reaction was continued in an ice-water bath for 4 h. Ammonium salt precipitated from ethanol during the reaction. After the reaction was completed, the solvent was removed by suction filtration. The crude salt was washed with ethanol 3-5 times and then dried in a vacuum drying oven at 60°C for use.
[0037] Preparation of chiral perovskite: Weigh 4mmol InBr3 and 10mmol SS-DACH bromate and place them in the polytetrafluoroethylene lining of the reactor, then add 16mL HBr as the reaction solvent, and seal the hydrothermal reactor to react at 130℃ for 12h, and cool it at a cooling rate of 2℃ / h, and large pieces of colorless transparent crystals precipitate.
[0038] Fluorescence and circularly polarized light testing under pressure control: First, use a diamond anvil to pre-press the T301 steel sheet, with an indentation of 30 to 70 μm; then use a laser puncher to punch holes in the indentation, with a hole diameter of 150 μm; use ethanol to clean the gasket and diamond; reset the gasket with holes to the lower anvil surface of the diamond anvil press to form a sample cavity, then fill the sample cavity with an appropriate amount of crystals, put rubies in appropriate positions, and drip pressure-transmitting medium silicone oil. Snap the upper and lower diamond anvil surfaces together to complete the sample loading. Place the anvil in the test light path to calibrate the pressure, lock the pressure after each pressure calibration, and place the diamond anvil in the fluorescence and circularly polarized light test light path for testing.
[0039] like Figure 2 As shown, the fluorescence of (SS-DACH)2InBr7 increases when the hydrostatic pressure reaches 2 GPa. When the pressure reaches 4 GPa, the fluorescence intensity reaches the maximum, and then gradually decreases with the increase of pressure. When the pressure increases to 8 GPa, the fluorescence is too weak to be visible to the naked eye.
[0040] In the process of applying hydrostatic pressure, circularly polarized light signals were gradually detected due to the enhancement of fluorescence, and the circularly polarized light signals also showed a trend of first strengthening and then weakening with the increase of pressure. Through testing, the prepared chiral perovskite had a PLQY of 48.33% under pressure regulation, and the CPL signal first strengthened and then weakened. lum The value can reach 4.7×10 -3 .
[0041] Comparative Example 1
[0042] This example is used to prepare chiral perovskite (SS-DACH)2InBr7 and its pressure response.
[0043] Preparation of chiral ammonium salt: 6 g of SS-DACH (0.06 mmol) and 35 mL of ethanol were placed in a round-bottom flask and mixed evenly. The round-bottom flask was placed in an ice-water bath. 10 mL of HBr aqueous solution (13-38% wt) was added to the dropping funnel and added dropwise to the round-bottom flask. After the addition was completed, the reaction was continued in an ice-water bath for 4 h. Ammonium salt precipitated from ethanol during the reaction. After the reaction was completed, the solvent was removed by suction filtration. The crude salt was washed with ethanol 3-5 times and then dried in a vacuum drying oven at 60°C for use.
[0044] Preparation of chiral perovskite: Weigh 4 mmol InBr3 and 4 mmol SS-DACH bromate and place them in the polytetrafluoroethylene liner of the reactor, then add 8 mL HBr as the reaction solvent, and seal the hydrothermal reactor to react at 130°C for 12 h, and cool it at a cooling rate of 2°C / h to obtain a white powder.
[0045] Fluorescence and circularly polarized light testing under pressure control: First, use a diamond anvil to pre-press the T301 steel sheet, with an indentation of 30 to 70 μm; then use a laser puncher to punch holes in the indentation, with a hole diameter of 150 μm; use ethanol to clean the gasket and diamond; reset the gasket with holes to the lower anvil surface of the diamond anvil press to form a sample cavity, then fill the sample cavity with an appropriate amount of crystals, put rubies in appropriate positions, and drip pressure-transmitting medium silicone oil. Snap the upper and lower diamond anvil surfaces together to complete the sample loading. Place the anvil in the test light path to calibrate the pressure, lock the pressure after each pressure calibration, and place the diamond anvil in the fluorescence and circularly polarized light test light path for testing.
[0046] Through testing, the prepared chiral perovskite had a PLQY of 5% under pressure regulation, and no circularly polarized light signal was observed.
[0047] Therefore, the present invention provides a method for regulating chiral perovskite to produce circularly polarized luminescence by pressure, and obtains a chiral perovskite single crystal by a cooling crystallization method. The single crystal has a symmetrical circular dichroism spectrum, that is, a chiral property, but a weak fluorescence property and does not have a circularly polarized luminescence performance. Under high pressure, the chiral spatial structure and electronic structure of the single crystal are regulated, so that the single crystal has both chirality and fluorescence properties, thereby showing symmetrical circularly polarized luminescence characteristics, a luminescent region of 380-740nm, and an asymmetry factor g lum Up to 5.0×10 -3 , which is of great significance to the study of circularly polarized luminescence properties.
[0048] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for producing circularly polarized luminescence by regulating chiral perovskite through pressure. It is characterized in that The following steps are involved: S1. Preparation of chiral perovskite single crystals: 1) Preparation of chiral ammonium salt: react chiral amine with HBr in ethanol, remove water and ethanol solution after the reaction, wash and dry the crude salt; The chiral amines are left-handed cyclohexanediamine SS-DACH and right-handed cyclohexanediamine RR-DACH, with the structural formula being: The mass fraction of HBr aqueous solution is 13-38%; 2) Synthesis of chiral perovskite single crystals: InBr3 and chiral ammonium salt are added to HBr in a certain proportion, reacted at high temperature, then cooled to room temperature at a constant rate, and allowed to stand for 1 to 2 days for volatilization, and large pieces of colorless and transparent crystals are precipitated to obtain chiral perovskite single crystals; S2. Preparation before high-pressure experiment: Use diamond anvil to pre-press the steel sheet, load an appropriate amount of chiral perovskite single crystal sample into the sample cavity, load ruby, drip pressure-transmitting medium silicone oil, buckle the upper and lower diamond anvil surfaces, and complete the sample loading; S3. Calibrate the pressure: Use the spectral method to calibrate the pressure. Lock the pressure after each calibration. First, aim the laser at the ruby, record the position of the fluorescence peak of the ruby, and then determine the internal hydrostatic pressure of the sample chamber according to the position of the fluorescence peak. S4. Conduct fluorescence and circularly polarized light tests: Place the pressurized sample in the light path of a fluorescence spectrometer or a circularly polarized fluorescence spectrometer for testing.
2. A method for producing circularly polarized light by regulating chiral perovskite through pressure according to claim 1, Features: In the synthesized chiral perovskite single crystal, InBr 3 The ratio of HBr to chiral ammonium salt is 1:(0.5-6), and the addition ratio of HBr is 4 mmol of InBr 3 Add 10-16 mL of HBr; the high temperature reaction temperature is 90-130°C, the reaction time is 8-16h, and the cooling rate is 2-10°C / h.
3. The method for producing circularly polarized light by regulating chiral perovskite through pressure according to claim 2, Features: In S2, after the pre-pressing of the steel sheet is completed, a laser puncher is used to punch holes in the indentations, and the diameter of the holes is 150 μm.
4. The method of producing circularly polarized light by regulating chiral perovskite through pressure according to claim 3, Features: In S4, the locked anvil is placed on the optical test light path, and the laser, diamond anvil pressure chamber and detector are ensured to be in a straight line. After adjusting the parameters of fluorescence and circularly polarized fluorescence testing, the test is performed.