Antioxidant and preparation method thereof, film prepared based on the antioxidant and method thereof

By using components such as phosphorus-aluminum molecular sieve, modified titanium dioxide/phosphoraluminum composite and modified mesoporous nanosilicon dioxide in polyethylene films, antioxidants with flame retardancy and breathability are prepared to solve the problem of The problems of aging and insufficient flame retardancy of polyethylene films are achieved, and better anti-oxidation aging and flame retardancy are achieved.

CN118307850BActive Publication Date: 2024-11-15HAIAN HO CHI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410608305.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-11-15
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

Existing polyethylene films are prone to aging during use, reduce mechanical properties, and lack other performance improvements such as flame retardancy.

Method used

Using an antioxidant preparation method, the synergistic effect of components such as phospho-aluminum molecular sieve, modified titanium dioxide/phospho-aluminum composite, modified mesoporous nanosilicon dioxide and ferrocene chaltone was prepared. A flammable and breathable antioxidant is melt blended with a polyethylene film matrix to obtain a film with excellent antioxidant aging properties and flame retardant properties by blow molding.

Benefits of technology

It significantly improves the antioxidant aging and flame retardant properties of polyethylene films, while maintaining breathability, extending the service life of the film and improving its value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307850B_ABST
    Figure CN118307850B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polymer composite materials, and discloses an antioxidant and a preparation method thereof, a film prepared based on the antioxidant and a method thereof. The preparation method of the antioxidant comprises: mixing γ-aminopropyltriethoxysilane with a titanium dioxide / aluminum phosphate molecular sieve composite material, and continuously reacting the obtained modified titanium dioxide / aluminum phosphate molecular sieve composite material with ferrocene chalcone to obtain an antioxidant component A; mixing modified mesoporous nano-silica with 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride to obtain an antioxidant component B; and mixing the antioxidant component A, the antioxidant component B, and an antioxidant 168 to obtain an antioxidant. The antioxidant and linear low-density polyethylene are melt-extruded and granulated, and the obtained antioxidant masterbatch is melt-blended with low-density polyethylene, linear low-density polyethylene, metallocene linear low-density polyethylene, and maleic anhydride grafted polyolefin elastomer, extruded, and blown to obtain a film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer composite materials, and in particular to an antioxidant and a preparation method thereof, and a film prepared based on the antioxidant and a method thereof. Background Art

[0002] Polyethylene (PE) has many excellent properties such as light weight, low price, heat resistance, easy processing, good chemical corrosion resistance, etc. Therefore, it is widely used in the film field and can be used to prepare architectural membranes. According to the synthesis process and molecular weight of polyethylene, polyethylene can also be divided into low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), high-density polyethylene (HDPE), ultra-high molecular weight polyethylene (UHMW-PE), and metallocene polyethylene (mLLDPE).

[0003] As a polymer plastic, polyethylene is easy to burn and has a melting drop phenomenon when burning, which limits the application of polyethylene. In addition, during the storage and use of polyethylene film, it will inevitably be disturbed by external factors such as light and heat and age, causing it to gradually become hard and brittle, discolored, cracked, and sticky, which will reduce the mechanical properties of the polyethylene film and eventually lose its use value. Therefore, additives that can delay its aging, namely antioxidants, are currently added during the preparation of polyethylene film. Antioxidants can not only extend the service life of polyethylene film, but also improve its use value. The development of multifunctional antioxidants is the current mainstream development direction of new antioxidants.

[0004] Prior art, such as Chinese patent application CN106633325A, discloses a polyethylene composition and a durable film, which improves the aging resistance of the polyethylene film by adding an antioxidant to the polyethylene matrix resin. Although the polyethylene film prepared by the method has excellent aging resistance, high tensile strength and puncture resistance, and low haze, it does not improve other properties of the polyethylene film, such as flame retardancy. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an antioxidant and a preparation method thereof, a film prepared based on the antioxidant and a method thereof. The antioxidant has excellent antioxidant properties. The film prepared based on the antioxidant prepared by the present invention not only has excellent antioxidant properties, but also has flame retardancy and air permeability.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing an antioxidant comprises the following steps:

[0008] Step (1), mixing phosphoric acid aqueous solution, aluminum isopropoxide and water uniformly, adding cyclohexylamine, crystallizing, and after the crystallization is completed, cooling, filtering, washing, drying, and calcining for the first time to obtain a phosphorus aluminum molecular sieve;

[0009] Tetrabutyl titanate, hydrochloric acid aqueous solution and ethanol are mixed, and the ethanol aqueous solution is added dropwise. After the addition is completed, a phosphorus aluminum molecular sieve is added, and a first reaction is performed. After the reaction is completed, the reaction is dried and a second calcination is performed to obtain a titanium dioxide / phosphorus aluminum molecular sieve composite material;

[0010] Mixing γ-aminopropyltriethoxysilane, toluene and titanium dioxide / aluminum phosphate molecular sieve composite material, reacting for the second time, cooling, centrifuging, filtering, washing and drying after the reaction is completed to obtain a modified titanium dioxide / aluminum phosphate molecular sieve composite material;

[0011] Step (2), mixing acetylferrocene, ethanol aqueous solution and sodium hydroxide aqueous solution by ultrasonication, adding benzaldehyde dropwise, and after the addition is complete, performing a first reaction. After the reaction is complete, filtering, washing, purifying and drying are performed to obtain ferrocene chalcone;

[0012] The modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide and ethanol are mixed by ultrasonication, and ferrocene chalcone is added to react for the second time. After the reaction is completed, the mixture is filtered, washed to neutrality, and dried to obtain an antioxidant component A;

[0013] Step (3), mixing the mesoporous nano-silica with ethanol and sonicating, adding the dopamine hydrochloride solution dropwise, and performing a first reaction after the addition is complete. After the reaction is complete, filtering, washing, and drying are performed to obtain modified mesoporous nano-silica;

[0014] The modified mesoporous nano-silica and toluene are mixed by ultrasonication, triethylamine is added, and a mixed solution of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene is added dropwise. After the addition is completed, a second reaction is performed. After the reaction is completed, the mixture is filtered, washed, and dried to obtain an antioxidant component B.

[0015] The antioxidant component A, the antioxidant component B and the antioxidant 168 are mixed to obtain an antioxidant.

[0016] Preferably, in step (1), the mass ratio of phosphoric acid aqueous solution, aluminum isopropoxide, water and cyclohexylamine is 16-17:28-30:160-180:7.4-7.6, the phosphoric acid aqueous solution is 85wt% phosphoric acid aqueous solution; the crystallization conditions are: crystallization at a temperature of 180-200°C for 96-100h; the first calcination conditions are: first calcination at a temperature of 520-550°C for 6-8h.

[0017] Preferably, in step (1), the mass ratio of tetrabutyl titanate, hydrochloric acid aqueous solution, ethanol, ethanol aqueous solution, and phosphorus aluminum molecular sieve is 2:0.11-0.12:4.8-5:2.2-2.3:1-1.5, the hydrochloric acid aqueous solution is a 36wt% hydrochloric acid aqueous solution, and the ethanol aqueous solution is a 75vol% ethanol aqueous solution; the dropping time is 10-15min; the first reaction condition is: the first reaction is at room temperature for 12-18h; the second calcination condition is: the second calcination is at a temperature of 500-520°C for 1.5-2h.

[0018] Preferably, in step (1), the mass ratio of γ-aminopropyltriethoxysilane, toluene and titanium dioxide / aluminum phosphate molecular sieve composite material is 4.7-5:40-50:10-12; and the second reaction conditions are: in a nitrogen atmosphere, at a temperature of 70-80° C., for 20-24 hours.

[0019] Preferably, the washing operation is: taking the filter cake, adding toluene and methanol in an amount 5-8 times the mass of the filter cake, and washing three times in sequence.

[0020] Preferably, in step (2), the mass ratio of acetylferrocene, ethanol aqueous solution, sodium hydroxide aqueous solution and benzaldehyde is 13.5-15:480-530:200-220:18-20, the ethanol aqueous solution is 95wt% ethanol aqueous solution, and the sodium hydroxide aqueous solution is 9wt% sodium hydroxide aqueous solution; the dripping conditions are: dripping at 20°C for 20-30min; the first reaction conditions are: the first reaction at 20-30°C for 1-1.5h.

[0021] Preferably, the purification operation is: mixing and dissolving the reaction product obtained after washing with a 50wt% ethanol aqueous solution at 60°C to form a saturated solution, cooling the saturated solution to 0°C, filtering, taking the filter cake, and repeating the dissolving, cooling, and filtering operations.

[0022] Preferably, in step (2), the mass ratio of the modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, ethanol, and ferrocene chalcone is 60-70:2.5-3:260-300:3-3.5; and the second reaction conditions are: in a nitrogen atmosphere, at a temperature of 70-80°C for 6-8h.

[0023] Preferably, the washing liquid used in the washing operation comprises ethanol.

[0024] Preferably, in step (3), the mass ratio of mesoporous nano-silica, ethanol and dopamine hydrochloride solution is 3:250-300:45-50; the first reaction conditions are: in a nitrogen atmosphere, at a temperature of 45-50° C. for 6-7 hours.

[0025] Furthermore, the dopamine hydrochloride solution is prepared by mixing dopamine hydrochloride and ethanol in a mass ratio of 3:40.

[0026] Preferably, in the step (3), the mass ratio of modified mesoporous nano-silica, toluene, triethylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride is 8-10:450-500:1.8-2:0.8-1; the dripping conditions of the 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution are: dripping at 0-5°C for 20-30min, and the second reaction conditions are: the second reaction is carried out in a nitrogen atmosphere at 0-5°C for 6-8h; the mass ratio of antioxidant component A, antioxidant component B and antioxidant 168 is 5-8:5-8:3-5.

[0027] Preferably, the scrubbing liquid used in the scrubbing operation comprises tetrahydrofuran.

[0028] Furthermore, the 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution is prepared by mixing 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and toluene solution in a mass ratio of 3.5:26.

[0029] Preferably, an antioxidant is prepared by the antioxidant preparation method as described above.

[0030] The present invention discloses a method for preparing a film using the above antioxidant, comprising the following steps:

[0031] The antioxidant is melt-blended with linear low-density polyethylene, extruded, and granulated to obtain an antioxidant masterbatch;

[0032] The low-density polyethylene, linear low-density polyethylene, metallocene linear low-density polyethylene, maleic anhydride grafted polyolefin elastomer and antioxidant masterbatch are melt-blended, extruded, blow-molded, trimmed and rolled to obtain a film.

[0033] Preferably, in the preparation process of the antioxidant masterbatch: the mass ratio of antioxidant to linear low-density polyethylene is 15-20:60-80; the melt blending conditions are: melt blending at a temperature of 140-150°C; and the extrusion conditions are: extrusion at a speed of 20-30r / min and a temperature of 155-165°C.

[0034] Preferably, in the preparation process of the film: the mass ratio of low-density polyethylene, linear low-density polyethylene, metallocene linear low-density polyethylene, maleic anhydride grafted polyolefin elastomer, and antioxidant masterbatch is 90-100:500-550:250-300:60-70:350-450; the conditions for melt blending are: melt blending at a temperature of 140-150°C; the extrusion conditions are: extrusion through a twin-screw extruder at a screw speed of 30-40r / min, a zone temperature of 108-112°C, a zone temperature of 148-152°C, a zone temperature of 158-162°C, and a die temperature of 148-152°C; the conditions for blow molding are: blow molding at a temperature of 170-180°C by a blow molding film unit.

[0035] Preferably, a film is prepared using the film preparation method as described above.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] Molecular sieves are a porous material. When added to polymers, they can not only serve as nucleating agents to improve the mechanical properties of the film, but also improve the air permeability of the film due to the presence of their porous structure. Phosphorus-aluminum molecular sieves contain phosphorus elements, and can enhance the flame retardant properties of polymers by catalyzing the cross-linking of polymer composites into carbon during the combustion process, improving the quality of residual carbon, and the like. The present invention uses a sol-gel method to load titanium dioxide particles with ultraviolet absorption effect on the surface of the phosphorus-aluminum molecular sieve, effectively avoiding the agglomeration of titanium dioxide and increasing the stability of titanium dioxide. The obtained titanium dioxide / phosphorus-aluminum molecular sieve composite material not only has a flame retardant effect, but can also be used as an antioxidant component to improve the anti-oxidation and aging ability of the polymer.

[0038] Ferrocene is an organic transition metal compound with aromatic properties. Its special structure makes it have high thermal stability and chemical stability. It has the functions of eliminating smoke and promoting carbonization of general iron compounds, and can improve the combustion performance and melting drop phenomenon of polymers. The present invention obtains ferrocene chalcone with carbon-carbon double bond and benzene ring structure by condensation reaction of acetyl ferrocene and benzaldehyde, and grafts it with modified titanium dioxide / phosphorus aluminum molecular sieve composite material with amino group on the surface through Michael addition reaction. The obtained antioxidant component A has better thermal stability and flame retardancy, and has good dispersibility in the matrix.

[0039] The present invention performs surface treatment on nano titanium dioxide by dopamine hydrochloride to obtain modified mesoporous nano silica having dopamine hydrochloride on the surface, and the organic amine hydrochloride group on the surface of the modified mesoporous nano silica undergoes an amidation reaction with the acyl chloride group of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, thereby grafting the antioxidant hindered amine functional group on the mesoporous nano silica. The mesoporous nano silica in the obtained antioxidant component B is used as a carrier to reduce the migration of the antioxidant functional group in the polymer matrix, and the porous structure of the mesoporous nano silica can cooperate with the phosphorus aluminum molecular sieve to improve the air permeability of the film. The present invention melt blends the antioxidant component A, the antioxidant component B, the antioxidant 168 and the polymer matrix, and blows the film. In the obtained film, the hindered phenol group in the antioxidant component B and the phosphite structure in the antioxidant 168 have a synergistic antioxidant effect, and since the antioxidant 168 is a phosphite antioxidant and has phosphorus elements, the flame retardant effect of the polymer can be further improved. Through the synergistic effect of various components, the prepared film has better anti-oxidation and aging properties and flame retardancy. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a process flow chart of preparing an antioxidant and a film prepared based on the antioxidant in the present invention;

[0041] Figure 2 It is a line graph of MD tensile strength retention rate of Examples 4-6 and Comparative Examples 3-4 in the performance test of the present invention;

[0042] Figure 3 It is a line graph of TD tensile strength retention rate of Examples 4-6 and Comparative Examples 3-4 in the performance test of the present invention;

[0043] Figure 4 It is a line graph of the limiting oxygen index of Examples 4-6 and Comparative Examples 3-4 in the performance test of the present invention. DETAILED DESCRIPTION

[0044] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0045] Example 1: This example discloses a method for preparing an antioxidant, comprising the following steps:

[0046] Step (1), 85wt% phosphoric acid aqueous solution, aluminum isopropoxide, and water are uniformly mixed, cyclohexylamine is added, the mass ratio of 85wt% phosphoric acid aqueous solution, aluminum isopropoxide, water, and cyclohexylamine is 16:28:160:7.4, crystallization is carried out at 180°C for 100h, after the crystallization is completed, cooling to room temperature, filtering, taking the filter cake, adding water 5 times the mass of the filter cake for washing, drying at 100°C for 8h, and after drying, calcining at 520°C for 8h to obtain a phosphorus aluminum molecular sieve;

[0047] Tetrabutyl titanate, 36 wt% hydrochloric acid aqueous solution and ethanol are mixed, 75 vol% ethanol aqueous solution is added dropwise for 10 min, after the addition is completed, phosphate aluminum molecular sieve is added, the mass ratio of tetrabutyl titanate, 36 wt% hydrochloric acid aqueous solution, ethanol, 75 vol% ethanol aqueous solution and phosphate aluminum molecular sieve is 2:0.11:4.8:2.2:1, the first reaction is carried out at room temperature for 12 h, after the reaction is completed, it is dried at 90°C for 24 h, and calcined at 500°C for 2 h to obtain a titanium dioxide / phosphate aluminum molecular sieve composite material;

[0048] γ-aminopropyltriethoxysilane, toluene, and titanium dioxide / phosphorus aluminum molecular sieve composite material were mixed in a mass ratio of 4.7:40:10, and reacted for a second time in a nitrogen atmosphere at 70°C for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, filtered, and the filter cake was taken. Toluene and methanol with a mass of 5 times that of the filter cake were added and washed three times in sequence, and dried at 90°C for 18 hours to obtain a modified titanium dioxide / phosphorus aluminum molecular sieve composite material;

[0049] Step (2), acetylferrocene, 95wt% ethanol aqueous solution, and 9wt% sodium hydroxide aqueous solution are mixed and ultrasonically treated for 15min, and benzaldehyde is added dropwise at a temperature of 20°C, wherein the mass ratio of acetylferrocene, 95wt% ethanol aqueous solution, 9wt% sodium hydroxide aqueous solution, and benzaldehyde is 13.5:480:200:18, and the dropping time is 20min. After the dropping is completed, the first reaction is carried out at a temperature of 20°C for 1.5h. After the reaction is completed, the filter is filtered, the filter cake is taken, and water 5 times the mass of the filter cake is added to wash to obtain a reaction product, the reaction product is mixed and dissolved with a 50wt% ethanol aqueous solution at a temperature of 60°C to form a saturated solution, the saturated solution is cooled to 0°C, filtered, the filter cake is taken, and the dissolution, cooling, and filtering operations are repeated once, and the filter cake is dried at a temperature of 70°C for 28h to obtain ferrocene chalcone;

[0050] The modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, and ethanol were mixed by ultrasound for 20 minutes, and ferrocene chalcone was added, and the mass ratio of the modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, ethanol, and ferrocene chalcone was 60:2.5:260:3. The ... were reacted for a second time at 70°C in a nitrogen atmosphere for 8 hours. After the reaction was completed, the filter was filtered, and the filter cake was taken. Ethanol 5 times the mass of the filter cake was added to wash until neutral, and dried at 50°C for 24 hours to obtain an antioxidant component A.

[0051] Step (3), mixing the mesoporous nano-silica with ethanol and ultrasonically adding the dopamine hydrochloride solution dropwise for 15 min. After the addition is complete, reacting for the first time in a nitrogen atmosphere at 45° C. for 7 h. After the reaction is complete, filtering and taking the filter cake, washing it three times with ethanol 5 times the mass of the filter cake, and drying it at 50° C. for 28 h to obtain modified mesoporous nano-silica;

[0052] Wherein, the dopamine hydrochloride solution is prepared by mixing dopamine hydrochloride and ethanol in a mass ratio of 3:40; the mass ratio of mesoporous nano-silica, ethanol, and dopamine hydrochloride solution is 3:250:45;

[0053] The modified mesoporous nano-silica was mixed with toluene and ultrasonicated for 10 minutes, triethylamine was added, and a 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution was added dropwise at 0°C for 30 minutes. After the addition was completed, a second reaction was carried out in a nitrogen atmosphere at 0°C for 8 hours. After the reaction was completed, the filter cake was filtered and washed three times with tetrahydrofuran 5 times the mass of the filter cake, and dried at 50°C for 24 hours to obtain an antioxidant component B.

[0054] The mass ratio of modified mesoporous nano-silica, toluene, triethylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride is 8:450:1.8:0.8; the 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution is prepared by mixing 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and toluene solution in a mass ratio of 3.5:26;

[0055] The antioxidant component A, the antioxidant component B and the antioxidant 168 were mixed in a mass ratio of 5:5:3 to obtain an antioxidant.

[0056] Example 2: This example discloses a method for preparing an antioxidant, comprising the following steps:

[0057] Step (1), 85wt% phosphoric acid aqueous solution, aluminum isopropoxide, and water are uniformly mixed, cyclohexylamine is added, the mass ratio of 85wt% phosphoric acid aqueous solution, aluminum isopropoxide, water, and cyclohexylamine is 16.5:29:170:7.5, crystallization is carried out at 190°C for 98h, after the crystallization is completed, cooling to room temperature, filtering, taking the filter cake, adding water 6 times the mass of the filter cake for washing, drying at 110°C for 7h, and after drying, calcining at 535°C for 7h to obtain a phosphorus aluminum molecular sieve;

[0058] Tetrabutyl titanate, 36 wt% hydrochloric acid aqueous solution and ethanol are mixed, 75 vol% ethanol aqueous solution is added dropwise for 12 min, after the addition is completed, phosphate aluminum molecular sieve is added, the mass ratio of tetrabutyl titanate, 36 wt% hydrochloric acid aqueous solution, ethanol, 75 vol% ethanol aqueous solution and phosphate aluminum molecular sieve is 2:0.115:4.9:2.25:1.2, the first reaction is carried out at room temperature for 15 h, after the reaction is completed, it is dried at 95 ° C for 21 h, and calcined at 510 ° C for 1.8 h to obtain a titanium dioxide / phosphate aluminum molecular sieve composite material;

[0059] γ-aminopropyltriethoxysilane, toluene, and titanium dioxide / phosphorus aluminum molecular sieve composite material were mixed in a mass ratio of 4.8:45:11, and reacted for a second time in a nitrogen atmosphere at 75°C for 22 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, filtered, and the filter cake was taken. Toluene and methanol with a mass of 6 times that of the filter cake were added to wash the mixture three times in sequence, and dried at 100°C for 15 hours to obtain a modified titanium dioxide / phosphorus aluminum molecular sieve composite material.

[0060] Step (2), acetylferrocene, 95wt% ethanol aqueous solution, and 9wt% sodium hydroxide aqueous solution are mixed and ultrasonically treated for 18min, and benzaldehyde is added dropwise at a temperature of 20°C, wherein the mass ratio of acetylferrocene, 95wt% ethanol aqueous solution, 9wt% sodium hydroxide aqueous solution, and benzaldehyde is 14:500:210:19, and the dropping time is 25min. After the dropping is completed, the first reaction is carried out at a temperature of 25°C for 1.2h. After the reaction is completed, the filter is filtered, the filter cake is taken, and water 5-8 times the mass of the filter cake is added for washing to obtain a reaction product, the reaction product is mixed and dissolved with a 50wt% ethanol aqueous solution at a temperature of 60°C to form a saturated solution, the saturated solution is cooled to 0°C, filtered, the filter cake is taken, and the dissolution, cooling, and filtering operations are repeated once, and the filter cake is dried at a temperature of 75°C for 26h to obtain ferrocene chalcone;

[0061] The modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, and ethanol were mixed and ultrasonicated for 25 minutes, and ferrocene chalcone was added, and the mass ratio of the modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, ethanol, and ferrocene chalcone was 65:2.8:280:3.2. The ... were reacted for a second time in a nitrogen atmosphere at 75°C for 7 hours. After the reaction was completed, the filter was filtered, and the filter cake was taken. Ethanol 6 times the mass of the filter cake was added to wash until neutral, and dried at 55°C for 21 hours to obtain an antioxidant component A;

[0062] Step (3), mixing the mesoporous nano-silica with ethanol and ultrasonically adding the dopamine hydrochloride solution dropwise for 18 min. After the addition is complete, the first reaction is carried out in a nitrogen atmosphere at 48° C. for 6.5 h. After the reaction is complete, the filter is filtered to obtain the filter cake, and ethanol 6 times the mass of the filter cake is added to wash it three times, and then dried at 55° C. for 26 h to obtain the modified mesoporous nano-silica;

[0063] Wherein, the dopamine hydrochloride solution is prepared by mixing dopamine hydrochloride and ethanol in a mass ratio of 3:40; the mass ratio of mesoporous nano-silica, ethanol, and dopamine hydrochloride solution is 3:280:48;

[0064] The modified mesoporous nano-silica was mixed with toluene and ultrasonicated for 12 minutes, triethylamine was added, and a 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution was added dropwise at 2°C for 25 minutes. After the addition was completed, a second reaction was carried out in a nitrogen atmosphere at 2°C for 7 hours. After the reaction was completed, the filter cake was filtered and washed three times with tetrahydrofuran 5-8 times the mass of the filter cake, and dried at 55°C for 21 hours to obtain an antioxidant component B.

[0065] The mass ratio of modified mesoporous nano-silica, toluene, triethylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride is 9:480:1.9:0.9; the 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution is prepared by mixing 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and toluene solution in a mass ratio of 3.5:26;

[0066] The antioxidant component A, the antioxidant component B and the antioxidant 168 were mixed in a mass ratio of 6:6:4 to obtain an antioxidant.

[0067] Example 3: This example discloses a method for preparing an antioxidant, comprising the following steps:

[0068] Step (1), 85wt% phosphoric acid aqueous solution, aluminum isopropoxide, and water are uniformly mixed, cyclohexylamine is added, the mass ratio of 85wt% phosphoric acid aqueous solution, aluminum isopropoxide, water, and cyclohexylamine is 17:30:180:7.6, crystallization is carried out at 200°C for 96h, after the crystallization is completed, cooling to room temperature, filtering, taking the filter cake, adding water 8 times the mass of the filter cake for washing, drying at 120°C for 6h, and after drying, calcining at 550°C for 6h to obtain a phosphorus aluminum molecular sieve;

[0069] Tetrabutyl titanate, 36 wt% hydrochloric acid aqueous solution and ethanol are mixed, 75 vol% ethanol aqueous solution is added dropwise for 15 min, after the addition is completed, phosphate aluminum molecular sieve is added, the mass ratio of tetrabutyl titanate, 36 wt% hydrochloric acid aqueous solution, ethanol, 75 vol% ethanol aqueous solution and phosphate aluminum molecular sieve is 2:0.12:5:2.3:1.5, the first reaction is carried out at room temperature for 18 h, after the reaction is completed, it is dried at 100° C. for 18 h, and calcined at 520° C. for 1.5 h to obtain a titanium dioxide / phosphate aluminum molecular sieve composite material;

[0070] γ-aminopropyltriethoxysilane, toluene, and titanium dioxide / phosphorus aluminum molecular sieve composite material were mixed in a mass ratio of 5:50:12, and reacted for a second time in a nitrogen atmosphere at 80°C for 20 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, filtered, and the filter cake was taken. Toluene and methanol in an amount 8 times the mass of the filter cake were added and washed three times in sequence, and dried at 110°C for 12 hours to obtain a modified titanium dioxide / phosphorus aluminum molecular sieve composite material;

[0071] Step (2), acetylferrocene, 95wt% ethanol aqueous solution, and 9wt% sodium hydroxide aqueous solution are mixed and ultrasonically treated for 20min, and benzaldehyde is added dropwise at a temperature of 20°C, wherein the mass ratio of acetylferrocene, 95wt% ethanol aqueous solution, 9wt% sodium hydroxide aqueous solution, and benzaldehyde is 15:530:220:20, and the dropping time is 30min. After the dropping is completed, the first reaction is carried out at a temperature of 30°C for 1h. After the reaction is completed, suction filtration is performed, the filter cake is taken, and water 8 times the mass of the filter cake is added to wash to obtain a reaction product, the reaction product is mixed and dissolved with a 50wt% ethanol aqueous solution at a temperature of 60°C to form a saturated solution, the saturated solution is cooled to 0°C, filtered, the filter cake is taken, and the dissolution, cooling, and filtering operations are repeated once, and the filter cake is dried at a temperature of 80°C for 24h to obtain ferrocene chalcone;

[0072] The modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, and ethanol were mixed by ultrasound for 30 minutes, and ferrocene chalcone was added, and the mass ratio of the modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, ethanol, and ferrocene chalcone was 70:3:300:3.5. The ... were reacted for a second time at 80°C in a nitrogen atmosphere for 6 hours. After the reaction was completed, the filter was filtered, and the filter cake was taken. Ethanol 8 times the mass of the filter cake was added to wash until neutral, and dried at 60°C for 18 hours to obtain an antioxidant component A;

[0073] Step (3), mixing the mesoporous nano-silica with ethanol and ultrasonically adding the dopamine hydrochloride solution dropwise for 20 min. After the addition is completed, the first reaction is carried out in a nitrogen atmosphere at 50° C. for 6 h. After the reaction is completed, the filter is filtered to obtain the filter cake, and ethanol 8 times the mass of the filter cake is added to wash it three times, and then dried at 60° C. for 24 h to obtain the modified mesoporous nano-silica;

[0074] Wherein, the dopamine hydrochloride solution is prepared by mixing dopamine hydrochloride and ethanol in a mass ratio of 3:40; the mass ratio of mesoporous nano-silica, ethanol, and dopamine hydrochloride solution is 3:300:50;

[0075] The modified mesoporous nano-silica was mixed with toluene and ultrasonicated for 15 minutes, triethylamine was added, and a 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution was added dropwise at 5°C for 20 minutes. After the addition was completed, a second reaction was carried out in a nitrogen atmosphere at 5°C for 6 hours. After the reaction was completed, the filter cake was filtered and washed three times with tetrahydrofuran 8 times the mass of the filter cake, and dried at 60°C for 18 hours to obtain an antioxidant component B.

[0076] The mass ratio of modified mesoporous nano-silica, toluene, triethylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride is 10:500:2:1; the 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution is prepared by mixing 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and toluene solution in a mass ratio of 3.5:26;

[0077] The antioxidant component A, the antioxidant component B and the antioxidant 168 were mixed in a mass ratio of 8:8:5 to obtain an antioxidant.

[0078] Embodiment 4: This embodiment discloses a method for preparing a thin film, comprising the following steps:

[0079] The antioxidant prepared in Example 1 and the linear low-density polyethylene were melt-blended at a mass ratio of 15:80 at a temperature of 140° C., and extruded and granulated at a speed of 20 r / min and a temperature of 155° C. to obtain an antioxidant masterbatch;

[0080] Low-density polyethylene, linear low-density polyethylene, metallocene linear low-density polyethylene, maleic anhydride grafted polyolefin elastomer, antioxidant masterbatch were mixed in a mass ratio of 100:550:300:70:350 The products are melt blended at 140°C, extruded through a twin-screw extruder at a screw speed of 30 r / min, a temperature of 108°C in the first zone, 148°C in the second zone, 158°C in the third zone, and a die head temperature of 148°C, and blown by a blown film unit at 170°C, trimmed, and wound to obtain a film.

[0081] Embodiment 5: This embodiment discloses a method for preparing a thin film, comprising the following steps:

[0082] The antioxidant prepared in Example 2 and the linear low-density polyethylene were melt-blended at a mass ratio of 18:70 at a temperature of 145°C, and extruded and granulated at a speed of 25 r / min and a temperature of 160°C to obtain an antioxidant masterbatch;

[0083] Low density polyethylene, linear low density polyethylene, metallocene linear low density polyethylene, maleic anhydride grafted polyolefin elastomer and antioxidant masterbatch are melt-blended at a mass ratio of 95:530:280:65:400 at a temperature of 145°C, extruded through a twin-screw extruder at a screw speed of 35 r / min, a temperature of 110°C in the first zone, 150°C in the second zone, 160°C in the third zone and a die head temperature of 150°C, blown by a blown film unit at a temperature of 175°C, trimmed and rolled to obtain a film.

[0084] Embodiment 6: This embodiment discloses a method for preparing a thin film, comprising the following steps:

[0085] The antioxidant prepared in Example 3 and the linear low-density polyethylene were melt-blended at a mass ratio of 20:60 at a temperature of 150° C., and extruded and granulated at a speed of 30 r / min and a temperature of 165° C. to obtain an antioxidant masterbatch;

[0086] Low density polyethylene, linear low density polyethylene, metallocene linear low density polyethylene, maleic anhydride grafted polyolefin elastomer and antioxidant masterbatch are melt-blended at a mass ratio of 90:500:250:60:450 at a temperature of 150°C, extruded through a twin-screw extruder at a screw speed of 40 r / min, a temperature of 112°C in the first zone, 152°C in the second zone, 162°C in the third zone and a die head temperature of 152°C, blown by a blown film unit at a temperature of 180°C, trimmed and rolled to obtain a film.

[0087] Comparative Example 1: This comparative example discloses a method for preparing an antioxidant, comprising the following steps:

[0088] Step (1), 85wt% phosphoric acid aqueous solution, aluminum isopropoxide, and water are uniformly mixed, cyclohexylamine is added, the mass ratio of 85wt% phosphoric acid aqueous solution, aluminum isopropoxide, water, and cyclohexylamine is 16:28:160:7.4, crystallization is carried out at 180°C for 100h, after the crystallization is completed, cooling to room temperature, filtering, taking the filter cake, adding water 5 times the mass of the filter cake for washing, drying at 100°C for 8h, and after drying, calcining at 520°C for 8h to obtain a phosphorus aluminum molecular sieve;

[0089] Tetrabutyl titanate, 36 wt% hydrochloric acid aqueous solution and ethanol are mixed, 75 vol% ethanol aqueous solution is added dropwise for 10 min, after the addition is completed, phosphate aluminum molecular sieve is added, the mass ratio of tetrabutyl titanate, 36 wt% hydrochloric acid aqueous solution, ethanol, 75 vol% ethanol aqueous solution and phosphate aluminum molecular sieve is 2:0.11:4.8:2.2:1, the first reaction is carried out at room temperature for 12 h, after the reaction is completed, it is dried at 90°C for 24 h, and calcined at 500°C for 2 h to obtain a titanium dioxide / phosphate aluminum molecular sieve composite material;

[0090] γ-aminopropyltriethoxysilane, toluene, and titanium dioxide / phosphorus aluminum molecular sieve composite material were mixed in a mass ratio of 4.7:40:10, and reacted for a second time in a nitrogen atmosphere at 70°C for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, filtered, and the filter cake was taken. Toluene and methanol with a mass of 5 times that of the filter cake were added and washed three times in sequence, and dried at 90°C for 18 hours to obtain a modified titanium dioxide / phosphorus aluminum molecular sieve composite material;

[0091] Step (2), acetylferrocene, 95wt% ethanol aqueous solution, and 9wt% sodium hydroxide aqueous solution are mixed and ultrasonically treated for 15min, and benzaldehyde is added dropwise at a temperature of 20°C, wherein the mass ratio of acetylferrocene, 95wt% ethanol aqueous solution, 9wt% sodium hydroxide aqueous solution, and benzaldehyde is 13.5:480:200:18, and the dropping time is 20min. After the dropping is completed, the first reaction is carried out at a temperature of 20°C for 1.5h. After the reaction is completed, the filter is filtered, the filter cake is taken, and water 5 times the mass of the filter cake is added to wash to obtain a reaction product, the reaction product is mixed and dissolved with a 50wt% ethanol aqueous solution at a temperature of 60°C to form a saturated solution, the saturated solution is cooled to 0°C, filtered, the filter cake is taken, and the dissolution, cooling, and filtering operations are repeated once, and the filter cake is dried at a temperature of 70°C for 28h to obtain ferrocene chalcone;

[0092] The modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, and ethanol were mixed by ultrasound for 20 minutes, and ferrocene chalcone was added, and the mass ratio of the modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, ethanol, and ferrocene chalcone was 60:2.5:260:3. The ... were reacted for a second time at 70°C in a nitrogen atmosphere for 8 hours. After the reaction was completed, the filter was filtered, and the filter cake was taken. Ethanol 5 times the mass of the filter cake was added to wash until neutral, and dried at 50°C for 24 hours to obtain an antioxidant component A.

[0093] The antioxidant component A and the antioxidant 168 were mixed in a mass ratio of 5:8 to obtain an antioxidant.

[0094] Comparative Example 2: This comparative example discloses a method for preparing an antioxidant, comprising the following steps:

[0095] The mesoporous nano-silica was mixed with ethanol by ultrasonication, and the dopamine hydrochloride solution was added dropwise for 15 minutes. After the addition was completed, the first reaction was carried out in a nitrogen atmosphere at 45°C for 7 hours. After the reaction was completed, the filter cake was taken out by suction, and ethanol 5 times the mass of the filter cake was added to wash it three times, and it was dried at 50°C for 28 hours to obtain modified mesoporous nano-silica;

[0096] Wherein, the dopamine hydrochloride solution is prepared by mixing dopamine hydrochloride and ethanol in a mass ratio of 3:40; the mass ratio of mesoporous nano-silica, ethanol, and dopamine hydrochloride solution is 3:250:45;

[0097] The modified mesoporous nano-silica was mixed with toluene and ultrasonicated for 10 minutes, triethylamine was added, and a 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution was added dropwise at 0°C for 30 minutes. After the addition was completed, a second reaction was carried out in a nitrogen atmosphere at 0°C for 8 hours. After the reaction was completed, the filter cake was filtered and washed three times with tetrahydrofuran 5 times the mass of the filter cake, and dried at 50°C for 24 hours to obtain an antioxidant component B.

[0098] The mass ratio of modified mesoporous nano-silica, toluene, triethylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride is 8:450:1.8:0.8; the 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution is prepared by mixing 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and toluene solution in a mass ratio of 3.5:26;

[0099] The antioxidant component B and the antioxidant 168 were mixed in a mass ratio of 5:8 to obtain an antioxidant.

[0100] Comparative Example 3: This comparative example discloses a method for preparing a thin film, comprising the following steps:

[0101] The antioxidant prepared in Comparative Example 1 was melt-blended with linear low-density polyethylene at a mass ratio of 15:80 at 140°C, and extruded and granulated at a speed of 20 r / min and a temperature of 155°C to obtain an antioxidant masterbatch;

[0102] Low density polyethylene, linear low density polyethylene, metallocene linear low density polyethylene, maleic anhydride grafted polyolefin elastomer and antioxidant masterbatch are melt-blended at a mass ratio of 100:550:300:70:350 at 140°C, extruded through a twin-screw extruder at a screw speed of 30 r / min, a temperature of 108°C in the first zone, 148°C in the second zone, 158°C in the third zone and a die head temperature of 148°C, blown by a blown film unit at 170°C, trimmed and rolled to obtain a film.

[0103] Comparative Example 4: This comparative example discloses a method for preparing a thin film, comprising the following steps:

[0104] The antioxidant prepared in Comparative Example 2 was melt-blended with linear low-density polyethylene at a mass ratio of 15:80 at a temperature of 140° C., and extruded and granulated at a speed of 20 r / min and a temperature of 155° C. to obtain an antioxidant masterbatch;

[0105] Low density polyethylene, linear low density polyethylene, metallocene linear low density polyethylene, maleic anhydride grafted polyolefin elastomer and antioxidant masterbatch are melt-blended at a mass ratio of 100:550:300:70:350 at 140°C, extruded through a twin-screw extruder at a screw speed of 30 r / min, a temperature of 108°C in the first zone, 148°C in the second zone, 158°C in the third zone and a die head temperature of 148°C, blown by a blown film unit at 170°C, trimmed and rolled to obtain a film.

[0106] In the above embodiments and comparative examples: the phosphoric acid aqueous solution is from Shandong Ranxi Chemical Technology Co., Ltd., the product name is concentrated phosphoric acid, the model is 85wt% concentrated phosphoric acid aqueous solution; aluminum isopropoxide is from Shandong Maofa Chemical Co., Ltd., CAS No.: 555-31-7; tetrabutyl titanate is from Shanghai McLean Biochemical Technology Co., Ltd., CAS No.: 5593-70-4; the hydrochloric acid aqueous solution is from AlfaAesar, the product name is concentrated hydrochloric acid, the model is 36wt% hydrochloric acid aqueous solution; ethanol is from Shanghai Yishi Chemical Co., Ltd., CAS No.: 64- 17-5; γ-aminopropyltriethoxysilane is from Guangdong Lvwei New Materials Technology Co., Ltd., CAS No.: 919-30-2; toluene is from Shanghai MacLean Biochemical Technology Co., Ltd., CAS No.: 108-88-3; methanol is from Dongguan Xunye Chemical Reagent Co., Ltd., CAS No.: 67-56-1; acetylferrocene is from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd., CAS No.: 1271-55-2; sodium hydroxide is from Anhui Jinyueguan New Materials Technology Co., Ltd., CAS No.: 1310-73- 2; benzaldehyde was from Hubei Mingtuo Biotechnology Co., Ltd., CAS number: 100-52-7; sodium ethoxide was from Shandong New Kinetic Energy Chemical Co., Ltd., CAS number: 141-52-6; mesoporous nano-silica was from Beijing Zhongke Keyou Technology Co., Ltd., particle size 200nm, pore size 2-3nm, CAS number: 7631-86-9; dopamine hydrochloride was from Shanghai McLean Biochemical Technology Co., Ltd., item number D806618, CAS number: 62-31-7; triethylamine was from Shanghai Aladdin Biochemical Technology Co., Ltd. Co., Ltd., CAS No.: 121-44-8; 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride comes from Yantai Shengkailun Biological Products Co., Ltd., CAS No.: 3062-64-4; tetrahydrofuran comes from Guangzhou Jiatu Technology Co., Ltd., CAS No.: 109-99-9; antioxidant 168 comes from Nanjing Milan Chemical Co., Ltd., CAS No.: 31570-04-4; low-density polyethylene comes from Dongguan Shenghua Plastic Raw Materials Co., Ltd., product name LDPE, brand Saudi ExxonMobil, model LDPE 165BW1; Saudi 165BW1; linear low-density polyethylene comes from Dongguan Hongchuang Plastic Co., Ltd., product name LLDPE, brand Saudi ExxonMobil, model LLDPE 1001XV; metallocene linear low-density polyethylene comes from Wuxi Huasu Plastic Chemical Co., Ltd., product name mLLDPE, brand American ExxonMobil, model mLLDPE 2010HA; maleic anhydride grafted polyolefin elastomer comes from Dongguan Kaiwan Engineering Plastic Raw Materials Co., Ltd., product name POE-g-MAH, brand Japan Mitsui, model POE-g-MAH MA8510; the blown film unit comes from Dalian Rubber and Plastic Machinery Co., Ltd., model SJ-FM30×28.

[0107] Test Example: The performance of the films prepared in Examples 4-6 and Comparative Examples 3-4 was tested. The specific test results are shown in Table 1:

[0108]

[0109] The tests of various indicators in Table 1 are based on the following standards: tensile strength is measured by GB / T1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets"; tensile strength retention rate is measured by GB / T16422.2-2014 "Plastics laboratory light source exposure test method Part 2: Xenon arc lamp"; limiting oxygen index is measured by ISO4589-1981 "Plastic oxygen index method for determining flammability"; air permeability is measured by GB / T1038-2000 "Plastic film and sheet gas permeability test method pressure difference method".

[0110] It can be seen from the test results in Table 1 that the film prepared based on the antioxidant prepared by the present invention not only has excellent antioxidant properties, but also has flame retardancy and air permeability.

[0111] Molecular sieves are porous materials that can be added to polymers to not only improve the mechanical properties of the film as a nucleating agent, but also improve the air permeability of the film due to the presence of its porous structure. Phosphorus-aluminum molecular sieves contain phosphorus elements and can enhance the flame retardant properties of polymers by catalyzing the cross-linking of polymer composites into carbon during the combustion process and improving the quality of residual carbon. The present invention loads titanium dioxide particles with ultraviolet absorption effect on the surface of the phosphorus-aluminum molecular sieve, and the obtained titanium dioxide / phosphorus-aluminum molecular sieve composite material not only has a flame retardant effect, but can also be used as an antioxidant component to improve the anti-oxidation and aging ability of the polymer.

[0112] Ferrocene is an organic transition metal compound with aromatic properties. Its special structure makes it have high thermal stability and chemical stability. It also has the functions of eliminating smoke and promoting carbonization of general iron compounds, and can improve the combustion performance and melting drop phenomenon of polymers. The present invention obtains ferrocene chalcone with a carbon-carbon double bond and a benzene ring structure by condensation reaction of acetylferrocene and benzaldehyde, and grafts it with a modified titanium dioxide / phosphorus aluminum molecular sieve composite material with amino groups on the surface through Michael addition reaction, and the obtained antioxidant component A has better thermal stability and flame retardancy.

[0113] The present invention performs surface treatment on nano titanium dioxide by dopamine hydrochloride to obtain modified mesoporous nano silica having dopamine hydrochloride on the surface, and the organic amine hydrochloride group on the surface of the modified mesoporous nano silica undergoes an amidation reaction with the acyl chloride group of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, thereby grafting the antioxidant hindered amine functional group on the mesoporous nano silica. The mesoporous nano silica in the obtained antioxidant component B is used as a carrier to reduce the migration of the antioxidant functional group in the polymer matrix, and the porous structure of the mesoporous nano silica can cooperate with the phosphorus aluminum molecular sieve to improve the air permeability of the film. The present invention melt blends the antioxidant component A, the antioxidant component B, the antioxidant 168 and the polymer matrix, and blows the film. In the obtained film, the hindered phenol group in the antioxidant component B and the phosphite structure in the antioxidant 168 have a synergistic antioxidant effect, and since the antioxidant 168 is a phosphite antioxidant and has phosphorus elements, the flame retardant effect of the polymer can be further improved. Through the synergistic effect of various components, the prepared film has better anti-oxidation and aging properties and flame retardancy.

[0114] In Comparative Example 1, the antioxidant contains only antioxidant component A and antioxidant 168, without adding antioxidant component B. Due to the lack of antioxidant effect of hindered amine functional groups in antioxidant component B and the role of mesoporous nano-silica in improving the air permeability of the film, the antioxidant properties and air permeability of Comparative Example 3 prepared from Comparative Example 1 are lower than those of the embodiment.

[0115] The antioxidant in Comparative Example 2 only contains antioxidant component B and antioxidant 168, and no antioxidant component A is added. Due to the lack of flame retardant effects of phosphoaluminum molecular sieve and ferrocene in antioxidant component A, antioxidant effect of titanium dioxide, and effect of phosphoaluminum molecular sieve in improving film permeability, the flame retardancy, antioxidant effect and air permeability of Comparative Example 4 prepared from Comparative Example 2 are all lower than those of the embodiment.

[0116] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing an antioxidant, It is characterized in that The following steps are involved: Step (1), mixing γ-aminopropyltriethoxysilane, toluene, and titanium dioxide / aluminum phosphate molecular sieve composite material, reacting, and after the reaction is completed, cooling, centrifuging, filtering, washing, and drying to obtain a modified titanium dioxide / aluminum phosphate molecular sieve composite material; Step (2), mixing the modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, and ethanol by ultrasonication, adding ferrocene chalcone, reacting, filtering after the reaction, washing to neutrality, and drying to obtain an antioxidant component A; Step (3), mixing the modified mesoporous nano-silica with toluene by ultrasonication, adding triethylamine, and dropping 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution, reacting after the dropwise addition is completed, and filtering after the reaction is completed, washing, and drying to obtain an antioxidant component B; Mixing antioxidant component A, antioxidant component B, and antioxidant 168 to obtain an antioxidant; the mass ratio of antioxidant component A, antioxidant component B, and antioxidant 168 is 5-8:5-8:3-5; In the step (1), the titanium dioxide / aluminum phosphate molecular sieve composite material is prepared by the following steps: The phosphoric acid aqueous solution, aluminum isopropoxide and water are uniformly mixed, cyclohexylamine is added, crystallization is carried out, and after the crystallization is completed, the mixture is cooled, filtered, washed, dried, and calcined for the first time to obtain a phosphorus aluminum molecular sieve; Tetrabutyl titanate, hydrochloric acid aqueous solution and ethanol are mixed, and the ethanol aqueous solution is added dropwise. After the addition is completed, a phosphorus aluminum molecular sieve is added to react. After the reaction is completed, the reaction is dried and calcined for the second time to obtain a titanium dioxide / phosphorus aluminum molecular sieve composite material; The mass ratio of phosphoric acid aqueous solution, aluminum isopropoxide, water and cyclohexylamine is 16-17:28-30:160-180:7.4-7.6, and the phosphoric acid aqueous solution is 85wt% phosphoric acid aqueous solution; the crystallization conditions are: crystallization at a temperature of 180-200°C for 96-100h; the first calcination conditions are: calcination at a temperature of 520-550°C for 6-8h; The mass ratio of tetrabutyl titanate, hydrochloric acid aqueous solution, ethanol, ethanol aqueous solution and phosphorus aluminum molecular sieve is 2:0.11-0.12:4.8-5:2.2-2.3:1-1.5, the hydrochloric acid aqueous solution is 36wt% hydrochloric acid aqueous solution, and the ethanol aqueous solution is 75vol% ethanol aqueous solution; the dropping time is 10-15min; the reaction conditions are: react at room temperature for 12-18h; the second calcination conditions are: calcination at a temperature of 500-520°C for 1.5-2h; In step (3), the modified mesoporous nano-silica is prepared by the following steps: The mesoporous nano-silica is mixed with ethanol by ultrasonication, and a dopamine hydrochloride solution is added dropwise. After the addition is completed, the mixture is reacted. After the reaction is completed, the mixture is filtered, washed, and dried to obtain modified mesoporous nano-silica. The mass ratio of mesoporous nano-silica, ethanol and dopamine hydrochloride solution is 3:250-300:45-50; the reaction conditions are: reacting in a nitrogen atmosphere at a temperature of 45-50° C. for 6-7 hours.

2. The method for preparing an antioxidant according to claim 1, It is characterized in that In the step (1), the mass ratio of γ-aminopropyltriethoxysilane, toluene and titanium dioxide / aluminum phosphate molecular sieve composite material is 4.7-5:40-50:10-12; the reaction conditions are: reacting in a nitrogen atmosphere at a temperature of 70-80° C. for 20-24 hours.

3. The method for preparing an antioxidant according to claim 1, It is characterized in that In the step (2), ferrocenechalcone is prepared by the following steps: Acetylferrocene, ethanol aqueous solution and sodium hydroxide aqueous solution are mixed by ultrasonication, benzaldehyde is added dropwise, and after the addition is complete, the mixture is reacted. After the reaction is complete, the mixture is filtered, washed, purified and dried to obtain ferrocene chalcone; Among them, the mass ratio of acetylferrocene, ethanol aqueous solution, sodium hydroxide aqueous solution and benzaldehyde is 13.5-15:480-530:200-220:18-20, the ethanol aqueous solution is 95wt% ethanol aqueous solution, and the sodium hydroxide aqueous solution is 9wt% sodium hydroxide aqueous solution; the dropping conditions are: dropping at 20°C for 20-30min; the reaction conditions are: reacting at 20-30°C for 1-1.5h.

4. The method for preparing an antioxidant according to claim 1, It is characterized in that In the step (2), the mass ratio of the modified titanium dioxide / aluminum phosphate molecular sieve composite material, sodium ethoxide, ethanol, and ferrocene chalcone is 60-70:2.5-3:260-300:3-3.5; the reaction conditions are: reacting in a nitrogen atmosphere at a temperature of 70-80°C for 6-8h.

5. The method for preparing an antioxidant according to claim 1, It is characterized in that In the step (3), the mass ratio of modified mesoporous nano-silica, toluene, triethylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride is 8-10:450-500:1.8-2:0.8-1; the dripping conditions of the 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride / toluene mixed solution are: dripping at a temperature of 0-5°C for 20-30 minutes, and the reaction conditions are: reacting at a temperature of 0-5°C for 6-8 hours in a nitrogen atmosphere.

6. An antioxidant prepared by the method for preparing an antioxidant as claimed in any one of claims 1 to 5.

7. A method for preparing a thin film, It is characterized in that The method is prepared by using the antioxidant as claimed in claim 6, comprising the following steps: The antioxidant is melt-blended with linear low-density polyethylene, extruded, and granulated to obtain an antioxidant masterbatch; Low-density polyethylene, linear low-density polyethylene, metallocene linear low-density polyethylene, maleic anhydride grafted polyolefin elastomer, and antioxidant masterbatch are melt-blended, extruded, blow-molded, trimmed, and rolled to obtain a film; Wherein, in the preparation process of the antioxidant masterbatch: the mass ratio of the antioxidant to the linear low-density polyethylene is 15-20:60-80; the melt blending conditions are: melt blending at a temperature of 140-150°C; the extrusion conditions are: extrusion at a speed of 20-30r / min and a temperature of 155-165°C; In the preparation process of the film, the mass ratio of low-density polyethylene, linear low-density polyethylene, metallocene linear low-density polyethylene, maleic anhydride grafted polyolefin elastomer and antioxidant masterbatch is 90-100:500-550:250-300:60-70:350-450; the melt blending conditions are: melt blending at a temperature of 140-150°C; the extrusion conditions are: extrusion through a twin-screw extruder at a screw speed of 30-40r / min, a zone one temperature of 108-112°C, a zone two temperature of 148-152°C, a zone three temperature of 158-162°C and a die head temperature of 148-152°C; the blow molding conditions are: blow molding through a blow molding film unit at a temperature of 170-180°C.