A kind of polyurethane adhesive capable of resisting yellowing and its application

By introducing yellowing-resistant stabilizer and modified fluoroelastomer into polyurethane adhesives, the performance problems of polyurethane adhesives under sunlight and rainwater erosion are solved, and the UV resistance and water resistance are improved to ensure that they are outdoors Stability and effects in the environment.

CN118308060BActive Publication Date: 2024-11-15GUANGZHOU AOYUESHENG SPORTS IND CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410311581.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2024-11-15
Estimated Expiration
2044-03-19

AI Technical Summary

Technical Problem

Polyurethane adhesives are prone to yellowing under long-term exposure to sunlight, affecting their aesthetics, and their adhesion is greatly reduced under rainwater erosion, resulting in poor performance in outdoor environments.

Method used

Polycarbonate derivatives containing ultraviolet absorbers in the structure are used as yellowing stabilizers, and graft them at the end of the polycarbonate molecular chain through click-through reaction, combining fluorine elements and tert-butyl groups in modified fluorine rubber Structure, forming polyurethane adhesive with excellent UV resistance and waterproof properties.

Benefits of technology

It significantly enhances the UV yellowing resistance and heat resistance of polyurethane adhesives, forms a strong hydrophobic barrier layer to prevent rainwater from infiltration, thereby maintaining high adhesion and waterproofing effect during long-term outdoor use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118308060B_ABST
    Figure CN118308060B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, and discloses a polyurethane adhesive capable of resisting yellowing and an application thereof. The polyurethane adhesive is based on a polyol as a soft segment and a diisocyanate as a hard segment. By adding a yellowing-resistant stabilizer and modified fluororubber and participating in the synthesis process of the polyurethane adhesive, the prepared polyurethane adhesive structure can contain an ultraviolet absorber capable of absorbing ultraviolet energy and a modified fluororubber segment with extremely low surface energy in a chemical bond manner. The ultraviolet absorption effect of the ultraviolet absorber can be utilized to enhance the anti-ultraviolet yellowing performance of the polyurethane adhesive, and the polycarbonate structure can be utilized to enhance the heat resistance of the polyurethane adhesive. The presence of the modified fluororubber segment can promote the formation of a strongly hydrophobic barrier layer on the surface of the polyurethane adhesive, effectively preventing rainwater from penetrating, and improving the water resistance of the adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, and in particular to a polyurethane adhesive capable of resisting yellowing and application thereof. Background Art

[0002] With the increasing popularity of national sports, the construction of outdoor sports venues is also increasing. In order to improve the safety and comfort of sports venues, a large number of sports venues use the method of laying mats to achieve the above effect. Among the many mat materials, EPDM rubber mats have excellent shock absorption and elasticity, and meet environmental protection standards, so they are often used as mats for outdoor sports venues. Generally speaking, in the production process of EPDM rubber mats, adhesives are needed to bond rubber particles. Since polyurethane adhesives have strong bonding strength, good cold resistance and excellent chemical resistance, they can be used as adhesives for rubber mats. Since outdoor sports venues are exposed to the environment for a long time, polyurethane adhesives are required to maintain good performance in harsh environments such as sun and rain, otherwise it will have a negative impact on the effect of rubber mats. However, studies have found that the anti-ultraviolet effect of polyurethane adhesives is poor. Under long-term sunlight exposure, it will not only turn yellow, affecting the appearance, but also cause the adhesive strength of the adhesive to decrease. In addition, the long-term erosion of polyurethane adhesives by rain will also cause a significant decrease in bonding strength. Therefore, it is necessary to improve polyurethane adhesives.

[0003] Invention patent publication number CN102732204B discloses a yellowing-resistant polyurethane composite adhesive. By adding an anti-ultraviolet light stabilizer, the prepared polyurethane composite adhesive has excellent yellowing resistance. However, the anti-ultraviolet light stabilizers currently used are mostly small molecule types. As the use time increases, they will gradually volatilize and migrate, and are not durable. Therefore, there are still defects in practical applications.

[0004] Based on this, the present invention provides a polyurethane adhesive, which has good anti-yellowing, waterproof and other effects, can maintain high performance for a long time outdoors, and can therefore be directly applied to the production of EPDM rubber floor mats. Summary of the invention

[0005] The purpose of the present invention is to provide a polyurethane adhesive that is resistant to yellowing and its application, so as to solve the problem that the polyurethane adhesive has poor anti-ultraviolet yellowing performance and poor waterproof performance.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A polyurethane adhesive capable of resisting yellowing, comprising the following components by weight: 50-55 parts of polyol, 1-2 parts of anti-yellowing stabilizer, 35-45 parts of diisocyanate, 0.1-0.5 parts of catalyst, 2-4.5 parts of modified fluororubber, 1-2 parts of defoamer, and 5-15 parts of chain extender;

[0008] The anti-yellowing stabilizer is a polycarbonate derivative containing an ultraviolet absorber in its structure.

[0009] Furthermore, the polyol is a polyether diol or polytetramethylene ether diol; the diisocyanate is any one or more of hexamethylene diisocyanate, isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate or cyclohexane dimethylene diisocyanate; the catalyst is any one of stannous octoate, dibutyltin dilaurate or dibutyltin diacetate; the defoamer is polyoxypropylene glycerol ether; and the chain extender is any one or two of ethylene glycol, 1,3-propylene glycol or 1,4-butanediol.

[0010] Furthermore, the anti-yellowing stabilizer is prepared by the following method:

[0011] Step A, polycarbonate diol and tetrahydrofuran are mixed, and after fully dissolved, nitrogen is introduced for protection, and then L-cysteine ​​is added, mixed, and the composite catalyst is added again. After the addition is completed, stirring is started, and the material is discharged after being treated at room temperature for 6-12 hours to form material ①;

[0012] In the above technical solution, the diol structure at the end of the polycarbonate diol molecular chain can undergo esterification condensation with the active carboxyl substituent in the L-cysteine ​​structure under the action of a composite catalyst to form a cysteine-modified polycarbonate derivative connected by an ester bond, namely material ①;

[0013] Step B, material ① and chloroform are mixed, mechanically stirred to form a uniform solution, nitrogen is introduced to deoxygenate, and then a UV absorber and benzoin dimethyl ether are added to the solution. After the addition is completed, an ultraviolet lamp with a wavelength of 365nm is used to irradiate the reaction system. After 30-60min, the product is separated to form a yellowing-resistant stabilizer.

[0014] Under the conditions of photoinitiator benzoin dimethyl ether and ultraviolet light irradiation, the thiol substituent at the end of the material structure ① can undergo an efficient click reaction with the unsaturated olefinic substituent in the ultraviolet absorber structure, thereby grafting the ultraviolet absorber to the end of the polycarbonate structure to prepare a yellowing-resistant stabilizer.

[0015] Furthermore, in step A, the number average molecular weight of the polycarbonate diol is 2000.

[0016] Furthermore, in step A, the composite catalyst is a composite mixture of dicyclohexylcarbodiimide and dimethylaminopyridine, and the mass ratio of the two is 1:0.3-0.4.

[0017] Furthermore, in step B, the ultraviolet absorber is 2-acrylate 2-(4-benzoyl-3-hydroxyphenoxy)ethyl ester or 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate.

[0018] Furthermore, the modified fluororubber is prepared by the following method:

[0019] Add carboxyl-terminated liquid fluororubber and 1,4-dioxane solvent to a reactor filled with nitrogen, and start stirring. After mixing evenly, add tert-butyldimethylsilyl (R)-(–)-glycidyl ether to the reactor, increase the temperature to maintain the reactor temperature at 70-80°C, and then add tetrabutylammonium bromide to the reactor. After adding, keep the temperature constant for 4-6 hours, stop heating, remove nitrogen, cool and discharge, and the modified fluororubber can be obtained.

[0020] In the above technical scheme, tetrabutylammonium bromide is used as a catalyst to catalyze the ring-opening esterification of the unsaturated olefin group in the terminal carboxyl liquid fluororubber structure and the epoxy group in the tert-butyldimethylsilyl (R)-(–)-glycidyl ether structure, thereby introducing active hydroxyl groups and hydrophobic tert-butyl structures into the fluororubber molecular chain to obtain modified fluororubber.

[0021] Furthermore, the number average molecular weight of the carboxyl-terminated liquid fluororubber is 3,000.

[0022] Furthermore, the polyurethane adhesive is prepared by the following method:

[0023] Step 1: vacuum dehydrate the polyol at 100-110° C., control the temperature to 70-80° C., mix with the anti-yellowing stabilizer under stirring, stir evenly, then add diisocyanate, stir for 30-60 minutes after addition, to form a prepolymer;

[0024] Step 2: Add the modified fluororubber and chain extender to the prepolymer. After the addition, slowly add the catalyst under continuous stirring. After continuous stirring for 2-4 hours, cool and discharge the material to form an adhesive precursor.

[0025] Step 3: Add a defoamer to the adhesive precursor and stir for 20-40 minutes to form a polyurethane adhesive.

[0026] In the above technical scheme, polyol is used as the soft segment and diisocyanate is used as the hard segment. Since the end of the yellowing-resistant stabilizer molecular chain contains unreacted amino substituents in the cysteine ​​structure, and the end of the modified fluororubber structure contains active hydroxyl substituents produced by the ring-opening reaction, these active substituents can interact with the isocyanate groups in the diisocyanate structure, and thus can participate in the synthesis reaction of polyurethane under the action of a catalyst, thereby simultaneously introducing a large number of yellowing-resistant stabilizer segments and modified fluororubber segments into the polyurethane molecular chain to obtain a polyurethane adhesive.

[0027] The invention discloses an application of a polyurethane adhesive capable of resisting yellowing, and the polyurethane adhesive is applied to the production field of EPDM rubber floor mats.

[0028] Beneficial effects of the present invention:

[0029] 1) The present invention introduces an anti-yellowing stabilizer into the molecular chain of the polyurethane adhesive. Since the anti-yellowing stabilizer structure contains an ultraviolet absorber, the ultraviolet absorber can be fixed in the polyurethane adhesive in the form of a chemical bond, thereby enhancing the anti-ultraviolet yellowing performance of the polyurethane adhesive. At the same time, the anti-yellowing stabilizer structure also contains a polycarbonate structure, which can enhance the heat resistance of the polyurethane adhesive and prevent the polyurethane adhesive from being decomposed at high temperature under outdoor high temperature conditions, thereby preventing the problem of losing viscosity.

[0030] 2) The present invention introduces a modified fluororubber segment into the polyurethane adhesive molecular chain. Since the modified fluororubber segment contains both fluorine elements and tert-butyl structures, it can exhibit an ultra-low surface energy, thereby prompting the formation of a strong hydrophobic barrier layer on the surface of the polyurethane adhesive, thereby effectively preventing rainwater from penetrating and causing the adhesive strength to decrease.

[0031] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0033] Figure 1 This is an infrared analysis test chart of the anti-yellowing stabilizer of the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The polyglycol used in the following examples and comparative examples is polyether glycol N210.

[0036] The anti-yellowing stabilizers used in the following examples and comparative examples were prepared by the following method:

[0037] Step A, 1.2 g of polycarbonate diol with a number average molecular weight of 2000 and tetrahydrofuran are mixed, and after fully dissolved, nitrogen is introduced for protection, and then 0.15 g of L-cysteine ​​is added and mixed, and 0.2 g of dicyclohexylcarbodiimide and 0.08 g of dimethylaminopyridine are added again. After the addition is completed, stirring is started, and the material is discharged after being treated at room temperature for 8 hours to form material ①;

[0038] Step B, 0.8g of material ① and chloroform are mixed, mechanically stirred to form a uniform solution, nitrogen is introduced to deoxygenate, and then 0.3g of 2-acrylic acid 2-(4-benzoyl-3-hydroxyphenoxy)ethyl ester and 0.1g of benzoin dimethyl ether are added to the solution. After the addition is completed, the reaction system is irradiated with an ultraviolet lamp with a wavelength of 365nm. After 40min, the product is separated to form a yellowing-resistant stabilizer.

[0039] Figure 1 This is the infrared analysis test chart of the anti-yellowing stabilizer, where 3368cm -1 The characteristic absorption peak at 3266 cm is the NH stretching vibration peak in the amine group. -1 The characteristic absorption peak at 1742 cm is the stretching vibration peak of the phenolic hydroxyl group in the UV absorber 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate. -1 The characteristic absorption peak at 1041 cm is the stretching vibration peak of the ester group C=O. -1 The characteristic absorption peak appearing at is the CS characteristic absorption peak produced by the click reaction.

[0040] The modified fluororubber used in the following examples and comparative examples was prepared by the following method:

[0041] Add 1.5 g of carboxyl-terminated liquid fluororubber with a number average molecular weight of 3000 and 1,4-dioxane solvent to a reactor filled with nitrogen, and start stirring. After mixing evenly, add 0.6 g of tert-butyldimethylsilyl (R)-(–)-glycidyl ether to the reactor, increase the temperature to maintain the reactor temperature at 75°C, and then add 0.2 g of tetrabutylammonium bromide to the reactor. After adding, keep the temperature constant for 4 hours, stop heating, remove nitrogen, cool and discharge, and the modified fluororubber can be obtained.

[0042] The modified fluororubber was titrated using the soap back titration method to calculate the ester group content in the modified fluororubber structure. The test results showed that the ester group content in the modified fluororubber structure was 0.305 mmol / g. Since the carboxyl-terminated liquid fluororubber structure does not contain ester groups, the ester groups are derived from the ring-opening esterification reaction between the carboxyl-terminated liquid fluororubber and tert-butyldimethylsilyl (R)-(–)-glycidyl ether.

[0043] Example 1

[0044] A polyurethane adhesive capable of resisting yellowing, comprising the following components by weight: 50 parts of polyether diol, 1 part of anti-yellowing stabilizer, 35 parts of isophorone diisocyanate, 0.1 part of dibutyltin dilaurate, 2 parts of modified fluororubber, 1 part of polyoxypropylene glycerol ether, and 5 parts of ethylene glycol;

[0045] The polyurethane adhesive is prepared by the following method:

[0046] Step 1: vacuum dehydrate the polyether diol at 100° C., control the temperature to 70° C., mix with a yellowing stabilizer under stirring, stir evenly, then add isophorone diisocyanate, stir for 30 minutes after the addition is complete, to form a prepolymer;

[0047] Step 2: Add modified fluororubber and ethylene glycol to the prepolymer. After the addition is completed, slowly add dibutyltin dilaurate under continuous stirring. After continuous stirring for 2 hours, cool and discharge the material to form an adhesive precursor.

[0048] Step 3: Add polyoxypropylene glycerol ether to the adhesive precursor and stir for 20 minutes to form a polyurethane adhesive.

[0049] Example 2

[0050] A polyurethane adhesive capable of resisting yellowing, comprising the following components by weight: 50 parts of polyether diol, 1.5 parts of anti-yellowing stabilizer, 40 parts of diphenylmethane diisocyanate, 0.4 parts of stannous octoate, 4 parts of modified fluororubber, 2 parts of polyoxypropylene glycerol ether, and 12 parts of 1,3-propylene glycol;

[0051] The polyurethane adhesive is prepared by the following method:

[0052] Step 1: vacuum dehydrate the polyether diol at 110° C., control the temperature to 75° C., mix with the anti-yellowing stabilizer under stirring, stir evenly, then add diphenylmethane diisocyanate, stir for 40 minutes after addition, to form a prepolymer;

[0053] Step 2: Add modified fluororubber and 1,3-propylene glycol to the prepolymer. After the addition is completed, slowly add stannous octoate under continuous stirring. After continuous stirring for 3 hours, cool and discharge the material to form an adhesive precursor.

[0054] Step 3: Add polyoxypropylene glycerol ether to the adhesive precursor and stir for 30 minutes to form a polyurethane adhesive.

[0055] Example 3

[0056] A polyurethane adhesive capable of resisting yellowing, comprising the following components by weight: 55 parts of polyether diol, 2 parts of anti-yellowing stabilizer, 45 parts of cyclohexane dimethylene diisocyanate, 0.5 parts of dibutyltin diacetate, 4.5 parts of modified fluororubber, 2 parts of polyoxypropylene glycerol ether, and 15 parts of 1,4-butanediol;

[0057] The polyurethane adhesive is prepared by the following method:

[0058] Step 1: After vacuum dehydration of the polyether diol at 110° C., the temperature is controlled to 80° C., and the mixture is mixed with a yellowing-resistant stabilizer under stirring. After stirring evenly, cyclohexane dimethylene diisocyanate is added, and after the addition is completed, the mixture is stirred for 60 minutes to form a prepolymer;

[0059] Step 2: Add modified fluororubber and 1,4-butanediol to the prepolymer. After the addition is completed, slowly add dibutyltin diacetate under continuous stirring. After continuous stirring for 4 hours, cool and discharge the material to form an adhesive precursor.

[0060] Step 3: Add polyoxypropylene glycerol ether to the adhesive precursor and stir for 40 minutes to form a polyurethane adhesive.

[0061] Comparative Example 1

[0062] A polyurethane adhesive capable of resisting yellowing, comprising the following components by weight: 50 parts of polyether diol, 40 parts of diphenylmethane diisocyanate, 0.4 parts of stannous octoate, 4 parts of modified fluororubber, 2 parts of polyoxypropylene glycerol ether, and 12 parts of 1,3-propylene glycol;

[0063] The polyurethane adhesive is prepared by the following method:

[0064] Step 1: vacuum dehydrate the polyether diol at 110° C., control the temperature to 75° C., add diphenylmethane diisocyanate under stirring, stir for 40 minutes after the addition, and form a prepolymer;

[0065] Step 2: Add modified fluororubber and 1,3-propylene glycol to the prepolymer. After the addition is completed, slowly add stannous octoate under continuous stirring. After continuous stirring for 3 hours, cool and discharge the material to form an adhesive precursor.

[0066] Step 3: Add polyoxypropylene glycerol ether to the adhesive precursor and stir for 30 minutes to form a polyurethane adhesive.

[0067] Comparative Example 2

[0068] A polyurethane adhesive capable of resisting yellowing, comprising the following components by weight: 50 parts of polyether diol, 1.5 parts of anti-yellowing stabilizer, 40 parts of diphenylmethane diisocyanate, 0.4 parts of stannous octoate, 2 parts of polyoxypropylene glycerol ether, and 12 parts of 1,3-propylene glycol;

[0069] The polyurethane adhesive is prepared by the following method:

[0070] Step 1: vacuum dehydrate the polyether diol at 110° C., control the temperature to 75° C., mix with the anti-yellowing stabilizer under stirring, stir evenly, then add diphenylmethane diisocyanate, stir for 40 minutes after addition, to form a prepolymer;

[0071] Step 2: Add 1,3-propylene glycol to the prepolymer, add stannous octoate slowly under continuous stirring, continue stirring for 3 hours, cool and discharge the material to form an adhesive precursor;

[0072] Step 3: Add polyoxypropylene glycerol ether to the adhesive precursor and stir for 30 minutes to form a polyurethane adhesive.

[0073] Comparative Example 3

[0074] A polyurethane adhesive capable of resisting yellowing, comprising the following components by weight: 50 parts of polyether diol, 1.5 parts of anti-yellowing stabilizer, 40 parts of diphenylmethane diisocyanate, 0.4 parts of stannous octoate, 4 parts of carboxyl-terminated liquid fluororubber, 2 parts of polyoxypropylene glycerol ether, and 12 parts of 1,3-propylene glycol;

[0075] The polyurethane adhesive is prepared by the following method:

[0076] Step 1: vacuum dehydrate the polyether diol at 110° C., control the temperature to 75° C., mix with the anti-yellowing stabilizer under stirring, stir evenly, then add diphenylmethane diisocyanate, stir for 40 minutes after addition, to form a prepolymer;

[0077] Step 2: Add carboxyl-terminated liquid fluororubber and 1,3-propylene glycol to the prepolymer. After the addition is completed, slowly add stannous octoate under continuous stirring. After continuous stirring for 3 hours, cool and discharge the material to form an adhesive precursor.

[0078] Step 3: Add polyoxypropylene glycerol ether to the adhesive precursor and stir for 30 minutes to form a polyurethane adhesive.

[0079] The polyurethane adhesives prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 were uniformly coated on a clean glass plate, and after being completely cured to form an adhesive film, the following tests were performed:

[0080] a. According to the standard GB / T 2409-1980, the film was placed in a xenon lamp aging instrument, and the film was aged for 800 hours, the yellow index of the film was tested, and the anti-ultraviolet yellowing performance of the film was evaluated;

[0081] b. Place the glass plate containing the adhesive film in an oven at 150°C for 24 hours, then take it out and observe the adhesive film phenomenon;

[0082] c. Use PZ-200SD contact angle tester to test the water contact angle of the film. The test results are recorded in the following table:

[0083] Yellow Index Film phenomenon Water contact angle / ° Example 1 5 No obvious phenomenon 153 Example 2 4 No obvious phenomenon 155 Example 3 5 No obvious phenomenon 152 Comparative Example 1 18 The film is curled and partially cracked. 150 Comparative Example 2 6 No obvious phenomenon 108 Comparative Example 3 6 No obvious phenomenon 133

[0084] Analysis of the test results shows that the polyurethane adhesive made by adding anti-yellowing stabilizer and modified fluororubber has a small yellowing index under long-term ultraviolet irradiation conditions, showing excellent anti-ultraviolet yellowing performance. It also has good high temperature stability and super hydrophobic properties, so it can effectively resist outdoor sunlight and rain environments.

[0085] Comparative Example 1 only uses modified fluororubber as an additive, so the prepared polyurethane adhesive does not contain a polycarbonate structure and a UV absorber, resulting in a significant decrease in its anti-ultraviolet yellowing performance and high temperature resistance.

[0086] Comparative Example 2 uses an anti-yellowing stabilizer as an additive, which results in the polyurethane adhesive being unable to produce a super-hydrophobic surface. Therefore, the hydrophobic effect is poor and it is difficult to resist the erosion of rainwater, resulting in a greatly increased risk of loss of adhesion.

[0087] Comparative Example 3 uses carboxyl-terminated liquid fluororubber instead of modified fluororubber. Although it can improve the hydrophobic effect of the polyurethane adhesive, it cannot achieve a super-hydrophobic effect and still has the problem of loss of adhesion due to rain erosion.

[0088] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0089] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A polyurethane adhesive that resists yellowing, characterized in that: The composition comprises the following components by weight: 50-55 parts of polyol, 1-2 parts of anti-yellowing stabilizer, 35-45 parts of diisocyanate, 0.1-0.5 parts of catalyst, 2-4.5 parts of modified fluororubber, 1-2 parts of defoamer, and 5-15 parts of chain extender; The anti-yellowing stabilizer is a polycarbonate derivative containing an ultraviolet absorber in its structure; The anti-yellowing stabilizer is prepared by the following method: Step A, polycarbonate diol and tetrahydrofuran are mixed, and after fully dissolved, nitrogen is introduced for protection, and then L-cysteine ​​is added, mixed, and the composite catalyst is added again. After the addition is completed, stirring is started, and the material is discharged after being treated at room temperature for 6-12 hours to form material ①; Step B, mixing material ① and chloroform, mechanically stirring to form a uniform solution, introducing nitrogen to deoxygenate, and then adding an ultraviolet absorber and benzoin dimethyl ether to the solution. After the addition is completed, the reaction system is irradiated with an ultraviolet lamp with a wavelength of 365nm, and the product is separated after 30-60min to form a yellowing-resistant stabilizer; The ultraviolet absorber is 2-(4-benzoyl-3-hydroxyphenoxy)ethyl 2-acrylate or 2-[3-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate; The modified fluororubber is prepared by the following method: Add carboxyl-terminated liquid fluororubber and 1,4-dioxane solvent to a reactor filled with nitrogen, and start stirring. After mixing evenly, add tert-butyldimethylsilyl (R)-(–)-glycidyl ether to the reactor, increase the temperature to maintain the reactor temperature at 70-80°C, and then add tetrabutylammonium bromide to the reactor. After adding, keep the temperature constant for 4-6 hours, stop heating, remove nitrogen, cool and discharge, and the modified fluororubber can be obtained.

2. The anti-yellowing polyurethane adhesive according to claim 1, characterized in that: The polyol is a polyether diol or a polytetramethylene ether diol; the diisocyanate is any one or more of hexamethylene diisocyanate, isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate or cyclohexane dimethylene diisocyanate; the catalyst is any one of stannous octoate, dibutyltin dilaurate or dibutyltin diacetate; the defoamer is polyoxypropylene glycerol ether; and the chain extender is any one or two of ethylene glycol, 1,3-propylene glycol or 1,4-butanediol.

3. The anti-yellowing polyurethane adhesive according to claim 1, characterized in that: In step A, the number average molecular weight of the polycarbonate diol is 2000.

4. The anti-yellowing polyurethane adhesive according to claim 1, characterized in that: In step A, the composite catalyst is a composite mixture of dicyclohexylcarbodiimide and dimethylaminopyridine, and the mass ratio of the two is 1:0.3-0.

4.

5. The anti-yellowing polyurethane adhesive according to claim 1, characterized in that: The number average molecular weight of the carboxyl-terminated liquid fluororubber is 3,000.

6. The anti-yellowing polyurethane adhesive according to claim 1, characterized in that: The polyurethane adhesive is prepared by the following method: Step 1: vacuum dehydrate the polyol at 100-110° C., control the temperature to 70-80° C., mix with the anti-yellowing stabilizer under stirring, stir evenly, then add diisocyanate, stir for 30-60 minutes after addition, to form a prepolymer; Step 2: Add the modified fluororubber and chain extender to the prepolymer. After the addition, slowly add the catalyst under continuous stirring. After continuous stirring for 2-4 hours, cool and discharge the material to form an adhesive precursor. Step 3: Add a defoamer to the adhesive precursor and stir for 20-40 minutes to form a polyurethane adhesive.

7. An application of the anti-yellowing polyurethane adhesive as claimed in claim 1, characterized in that: The polyurethane adhesive is applied in the field of manufacturing EPDM rubber floor mats.

Citation Information

Patent Citations

  • Anti-yellowing polyurethane composite adhesive

    CN102732204B

  • Method for preparing and curing hydroxyl-terminated liquid fluoropolymer

    CN103980405A

  • Preparation method of single-component silane-terminated liquid fluorine sealing rubber

    CN107325208A

  • Hot-melt adhesive and preparation method thereof, reflective stripe and solar panel

    CN107502233A

  • UV absorption type fluorinated siliconized acrylic emulsion and preparation method thereof

    CN111234090A