Wound dressing and preparation method thereof

By using light-cured polycaprolactone and polysulfide propylene-sodium alginate compartmentalized wound dressings, the problems of infection and scarring caused by traditional dressings during the healing process of deep burns and other wounds have been solved, achieving the goal of promoting cell growth, scavenging reactive oxygen species and The effect of preventing adhesion improves the efficiency and safety of wound healing.

CN118320166BActive Publication Date: 2024-10-29SICHUAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410437769.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-10-29
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

Traditional wound dressings can easily lead to infection, slow wound healing, and hypertrophic scar formation when treating deep second- and third-degree burns, knife wounds, and diabetic wounds. They are also difficult to prevent wound adhesion, affecting patients' health and quality of life.

Method used

A wound dressing composed of polycaprolactone, polysulfide propylene and modified sodium alginate containing light-curing groups is used to form spacers through light-curing, which promotes directional growth of cells, removes reactive oxygen species, prevents wound adhesion, and has good Exudate absorption and fluid exchange functions.

Benefits of technology

The dressing promotes wound healing, reduces scar formation, prevents wound adhesion, provides anti-inflammatory effects, and improves wound healing efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118320166B_ABST
    Figure CN118320166B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of wound dressings, and in particular, to wound dressings and preparation methods thereof. The functional raw materials forming the wound dressings are composed of polycaprolactone containing photocurable groups, polypropylene sulfide and modified sodium alginate, and the side of the wound dressing in contact with the wound surface is provided with a photocurable polycaprolactone area and a photocurable polypropylene sulfide-sodium alginate area, and the two are arranged at intervals, wherein the photocurable polycaprolactone area is formed by photocuring of polycaprolactone containing photocurable groups, and the photocurable polypropylene sulfide-sodium alginate area is formed by photocuring of a mixture of polypropylene sulfide and modified sodium alginate. The wound dressing has good biological safety, can efficiently absorb exudate around the wound, provide a moist environment for the wound surface, promote wound healing, and can activate active oxygen, and then have a good anti-inflammatory effect, and at the same time, can promote the directional growth, proliferation and migration of cells, prevent wound adhesion, reduce scar formation, and facilitate wound healing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wound dressings, and in particular to a wound dressing and a preparation method thereof. Background Art

[0002] Wounds are damage to normal skin (tissue) caused by external factors such as surgery, external force, heat, electric current, chemicals, low temperature, and internal factors such as local blood supply disorders, often accompanied by the destruction of skin integrity. For example, burns are divided into I-III degrees according to the depth of the wound, among which II degree burns are divided into superficial II degree and deep II degree. Usually, I degree burns only involve the superficial layer of the skin, no blisters will appear, and most can be cured; superficial II degree burns involve the epidermal germinal layer and the dermal papillary layer, most of which will cause blisters, but will not leave scars after healing; deep II degree burns are more deeply damaged, involving below the dermal papillary layer, and are often accompanied by scar formation after healing; while III degree burns involve the entire layer of skin, and even damage the muscles and bones under the skin. The above-mentioned deep II and III degree burn wounds are usually accompanied by a large amount of exudate, and due to severe tissue damage and excessive inflammatory response, it is easy to cause wound infection, slow wound healing, and thickened scar formation, which seriously affects the patient's physical and mental health and quality of life. Similarly, wounds with exudate and transitional inflammation similar to deep second-degree and third-degree burn wounds include knife wounds, wounds of diabetic patients, and scalds. Based on the severity of various wounds and the urgency of treatment, the research on wound dressings has gradually become a hot topic. Traditional medical dressings include sterile gauze, medical absorbent cotton, etc. This type of dressing can isolate the external environment, stop bleeding, inhibit bacteria, and absorb exudate. However, this type of dressing is easy to adhere to the tissue, and the replacement of auxiliary materials often leads to secondary injury to the wound, and even complications such as infection, and there is no obvious improvement on the formation of hypertrophic scars.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The purpose of the present invention is to provide a wound dressing and a preparation method thereof. The wound dressing has good biological safety, can efficiently absorb exudate around the wound, provide a moist environment for the wound, promote wound healing, and can remove active oxygen, thereby having a good anti-inflammatory effect, and at the same time, can promote the directional growth, proliferation and migration of cells, prevent wound adhesion, reduce scar formation, and facilitate wound healing.

[0005] The present invention is achieved in that:

[0006] In a first aspect, the present invention provides a wound dressing, wherein the functional raw materials forming the wound dressing are composed of polycaprolactone containing a photocurable group (abbreviated as PCLMA), polypropylene sulfide (abbreviated as PPS) and modified sodium alginate (abbreviated as AlgMA),

[0007] The side of the wound dressing in contact with the wound surface is provided with a light-cured polycaprolactone area and a light-cured polypropylene sulfide-sodium alginate area, and the light-cured polycaprolactone area and the light-cured polypropylene sulfide-sodium alginate area are arranged at intervals.

[0008] The photocurable polycaprolactone region is formed by photocuring polycaprolactone containing photocurable groups, and the photocurable polypropylene sulfide-sodium alginate region is formed by photocuring a mixture of polypropylene sulfide and modified sodium alginate.

[0009] In an optional embodiment, a microstructure is provided on the photocurable polycaprolactone area.

[0010] Preferably, the microstructure is composed of parallel arranged peaks and valleys alternately;

[0011] Preferably, the photocurable polycaprolactone region is formed by 3D printing polycaprolactone containing photocurable groups and then photocuring;

[0012] Preferably, the side chain of the polycaprolactone containing a photocurable group contains a methacrylate group or an acrylate group.

[0013] In an optional embodiment, the side chain of the polypropylene sulfide contains a hydroxyl group;

[0014] The side chain of the modified sodium alginate contains a methacrylate group or an acrylate group;

[0015] Preferably, the mass ratio of the polypropylene sulfide to the modified sodium alginate is 1:3-1:10.

[0016] In an optional embodiment, the side of the wound dressing opposite to the wound surface contains only the photocurable polypropylene sulfide-sodium alginate area.

[0017] In a second aspect, the present invention provides a method for preparing the wound dressing according to the aforementioned embodiment, comprising:

[0018] photocuring the polycaprolactone containing the photocurable group to form a photocurable polycaprolactone region;

[0019] The mixture of the light-cured polypropylene sulfide and the modified sodium alginate forms a light-cured polypropylene sulfide-sodium alginate region;

[0020] The photocurable polycaprolactone area and the photocurable polypropylene sulfide-sodium alginate area are arranged at intervals.

[0021] In an optional embodiment, the preparation steps of polycaprolactone containing photocurable groups are as follows:

[0022] PCL triol, amine substances and solvents are mixed and cooled to 0°C, and then methacrylic anhydride is added and the temperature is raised to 20-30°C, and the reaction is carried out for 1-2 hours to form a PCLMA solution;

[0023] Next, the PCLMA solution is post-treated to obtain a PCLMA intermediate;

[0024] mixing the PCLMA intermediate with a light absorber to form a PCL prepolymer;

[0025] The PCL prepolymer and the photoinitiator are mixed and stirred, and then bubbles are removed by ultrasound;

[0026] Preferably, the post-treatment comprises: washing the PCLMA solution with hydrochloric acid, washing with deionized water, spin drying, washing with alcohol, precipitating and rotary evaporating;

[0027] Preferably, the precipitation temperature is -85°C to 75°C;

[0028] Preferably, the conditions for mixing the PCL prepolymer and the photoinitiator include: ultrasonic time of 5-10 minutes;

[0029] Preferably, the conditions for mixing the PCL prepolymer and the light absorber include: stirring for 1-2h at a temperature of 55-65°C;

[0030] Preferably, the amine substance includes triethylamine; the light absorber includes β-carotene, and the photoinitiator includes diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide and / or 2-hydroxy-2-methylpropiophenone;

[0031] Preferably, the mass / volume ratio of the PCL triol and the amine substance is 1:10, the mass ratio of the light absorber and the photoinitiator is (0.05%-0.075%):2%; and the molar ratio of the PCL triol and the amine substance is 1:1.

[0032] In an optional embodiment, before photocuring the polycaprolactone containing photocurable groups, 3D printing is performed using the polycaprolactone containing photocurable groups.

[0033] In an optional embodiment, the preparation steps of the polypropylene sulfide are as follows:

[0034] The degassed, dried and washed 1,8-diazabicyclo[5.4.0]undec-7-ene is mixed with 1-butanethiol for reaction, and then mixed with freshly distilled and degassed propylene sulfide for reaction, and then a reaction quencher is added to quench the reaction; and then post-treatment is performed;

[0035] Preferably, the molar ratio of the 1,8-diazabicyclo[5.4.0]undec-7-ene, the 1-butanethiol, the propylene sulfide and the reaction quencher is 3-4:1-2:55-65:2-3;

[0036] Preferably, the degassing conditions include: 0°C, 25-35min;

[0037] Preferably, the conditions for mixing with the 1-butanethiol include: 0°C, 25-35min;

[0038] The conditions for mixing with the propylene sulfide include: 0°C, 1-3h;

[0039] The conditions for quenching the reaction include: 20-30°C, 10-16h.

[0040] In an optional embodiment, the preparation steps of modified sodium alginate are as follows:

[0041] Sodium alginate is mixed with a buffer solution, a pH regulator and a carboxyl activation agent for reaction, and then a methacrylate compound is added for reaction, and stirred, for example, at 25 degrees for 24 hours to precipitate to obtain a precipitate; then, the precipitate is dissolved, dialyzed, filtered and freeze-dried;

[0042] Preferably, the carboxyl activation reagent includes NHS and EDC·HCl;

[0043] The methacrylate compound is selected from 2-aminoethyl methacrylate;

[0044] Preferably, the usage ratio of the sodium alginate, the buffer solution, the EDC·HCl, the NHS and the 2-aminoethyl methacrylate is (2-2.5 g): 200 mL: (5-6 g): (1-1.5 g): (1-2 g);

[0045] Preferably, the concentration ratio of the buffer solution and the pH adjuster is (0.1-0.2 mol / L): (0.1-0.2 mol / L);

[0046] Preferably, the carboxyl activation reagent is added and stirred for 3-6 hours, and the conditions for adding the methacrylate compound include: the temperature is 20-30° C., and the stirring time is 20-28 hours;

[0047] The dialysis conditions include: molecular weight cut-off of 3500, time of 48-72 hours; filtration pore of 0.2-0.25 μm, and freeze-drying time of 24-72 hours.

[0048] In an optional embodiment, the method comprises: mixing the polypropylene sulfide and the modified sodium alginate for 4-8 hours, and then dropping the mixture so that the mixture is distributed between two adjacent photocurable polycaprolactone regions and then photocuring.

[0049] The present invention has the following beneficial effects: the wound dressing provided by the embodiment of the present invention selects polycaprolactone, polypropylene sulfide and modified sodium alginate containing photocurable groups as its functional components, and the formed photocurable polycaprolactone area and the photocurable polypropylene sulfide-sodium alginate area are arranged at intervals, so that the wound dressing promotes directional growth and apical growth of cells, has good anti-wound adhesion effect, can react with active oxygen, has excellent antioxidant effect, and at the same time, has good absorption exudation and liquid exchange functions. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0051] Figure 1 A structural diagram of the wound dressing provided in Example 1 of the present invention;

[0052] Figure 2 The H NMR spectrum of PCLMA provided in Characterization 1 of the present invention;

[0053] Figure 3 The microstructure diagram of PCLMA provided for Characterization 2 of the present invention;

[0054] Figure 4 The H NMR spectrum of PPS provided by Characterization 3 of the present invention;

[0055] Figure 5 The PPS and H provided by the present invention are characterized in 3 2 O 2 H NMR spectra before and after treatment;

[0056] Figure 6 The nuclear magnetic hydrogen spectrum of the modified sodium alginate provided by Characterization 4 of the present invention;

[0057] Figure 7 The pictures of the mixture of PPS and modified sodium alginate provided in Characterization 4 of the present invention before and after light curing;

[0058] Figure 8 The mixture of PPS and modified sodium alginate provided by the present invention is characterized in Figure 4 and the H after light curing 2 O2 Scanning electron microscope (SEM) images before and after treatment;

[0059] Fig. 9 The result diagram provided for the detection example 1 of the present invention;

[0060] Figure 10-11 The result diagram provided for the detection example 2 of the present invention;

[0061] Fig.12 The result diagram provided for the detection example 3 of the present invention;

[0062] Figure 13-14 The result diagram provided for detection example 4 of the present invention;

[0063] Fig.15 This is a result diagram provided for detection example 5 of the present invention. DETAILED DESCRIPTION

[0064] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0065] The embodiment of the present invention provides a wound dressing, which can be used for various wounds such as burn wounds, knife wounds and diabetic wounds, and the shape of the wound dressing can be a cylinder, a cuboid, a cube or other irregular geometric shapes. In this embodiment, the wound dressing is designed as a cuboid.

[0066] The functional raw materials forming the wound dressing are composed of polycaprolactone containing photocurable groups, polypropylene sulfide and modified sodium alginate, wherein the side of the wound dressing in contact with the wound includes a central area and a peripheral area, the peripheral area is wrapped outside the central area, the central area is composed of a photocurable polycaprolactone area and a photocurable polypropylene sulfide-sodium alginate area, the photocurable polypropylene sulfide-sodium alginate area is formed by photocuring a mixture of polypropylene sulfide and modified sodium alginate; the peripheral area is only a photocurable polycaprolactone area. The central area is in full contact with the wound surface, and the peripheral area can be in contact with the wound surface or with normal tissue, preferably with normal tissue.

[0067] The photocurable polycaprolactone region is formed by 3D printing polycaprolactone containing photocurable groups and then photocuring; wherein the side chain of the polycaprolactone containing photocurable groups contains methacrylate groups or acrylate groups. The photocurable polypropylene sulfide-sodium alginate region is formed by photocuring a mixture of polypropylene sulfide and modified sodium alginate. The side chain of polypropylene sulfide contains hydroxyl groups; the side chain of the modified sodium alginate contains methacrylate groups or acrylate groups; the mass ratio of the polypropylene sulfide to the modified sodium alginate is 1:3-1:10.

[0068] The embodiment of the present invention removes active oxygen through the ROS responsiveness of polypropylene sulfide (PPS); and acts as the sweat gland function of the skin through the good hydrophilicity and degradability of AlgMA, thereby performing fluid exchange and promoting inflammatory exudation. At the same time, light-cured polycaprolactone promotes directional cell growth, promotes wound healing and exerts anti-adhesion effects.

[0069] Furthermore, a microstructure is provided on the photocurable polycaprolactone area in the central region, and the microstructure is composed of parallel peaks and valleys arranged alternately; that is, the microstructure is in a "wave" shape, which is more conducive to the directional growth of cells, promotes wound healing and plays an anti-adhesion role. The microstructure is formed by 3D printing.

[0070] Furthermore, the side of the wound dressing opposite to the wound surface only contains a photocured polypropylene sulfide-sodium alginate area, and the photocured polypropylene sulfide-sodium alginate area in this part is connected to the photocured polypropylene sulfide-sodium alginate area in the central area, which can then absorb more exudate and has a better anti-inflammatory effect.

[0071] In a second aspect, an embodiment of the present invention provides a method for preparing the above-mentioned wound dressing, comprising:

[0072] S1, preparing polycaprolactone containing photocurable groups;

[0073] PCL triol and amine substances (such as but not limited to triethylamine) are dissolved in a solvent, the solvent is selected from C1-C3 halogenated alkanes, preferably C1-C3 monochloroalkanes, and most preferably dichloromethane. The mixed solution is then cooled to 0°C, purged with nitrogen, and then methacrylic anhydride is added dropwise; the mixed solution is then gradually heated to room temperature (20-30°C), and reacted for 1-2 hours to form a PCLMA solution.

[0074] Next, the PCLMA solution is post-treated to obtain a PCLMA intermediate, the post-treatment comprising: washing the PCLMA solution 3 times with 1M hydrochloric acid, then washing it 2 times with deionized water, and then removing the solvent in the PCLMA solution by rotary evaporation; then washing it with an alcohol solvent (such as but not limited to methanol), and precipitating it (repeated 3-4 times), and then further removing the solvent by rotary evaporation. The precipitation temperature is -85°C--75°C.

[0075] The PCLMA intermediate is mixed with a light absorber to form a PCL prepolymer, wherein the light absorber includes but is not limited to β-carotene, and the stirring time is 1-2 hours.

[0076] The PCLMA prepolymer is mixed with a photoinitiator, and then the bubbles are removed by ultrasound; wherein the photoinitiator includes diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide and / or 2-hydroxy-2-methylpropiophenone; and the mass ratio of the two is 0.8-1.2:1.

[0077] Among them, the mass / volume ratio of PCL triol and the amine substance is 1:10, the mass ratio of the light absorber and the photoinitiator is (0.05%-0.075%):2%; the molar ratio of the PCL triol and the amine substance is 1:1.

[0078] Then, the polycaprolactone containing the photocurable group is 3D printed, and a central area and a peripheral area are formed during 3D printing, wherein the peripheral area is wrapped outside the central area, and a microstructure is printed on the central area. Then, the 3D printed material is photocured.

[0079] Specifically,

[0080] (1) According to the pre-designed parameters and structure, an ultra-fine resin mold (positive mold) is printed using an ultra-fine 3D printer.

[0081] (2) Silicone rubber with a certain fluidity (purchased by prior art) is injected into the resin positive mold, and vacuumed for 30 minutes to 1 hour at room temperature to remove bubbles. Then, it is placed in a vacuum drying oven at 60-80°C for curing and shaping, and the mold is turned over to form a silicone rubber negative mold.

[0082] (3) PCLMA with a certain fluidity (i.e., the polycaprolactone containing photocurable groups formed above) is injected into the silicone rubber female mold, and vacuumed at 50-80°C for 30 min-1 h to remove bubbles, then cooled for 1-5 min, irradiated under a blue light for 30 s-1 min, and after preliminary curing, the mold is flipped to form a PCLMA with a directional microstructure.

[0083] (4) The preliminarily solidified PCLMA was placed in a mixed solvent of isopropanol and methanol (volume ratio 1:1-1:3), and ultrasonically treated at 30-40 kHz for 3-5 min, and cleaned three times to complete the preliminary cleaning of the PCLMA.

[0084] (5) The PCLMA that has been initially cleaned is cured by blue light for 30 min-1 h to achieve complete curing.

[0085] (6) The completely solidified PCLMA was then placed in 75% ethanol for further cleaning, and ultrasonically treated at 30-40 kHz for 3-5 min, for three times.

[0086] (7) Soak the completely cleaned PCLMA in PBS for 30 min-1 h to remove the organic solvent.

[0087] (8) Vacuum dry and set aside.

[0088] S2, forming polypropylene sulfide;

[0089] 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) is degassed in anhydrous tetrahydrofuran, dried in a flask and flushed with an inert gas such as nitrogen.

[0090] A degassed solution of 1-butanethiol dissolved in anhydrous tetrahydrofuran is gradually added dropwise to the mixture in the above flask for mixed reaction. Freshly distilled and degassed propylene sulfide is added to the above reaction system to obtain a reaction mixture, and then a reaction quencher is added and stirred overnight to quench the reaction; the next day, the above polymer solution is filtered, washed with cold alcohol solvent, centrifuged, precipitated and dried to finally obtain a colorless viscous polymer PPS. 60 -OH.

[0091] Wherein, the reaction quencher is selected from 2-iodoethanol; the molar ratio of the above-mentioned 1,8-diazabicyclo[5.4.0]undec-7-ene, the 1-butanethiol, the propylene sulfide and the reaction quencher is 3-4:1-2:55-65:2-3.

[0092] The above-mentioned degassing conditions include: 0°C, 25-35min; the conditions for mixing with the 1-butanethiol include: 0°C, 25-35min; the conditions for mixing with the propylene sulfide include: 0°C, 1-3h; the conditions for quenching the reaction include: 20-30°C, 10-16h.

[0093] S3, forming modified sodium alginate;

[0094] Sodium alginate is dissolved in a buffer solution (including but not limited to a phosphate buffer solution), and a pH regulator (including but not limited to hydrochloric acid) is added to adjust the pH of the reaction, and then a carboxyl activation reagent (such as but not limited to NHS and EDC·HCl) is added to stir the reaction, and then a methacrylate compound (such as but not limited to 2-aminoethyl methacrylate (AEMA)) or an acrylate compound is added to stir the reaction; after the reaction is completed, an excess solvent (such as but not limited to acetone) is used for precipitation, and a precipitate is obtained by filtering, and the precipitate is dissolved in deionized water solvent, and then dialyzed, filtered and freeze-dried.

[0095] The dosage ratio of sodium alginate, the buffer solution, the EDC·HCl, the NHS and the 2-aminoethyl methacrylate is (2-2.5 g): 200 mL: (5-6 g): (1-1.5 g): (1-2 g); the concentration ratio of the buffer solution and the pH regulator is (0.1-0.2 mol / L): (0.1-0.2 mol / L).

[0096] It should be noted that, although the above amounts recorded in the embodiments of the present invention are g, ml and mol / L, it can be understood that the above amounts represent the ratios of the various substances and can be replaced by other mass units, volume units or concentration units in equal amounts.

[0097] Furthermore, after adding the carboxyl activation reagent, the mixture is stirred for 3-6 hours. The conditions for adding the methacrylate compound include: temperature of 20-30°C and stirring time of 20-28 hours; dialysis conditions include: molecular weight cutoff of 3500 and time of 48-72 hours; filtration pore size of 0.2-0.25 μm and freeze-drying time of 24-72 hours.

[0098] It should be noted that the above S1-S3 do not limit the preparation order, and they can be carried out simultaneously, or S3 can be carried out first, then S1 and S2, or S2 can be carried out first, then S3 and S1.

[0099] S4, forming a dressing;

[0100] Then, the polypropylene sulfide formed by S2 and S3 and the modified sodium alginate are mixed and stirred for 4-8 hours to form a uniform turbid liquid. The mass ratio of polypropylene sulfide to the modified sodium alginate is 1:3-1:10.

[0101] Then, the mixed solution is added dropwise to the side of the photocured polycaprolactone without microstructures in S1, and the mixed solution flows to between two adjacent photocured polycaprolactone areas in the central area, followed by photocuring.

[0102] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0103] Example 1

[0104] An embodiment of the present invention provides a method for preparing a wound dressing, comprising:

[0105] S1. Preparation of PCLMA:

[0106] (1) Dissolve 1 mol PCL triol and 6 mol triethylamine in 50 mL dichloromethane;

[0107] (2) The solution obtained in the above (1) was cooled to 0°C, purged with nitrogen, and then 6 mol of methacrylic anhydride was added dropwise;

[0108] (3) gradually heating the reactant obtained in (2) to room temperature (25° C.) and continuing the reaction for 24 hours;

[0109] (4) The PCLMA solution obtained in (3) was washed three times with 1M hydrochloric acid and then washed twice with deionized water;

[0110] (5) removing the solvent in the PCLMA obtained in (4) by rotary evaporation;

[0111] (6) washing the PCLMA intermediate obtained in (5) above in methanol and precipitating (3 times at -80°C), and then further removing the solvent by rotary evaporation;

[0112] (7) adding β-carotene to the above (6) and stirring for 1 hour to obtain a PCLMA prepolymer;

[0113] (8) The PCLMA prepolymer was dissolved in a mixture of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide and 2-hydroxy-2-methylpropiophenone, and stirred for 6 hours. The ratio of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide to 2-hydroxy-2-methylpropiophenone was 50 / 50, and then ultrasonicated to remove bubbles for 10 minutes.

[0114] The product obtained above is then 3D printed.

[0115] S2, forming polypropylene sulfide (abbreviated as PPS);

[0116] (1) At 0°C, 3 mmol of 1,8-diazabicyclo[5.4.0]undec-7-ene was dissolved in 15 mL of anhydrous tetrahydrofuran, degassed, dried in a flask and flushed with nitrogen.

[0117] (2) At 0°C, a degassed solution of 1.0 mmol, 0.070 mL, of 1-butanethiol dissolved in 10 mL of anhydrous tetrahydrofuran was dropwise added to the mixture in the flask in (1) above and reacted for 0.5 hours;

[0118] (3) adding 60 mmol, 4.68 mL of freshly distilled and degassed propylene sulfide monomer to the reaction mixture obtained in (2) above at 0°C and reacting for 2 hours;

[0119] (4) At 20° C., 2 mmol, 0.37 g 2-iodoethanol was added to quench the reaction mixture in (3) above, and stirred for 12 hours;

[0120] (5) The next day, the polymer solution obtained in (4) above was filtered, washed with methanol (3 times), centrifuged to collect the precipitate, and then vacuum dried to finally obtain a colorless viscous polymer PPS-OH.

[0121] S3, forming modified sodium alginate;

[0122] (1) 2.1 g of sodium alginate was dissolved in 200 mL of 0.2 mol / L phosphate buffer, and hydrochloric acid was added to the mixture to adjust the pH to 5-6;

[0123] (2) Add 5.75 g of EDC·HCl and 1.15 g of NHS to the mixed solution obtained in (1) above and stir for 4 hours;

[0124] (3) 1.66 g of 2-aminoethyl methacrylate was added to the solution obtained in (2) above, and the mixture was stirred for 24 hours;

[0125] (4) precipitating the mixed solution obtained in (3) above with excess acetone, and dissolving the filtered product in deionized water;

[0126] (5) The solution obtained in (4) above was dialyzed (molecular weight cut-off 3500, 72 h), filtered (filter membrane 0.22 μm), and freeze-dried for 48 h.

[0127] S4, forming a wound dressing;

[0128] The above-mentioned PPS and modified sodium alginate were mixed in a mass ratio of 1:3 and stirred at room temperature for 4 h to form a uniform turbid liquid (abbreviated as AlgMA / PPS);

[0129] The uniform turbid liquid is added to the side of the finished product without microstructure formed by S13D printing, so that it is evenly spread over the entire side of the PCLMA without structure, and light-cured to form a wound dressing. The structure of the wound dressing is shown in Figure 1 .

[0130] Representation 1

[0131] The PCLMA prepared in Example 1 was subjected to nuclear magnetic resonance detection, and the structure is shown in Figure 2 ,according to Figure 2 It can be seen that the characteristic peak of the methacrylate group appears (marked by the box), which confirms that PCLMA is successfully synthesized in the embodiment of the present invention.

[0132] Representation 2

[0133] The PCLMA product prepared by 3D printing in Example 1 was subjected to scanning electron microscopy. The structure is shown in Figure 3 ,according to Figure 3 It can be seen that the PCLMA microstructure (thickness of about 300um) is composed of parallel peaks and valleys, and the spacing between peaks is only about 30um. Through the enlarged SEM image, it can be seen that the PCLMA microstructure is composed of step-by-step printing, and the width of the highest point is only 2um. The peak-valley structure of the directional microstructure of PCLMA obtained by indirect 3D printing technology is the structural basis for promoting directional-apical growth of cells.

[0134] Representation 3

[0135] The PPS prepared in Example 1 was subjected to nuclear magnetic resonance detection (400 MHz, deuterated chloroform). The results are shown in Figure 4 ,according to Figure 4 It can be seen that PPS is synthesized in the embodiment of the present invention.

[0136] The PPS prepared in Example 1 was placed in 100 mM H 2 O 2 After 72 hours of treatment, HNMR was performed on PPS before and after oxidation. The peak shift and the generation of new signals in the HNMR spectrum confirmed that the sulfide (-S-) was oxidized to -SO( Figure 5 The results show that the hydrophobic group PPS has been oxidized to a hydrophilic sulfoxide group. Therefore, the HNMR results show that PPS has oxidation ability.

[0137] Representation 4

[0138] The modified sodium alginate prepared in Example 1 was subjected to HNMR. The results are shown in Figure 6 ,according to Figure 6 It can be seen that after the photocurable groups were grafted, new peaks appeared at 5.30 and 5.61 ppm, indicating that the desired modified sodium alginate was synthesized in the embodiment of the present invention.

[0139] Representation 5

[0140] The PPS and modified sodium alginate of Example 1 were mixed in different mass ratios, and then light-cured. The objects before and after light-curing were photographed. Figure 7 .

[0141] The photocured material was placed in 100 mM H 2 O 2 72 hours, and H 2 O 2 The samples before and after treatment were subjected to SEM examination, and the results are shown in Figure 8 .

[0142] according to Figure 7 It can be seen that the higher the PPS content, the closer the color is to milky white, forming a uniform and stable milky white turbid liquid. Figure 8 It can be seen that the freeze-dried composite hydrogel has a loose porous structure, the formation of which is conducive to fluid exchange at the burn site and the absorption of inflammatory exudate; and when Al gMA with PPS is added, small round protrusions can be observed, but it does not affect the structure of the material itself.

[0143] Test Example 1

[0144] The biosafety of the PCLMA finished product with microstructure prepared by 3D printing in Example 1 and whether it can promote directional cell growth were verified.

[0145] Fibroblasts were colonized on PCLMA with the best microstructure parameters, PCLMA with other microstructure parameters, and PCLMA without structure, and cell samples were collected for SEM observation after 1 day and 3 days. The results showed that ( Fig. 9 ), as time goes by, the cells of PCLMA with the best parameter microstructure proliferate well, and have a tendency of directional growth and apical growth. There are fewer cells in the microstructure valley, and most cells grow on the peak. In the other two groups, the cells are almost flat on the entire material surface. It can be seen that cells on the surface of PCLMA with other parameter microstructures and unstructured PCLMA do not show a better "upward, directional" growth trend, while the surface of PCLMA with the best parameter microstructure shows this growth phenomenon, resulting in a small cell contact area, which lays the foundation for the bionic epidermis to play an anti-adhesion function.

[0146] Test Example 2

[0147] The cell compatibility of AlgMA / PPS with different ratios was tested.

[0148] The PPS and modified sodium alginate of Example 1 were mixed in different mass ratios and then photocured, and fibroblasts were colonized on the surface of the photocured hydrogel. Fig.10 ,according to Fig.10 It can be seen that the cells grow well on the surface of the material and their morphology is extended.

[0149] Furthermore, cell proliferation and toxicity tests (CCK8) were performed on AlgMA / PPS at different ratios before and after oxidation. Fig.11 The results showed that on the 1st, 3rd, and 5th day, different groups had good cell proliferation status, and there was no difference between each group on the same day ( Fig.11 ), cell colonization and CCK8 results confirmed that different ratios of AlgMA / PPS had good biosafety before and after oxidation, which was beneficial to cell growth and wound healing.

[0150] Test Example 3

[0151] The PPS and modified sodium alginate of Example 1 were mixed in different mass ratios and then photocured. The photocured materials were placed in 100 mM H 2 O 2 The samples were treated for 72 hours and the hydrophilicity was tested before and after oxidation.

[0152] The test method is as follows: 7 groups of samples (different ratios of AlgMA / PPS before and after oxidation and a control group) were taken, and the contact angles of their smooth surfaces were measured.

[0153] Results Fig.12 ,according to Fig.12 It can be seen that the higher the PPS content, the more hydrophobic the AlgMA / PPS is; 2 O 2 After that, PPS underwent oxidation reaction, which increased the hydrophilicity of oxidized AlgMA / PPS. Among them, the contact angle of the 3:1 group of AlgMA / PPS oxidation was the smallest and the hydrophilicity was the best.

[0154] Test Example 4

[0155] The sample was prepared according to the method of detection example 3, and then the active oxygen was detected by the DCFH-DA fluorescent probe method. The results are shown in Fig.13 ,according to Fig.13 It can be seen that compared with other groups, 3:1 mass ratio AlgMA / PPS has the best ROS scavenging effect. Through the above biocompatibility test, contact angle test and reactive oxygen species test, the AlgMA / PPS composite hydrogel with the best ROS scavenging effect, namely the 3:1 mass ratio group, was screened out.

[0156] In order to further verify the ROS scavenging effect of AlgMA / PPS composite hydrogel, CCK8 detection was performed on AlgMA / PPS (3:1 mass ratio) before and after oxidation. The results are shown in Fig.14The results showed that compared with the control group and AlgMA group treated with hydrogen peroxide, the AlgMA / PPS group treated with hydrogen peroxide had no significant effect on cell activity, confirming that AlgMA / PPS has a good ability to remove H 2 O 2 effect.

[0157] Test Example 5 Animal Test

[0158] A deep second-degree burn model on the back of C57 mice was established to verify the in vivo function through intervention with biomimetic epidermal excipients. The groups were as follows: control group, unstructured PCLMA / AlgMA / PPS, structured PCLMA / AlgMA, and structured PCLMA / AlgMA / PPS, and HE staining was performed.

[0159] Results Fig.15 ,according to Fig.15 It can be seen that compared with the control group and the structured PCLMA / AlgMA group, the structured PCLMA / AlgMA / PPS group had less inflammatory infiltration, and the wound healed better 3 days after the burn, and part of the epidermis had been formed. Compared with the adhesion between the material and the wound in the unstructured PCLMA / AlgMA / PPS group, the structured PCLMA / AlgMA group and the structured PCLMA / AlgMA / PPS group did not show obvious adhesion between the material and the wound surface due to the directional microstructure of PCLMA. It can be seen that the structured PCLMA / AlgMA / PPS bionic epidermis has a good effect of promoting wound healing, preventing adhesion and anti-inflammatory.

[0160] In summary, it can be seen that the wound dressing provided by the embodiment of the present invention has the effects of promoting directional cell growth and anti-adhesion; it has a multi-site ROS scavenging effect, has an inflammatory responsive function, and is hydrophilic and adjustable, and has good water absorption, and finally forms an inflammatory responsive anti-adhesion wound dressing, which can be used as a temporary bionic epidermis during the healing period of burn wounds, thereby promoting the absorption of exudate, keeping the wound moist, preventing secondary damage caused by adhesion between the wound and the dressing, clearing inflammation and preventing infection, and finally achieving the purpose of promoting the healing of burn wounds.

[0161] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A wound dressing, characterized in that: The functional raw materials for forming the wound dressing are composed of polycaprolactone containing photocurable groups, polypropylene sulfide and modified sodium alginate. The side of the wound dressing in contact with the wound surface is provided with a light-cured polycaprolactone area and a light-cured polypropylene sulfide-sodium alginate area, and the light-cured polycaprolactone area and the light-cured polypropylene sulfide-sodium alginate area are arranged at intervals. The photocurable polycaprolactone region is formed by photocuring polycaprolactone containing photocurable groups, and the photocurable polypropylene sulfide-sodium alginate region is formed by photocuring a mixture of polypropylene sulfide and modified sodium alginate; A microstructure is arranged on the photocurable polycaprolactone area, and the microstructure is composed of parallel peaks and valleys arranged alternately.

2. The wound dressing according to claim 1, characterized in that: The photocurable polycaprolactone area is formed by 3D printing polycaprolactone containing photocurable groups and then photocuring it.

3. The wound dressing according to claim 2, characterized in that: The side chain of the photocurable group-containing polycaprolactone contains a methacrylate group or an acrylate group.

4. The wound dressing according to claim 1, characterized in that: The side chain of the polypropylene sulfide contains a hydroxyl group; The side chain of the modified sodium alginate contains a methacrylate group or an acrylate group.

5. The wound dressing according to claim 1, characterized in that: The mass ratio of the polypropylene sulfide to the modified sodium alginate is 1:3-1:

10.

6. The wound dressing according to claim 1, characterized in that: The side of the wound dressing opposite to the wound surface only contains the light-cured polypropylene sulfide-sodium alginate area.

7. A method for preparing the wound dressing according to claim 1, characterized in that: include: photocuring the polycaprolactone containing the photocurable group to form a photocurable polycaprolactone region; The mixture of the light-cured polypropylene sulfide and the modified sodium alginate forms a light-cured polypropylene sulfide-sodium alginate region; The photocurable polycaprolactone area and the photocurable polypropylene sulfide-sodium alginate area are arranged at intervals.

8. The preparation method according to claim 7, characterized in that: The preparation steps of polycaprolactone containing photocurable groups are as follows: PCL triol, amine substances and solvents are mixed and cooled to 0°C, and then methacrylic anhydride is added and the temperature is raised to 20-30°C, and the reaction is carried out for 1-2 hours to form a PCLMA solution; Next, the PCLMA solution is post-treated to obtain a PCLMA intermediate; mixing the PCLMA intermediate with a light absorber to form a PCL prepolymer; The PCL prepolymer and the photoinitiator are mixed and stirred, and then bubbles are removed by ultrasound.

9. The preparation method according to claim 8, characterized in that: Post-processing includes: The PCLMA solution is washed with hydrochloric acid, washed with deionized water, dried by rotation, washed with alcohol, precipitated and evaporated by rotation.

10. The preparation method according to claim 9, characterized in that: The precipitation temperature is -85℃--75℃.

11. The preparation method according to claim 8, characterized in that: The conditions for mixing the PCL prepolymer and the photoinitiator include: the ultrasonic time is 5-10 minutes.

12. The preparation method according to claim 8, characterized in that: The conditions for mixing the PCL prepolymer and the light absorber include: stirring for 1-2 hours at a temperature of 55-65°C.

13. The preparation method according to claim 8, characterized in that: The amine substance includes triethylamine; the light absorber includes beta-carotene; and the light initiator includes diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide and / or 2-hydroxy-2-methylpropiophenone.

14. The preparation method according to claim 8, characterized in that: The mass / volume ratio of the PCL triol and the amine substance is 1:10, the mass ratio of the light absorber and the photoinitiator is (0.05%-0.075%):2%; the molar ratio of the PCL triol and the amine substance is 1:

1.

15. The preparation method according to claim 7, characterized in that: Before photocuring the polycaprolactone containing photocurable groups, 3D printing is performed using the polycaprolactone containing photocurable groups.

16. The preparation method according to claim 7, characterized in that: The preparation steps of the polypropylene sulfide are as follows: The degassed, dried and washed 1,8-diazabicyclo[5.4.0]undec-7-ene is mixed with 1-butanethiol for reaction, and then mixed with freshly distilled and degassed propylene sulfide for reaction, and then a reaction quencher is added to quench the reaction; and then post-treatment is performed.

17. The preparation method according to claim 16, characterized in that: The molar ratio of the 1,8-diazabicyclo[5.4.0]undec-7-ene, the 1-butanethiol, the propylene sulfide and the reaction quencher is 3-4:1-2:55-65:2-3; Degassing conditions include: 0°C, 25-35min; The conditions for mixing with the 1-butanethiol include: 0° C., 25-35 min; The conditions for mixing with the propylene sulfide include: 0°C, 1-3h; The conditions for quenching the reaction include: 20-30°C, 10-16h.

18. The preparation method according to claim 7, characterized in that: The preparation steps of modified sodium alginate are as follows: Sodium alginate is mixed with a buffer solution, a pH regulator and a carboxyl activation reagent for reaction, and then a methacrylate compound is added for reaction, and then stirred for precipitation to obtain a precipitate; then, the precipitate is dissolved, dialyzed, filtered and freeze-dried.

19. The preparation method according to claim 18, characterized in that: Carboxyl activation reagents include NHS and EDC·HCl; The methacrylate compound is selected from 2-aminoethyl methacrylate.

20. The preparation method according to claim 19, characterized in that: The usage ratio of the sodium alginate, the buffer solution, the EDC·HCl, the NHS and the 2-aminoethyl methylacrylate is (2-2.5 g): 200 mL: (5-6 g): (1-1.5 g): (1-2 g).

21. The preparation method according to claim 20, characterized in that: The concentration ratio of the buffer solution to the pH adjuster is (0.1-0.2 mol / L): (0.1-0.2 mol / L).

22. The preparation method according to claim 20, characterized in that: After adding the carboxyl activation reagent, stirring and mixing for 3-6 hours, the conditions for adding the methacrylate compound include: temperature of 20-30° C., stirring time of 20-28 hours; The dialysis conditions include: molecular weight cut-off of 3500, time of 48-72 hours; filtration pore of 0.2-0.25 μm, and freeze-drying time of 24-72 hours.

23. The preparation method according to claim 7, characterized in that: include: The polypropylene sulfide and the modified sodium alginate are mixed and stirred for 4-8 hours, and then the mixture is added dropwise to distribute between two adjacent photocurable polycaprolactone areas and then photocured.

Citation Information

Patent Citations

  • Collagen peptide graft sodium alginate sulfate, as well as preparation method and use thereof

    CN103333270A

  • Multifunctional liposome based on hydrogen peroxide response and preparation method and application thereof

    CN110302396A