Bio-based flame retardant paint, coating and preparation method
By introducing modified cellulose and antimony compounds into the bromine antimony flame retardant system, a dense three-dimensional network structure is formed, which solves the smoke problem in the bromine antimony flame retardant system, improves the coating performance, and realizes the environmental protection of bio-based flame retardant coatings. and renewable applications.
Patent Information
- Application Number
- CN202410239451.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-04
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-04
AI Technical Summary
The bromine antimony flame retardant system produces a large amount of toxic and harmful smoke during use. The existing smoke suppressants are not effective. In the existing technology, cellulose is rarely used in flame retardant coatings, and there is a lack of effective bio-based flame retardant materials. solution.
By introducing modified cellulose into the bromine antimony flame retardant system, its three-dimensional network structure is used to prepare bio-based flame retardant coatings, and antimony compounds and metal hydroxides are used as flame retardant fillers to form a dense three-dimensional network structure to reduce smoke and dust. Generate and improve flame retardant properties.
It significantly reduces the volatilization of toxic smoke and dust during the bromine antimony flame retardant process, improves the water resistance, cracking resistance and hardness of the coating, meets the needs of environmental protection and reproducibility, and is suitable for fields such as construction, textiles and steel structures.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of flame retardant coatings, and in particular to a bio-based flame retardant coating, a coating and a preparation method thereof. Background Art
[0002] At present, the bromine antimony flame retardant system is still recognized as the most effective flame retardant system in the industry, but the bromine antimony flame retardant process will produce a lot of toxic and harmful smoke. Smoke suppression is the most urgent problem that needs to be solved in the bromine antimony flame retardant system. The existing solution is usually to add smoke suppressants, but there is no better smoke suppressant for the bromine antimony flame retardant system in the market.
[0003] In addition, cellulose is a renewable resource that exists in large quantities on the earth. With the depletion of resources such as oil, renewable resources are receiving more and more attention. How to utilize bio-based materials such as cellulose will become a hot topic of research.
[0004] In order to solve the above-mentioned problems of the bromine-antimony flame retardant system, the inventors of the present application attempted to introduce cellulose into the bromine-antimony flame retardant system. After in-depth research, they prepared a bio-based flame retardant coating containing cellulose. The coating has excellent comprehensive performance and can reduce the production of toxic and harmful smoke in the original bromine-antimony flame retardant system during the flame retardant process, thereby achieving the effect of smoke suppression.
[0005] After searching, the existing technologies for the application of cellulose in coatings in China are found, for example, the Chinese patent document announcement number is CN112144316B, and the name of the invention is: a nanocellulose modified acrylic resin and its preparation method and decorative paper; the Chinese patent document announcement number is CN115028774B, and the name of the invention is: a method for preparing a modified cellulose copolymer acrylic acid type amphoteric organic water-resistant dispersant; the Chinese patent document announcement number is CN106009458B, and the name of the invention is: a pineapple peel residue cellulose-g-acrylic acid / kaolin / squid ink gel and its preparation method and application; the Chinese patent document announcement number is CN109385185B, and the name of the invention is: a water-based hemicellulose / cellulose / acrylic acid-epoxy resin coating and its preparation method.
[0006] The above schemes are all innovative attempts to use cellulose in the field of coatings, but there are few literature reports on the use of cellulose for flame retardancy. Since flame retardant coatings are widely and long-term used in large quantities, they play an important role in national economic production safety and residents' lives. Therefore, how to combine renewable materials with flame retardant materials to prepare bio-based flame retardant coatings is of great value and significance for the application in the field of coatings. Summary of the invention
[0007] In view of the above problems, one of the objects of the present invention is to provide a bio-based flame retardant coating, coating and preparation method. By improving the material component system and introducing modified cellulose into the bromine antimony flame retardant system, a flame retardant coating with excellent comprehensive performance is prepared by utilizing the three-dimensional network structure of modified cellulose. The coating can be used in flame retardant fields such as construction, textiles, and steel structures.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] In a first aspect, the present invention provides a bio-based flame retardant coating, comprising the following raw materials in weight percentage:
[0010] Acrylic resin 5%~50%
[0011] Brominated styrene butadiene rubber resin 5%~50%
[0012] Modified cellulose 5%~30%
[0013] Flame retardant filler 10%~50%
[0014] Additives 1%~5%,
[0015] The flame retardant filler is a mixture of antimony compounds and metal hydroxides.
[0016] In an achievable implementation of the first aspect, the antimony compound is antimony trioxide;
[0017] And / or, the metal hydroxide is at least one of aluminum hydroxide or magnesium hydroxide.
[0018] In an achievable implementation of the first aspect, the molecular structure of the acrylic resin has a side chain, and the side chain contains a -NR1R2 structure, wherein R1 is a hydrogen atom, and R2 is composed of an alkane containing 1 to 6 carbon atoms.
[0019] The acrylic resin adopts either oil-soluble resin or emulsion;
[0020] And / or, the brominated styrene butadiene rubber resin is any one of an oily resin or an emulsion.
[0021] When using emulsion, the above two resin emulsions should have a higher solid content, preferably, the resin emulsion has a solid content exceeding 40%.
[0022] In an achievable embodiment of the first aspect, the auxiliary agent includes a defoamer and a leveling agent, and the leveling agent is an organic silicon auxiliary agent;
[0023] And / or, the defoaming agent is a silicone additive.
[0024] In an implementation manner that can be realized in the first aspect, the leveling agent is BYK307 leveling agent;
[0025] And / or, the defoamer is BYK024 defoamer.
[0026] In an achievable implementation of the first aspect, the modified cellulose is prepared by modifying cellulose with a silane coupling agent, and a certain number of epoxy groups are grafted onto the macromolecular chain segments of the modified cellulose.
[0027] In an achievable embodiment of the first aspect, the cellulose is a natural plant extract, and the plant sources include grasses and woody plants.
[0028] In a second aspect, the present invention provides a method for preparing a bio-based flame retardant coating, which is used to prepare the above-mentioned bio-based flame retardant coating, comprising the following steps:
[0029] (1) The acrylic resin and the brominated styrene butadiene rubber resin are mixed and ground under heating and stirring conditions. The stirring time is 1 h to 10 h and the heating temperature is 50°C to 80°C. The acrylic resin has a glass transition temperature of 10°C, and the oily brominated styrene butadiene rubber resin has a solid content of 45% and a viscosity of 10,000 centipoise.
[0030] (2) Add functional fillers, including modified cellulose and flame retardant fillers. During the addition of modified cellulose and flame retardant fillers, high-speed heating and stirring are performed at a heating temperature of 50°C to 80°C. The modified cellulose dry powder is dispersed in pure water and tested with a Malvern particle size analyzer. Its particle size distribution D50 is 15 microns. After cellulose is modified, its surface has good hydrophobicity. The flame retardant filler needs to pass through a 325-mesh screen to ensure that the flame retardant coating prepared later has fewer defects.
[0031] (3) Add paint additives while stirring, then let it sit for several hours before packaging.
[0032] In an achievable implementation of the second aspect, in step (1), a basket sand mill is used to mix and grind the acrylic resin and the brominated styrene butadiene rubber resin.
[0033] In a third aspect, the present invention provides a bio-based flame retardant coating, which is obtained by coating the above-mentioned bio-based flame retardant coating on a substrate and drying it.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. After the cellulose is modified in the present invention, a certain number of epoxy groups will be grafted onto the macromolecular chain segments of the cellulose. The epoxy groups of the modified cellulose and the secondary amine groups of the acrylic macromolecular side chains undergo a polymerization reaction when heated, thereby forming a more solid three-dimensional network structure between the acrylic resin and the modified cellulose, so that the obtained coating can produce better properties in terms of water resistance, crack resistance, hardness, etc. In addition, this three-dimensional network structure has a high density, and can effectively reduce the volatilization of volatiles in the flame retardant process of bromine antimony flame retardant during actual use, achieving a good smoke suppression effect.
[0036] 2. The construction of a three-dimensional network structure of modified cellulose has the following advantages: (1) The degradation of coating performance caused by the use of hydroxides is greatly improved; (2) The flame retardant effect of bromine antimony is partially replaced by magnesium hydroxide, which reduces the amount of bromine antimony used; (3) The coating is dense and has excellent comprehensive performance; (4) The dense three-dimensional network structure reduces the volatilization of smoke during the flame retardant process of bromine antimony.
[0037] 3. The modified cellulose in the present invention has many hydroxyl groups, is easy to modify, and can also increase the cross-linking density. The long cellulose chain segments can also play a supporting role in the resin, thereby improving the hardness of the coating.
[0038] 4. The combination of modified cellulose and flame retardant materials is conducive to the preparation of bio-based flame retardant coatings to meet the needs of environmental protection and renewability. The coating can be used in flame retardant fields such as construction, textiles, and steel structures.
[0039] 5. Antimony compounds and metal hydroxides are selected as flame retardant fillers, which have good flame retardant properties. They can effectively suppress the spread of fire when encountering a fire source, and can reduce the release of harmful substances during use, which is in line with modern environmental protection concepts.
[0040] 6. Antimony compounds and metal hydroxides have high heat resistance and can remain stable at higher temperatures. In addition, antimony compounds and metal hydroxides can be well mixed with various types of coating matrices to form coatings with good flame retardant properties.
[0041] 7. The addition of modified cellulose in the present invention significantly reduces the fine cracks caused by stress shrinkage during the drying process of the coating, preventing the coating from cracking. Since cellulose forms a three-dimensional network structure in the brominated flame retardant system, the adhesion of the coating to the substrate is also improved. Moreover, since its network structure can seal the volatile organic matter in the system during the flame retardant process, a good smoke suppression effect is achieved, which is of great significance for the brominated flame retardant system. DETAILED DESCRIPTION
[0042] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1: Currently, flame retardant coatings generally contain a large amount of chemical synthetic resins as the main body, which does not conform to the new trend of international coating development, namely the concept of environmental protection and the utilization of renewable resources. For this reason, we use cellulose, a plant extract that is widely present in nature, as one of the components of flame retardant materials, and modify the cellulose to achieve the replacement of synthetic resins.
[0044] To achieve the above objectives, in a first aspect, an embodiment of the present invention provides a bio-based flame retardant coating, comprising the following raw materials in percentage by weight:
[0045] Acrylic resin 5%~50%
[0046] Brominated styrene butadiene rubber resin 5%~50%
[0047] Modified cellulose 5%~30%
[0048] Flame retardant filler 10%~50%
[0049] Additives 1%~5%,
[0050] The flame retardant filler is a mixture of antimony compounds and metal hydroxides, and brominated styrene butadiene rubber and antimony compounds can form a bromine antimony flame retardant system. Since bromine antimony flame retardant is still recognized as the most effective flame retardant system, but the bromine antimony flame retardant process will produce a lot of toxic and harmful smoke, smoke suppression is the most urgent problem to be solved in the bromine antimony flame retardant system. The existing solution is usually to add smoke suppressants, but there is no better smoke suppressant for bromine antimony flame retardant system in the market, so it is an inevitable choice to reduce the use of bromine antimony flame retardant components as much as possible.
[0051] In order to ensure that the bromine antimony flame retardant system has good flame retardant properties, the mass percentage of the antimony compound in the mixture must be not less than 8% in actual use, so as to give full play to the good flame retardant properties of the bromine antimony flame retardant system in the coating. Preferably, in this embodiment, the antimony compound is antimony trioxide, and the metal hydroxide is aluminum hydroxide or magnesium hydroxide.
[0052] In this embodiment, hydroxide is used to replace part of the antimony compounds. On the one hand, it can solve the problem of reduced flame retardant efficiency caused by reducing bromine antimony flame retardant fillers. On the other hand, it can effectively reduce the toxic and harmful smoke generated by the bromine antimony flame retardant system during the flame retardant process, thereby achieving a better smoke suppression effect.
[0053] However, when hydroxide is added as a flame retardant filler, new problems will arise. That is, hydroxide will cause the coating's water resistance to decrease, the coating to crack easily, the construction performance to be poor, the coating's impact resistance to decrease, and other issues. These problems will not only cause the coating to be unqualified (metal components will cause internal rust), but will also cause a decrease in flame retardant efficiency.
[0054] In order to solve the above problems, in this embodiment, modified cellulose is introduced into the bromine antimony flame retardant system, and the modified cellulose is used to react with acrylic acid macromolecules to generate a three-dimensional network structure, thereby preparing a flame retardant coating with excellent comprehensive performance, so that the formed flame retardant coating meets the requirements of industrial coatings. This is specifically achieved by the following methods:
[0055] In this embodiment, the molecular structure of the acrylic resin has a side chain, and the side chain contains a -NR1R2 structure, wherein R1 is a hydrogen atom, and R2 is composed of an alkane containing 1 to 6 carbon atoms. The acrylic resin adopts any one of an oil-soluble resin or an emulsion; the brominated styrene-butadiene rubber resin adopts any one of an oily resin or an emulsion. When an emulsion is used, the above two resin emulsions should have a higher solid content, preferably, a resin emulsion with a solid content exceeding 40%.
[0056] In this embodiment, the additives include defoamers and leveling agents, the leveling agent is an organic silicon additive; the defoamer is an organic silicon additive. Preferably, in this embodiment, the leveling agent is BYK307 leveling agent; the defoamer is BYK024 defoamer.
[0057] In this embodiment, the modified cellulose is prepared by modifying cellulose with a silane coupling agent, and a certain number of epoxy groups are grafted onto the macromolecular chain segments of the modified cellulose. Preferably, the silane coupling agent in this embodiment is γ-(2,3-epoxypropoxy)propyltrimethoxysilane (i.e., silane coupling agent KH560), which can obtain a certain lipophilicity while retaining some hydrophilicity (cellulose is rich in -OH and cannot completely react with the modifier), and can play a certain emulsifying role, thereby improving the stability of the resin. The cellulose is a natural plant extract, and the plant sources include gramineous plants and woody plants.
[0058] In this embodiment, the addition of modified cellulose significantly reduces the fine cracks caused by stress shrinkage during the drying process of the coating, preventing the coating from cracking. Since cellulose forms a three-dimensional network structure in the brominated flame retardant system, the adhesion of the coating to the substrate is also improved. Moreover, since its network structure can seal the volatile organic matter in the system during the flame retardant process, a good smoke suppression effect is achieved, which is of great significance for the brominated flame retardant system.
[0059] Since the epoxy groups on the modified cellulose molecular chain segments and the secondary amine groups on the side chains of the acrylic macromolecules will undergo a polymerization reaction when heated, a more solid three-dimensional network structure is formed between the acrylic resin and the modified cellulose, making the coating high in density, good in water resistance, no cracking of the coating, and good in impact resistance. In addition, the three-dimensional network structure of the modified cellulose has a high density, which can effectively reduce the volatilization of volatiles in the bromine antimony flame retardant process during actual use, so that the obtained coating can have better characteristics in terms of water resistance, crack resistance, hardness, etc., making it meet the use requirements of industrial coatings.
[0060] In summary, the construction of the three-dimensional network structure of the modified cellulose has the following advantages: (1) the reduction in coating performance caused by the use of hydroxides is greatly improved; (2) the flame retardant part of bromine antimony is replaced by magnesium hydroxide, which reduces the use of bromine antimony; (3) the coating is dense and has excellent comprehensive performance; (4) the dense three-dimensional network structure reduces the volatilization of smoke during the flame retardant process of bromine antimony, achieving the effect of smoke suppression.
[0061] In a second aspect, the present invention provides a method for preparing a bio-based flame retardant coating, which is used to prepare the above-mentioned bio-based flame retardant coating, comprising the following steps:
[0062] (1) The two resins, acrylic resin and brominated styrene butadiene rubber resin, are mixed and stirred under heating and stirring conditions, the stirring time is 1h~10h, the heating temperature is 50℃~80℃, the acrylic resin has a glass transition temperature of 10℃, the oily brominated styrene butadiene rubber resin has a solid content of 45%, and its viscosity is 10000 centipoise. Among them, brominated butyl rubber (BIIR) is an isobutylene-isoprene copolymer elastomer containing active bromine. Since brominated butyl rubber has a basically saturated main chain of butyl rubber, it has many performance characteristics of butyl polymers, such as higher physical strength, better vibration damping performance, low permeability, aging resistance and weather aging resistance.
[0063] (2) Add functional fillers, including modified cellulose and flame retardant fillers. During the addition of modified cellulose and flame retardant fillers, high-speed heating and stirring are performed at a heating temperature of 50°C to 80°C. The modified cellulose dry powder is dispersed in pure water and tested with a Malvern particle size analyzer. Its particle size distribution D50 is 15 microns. After cellulose is modified, its surface has good hydrophobicity. The flame retardant filler needs to pass through a 325-mesh screen to ensure that the flame retardant coating prepared later has fewer defects.
[0064] (3) Add paint additives while stirring, then let it sit for several hours before packaging.
[0065] In an achievable implementation of the second aspect, in step (1), a basket sand mill is used to mix, stir and grind the acrylic resin and the brominated styrene butadiene rubber resin.
[0066] Specifically, in this embodiment, 450 grams of acrylic resin and 260 grams of brominated styrene-butadiene rubber resin are added to the mixing tank of the basket grinder, and the heat conduction oil bath device is connected to heat the mixture, and the oil bath temperature is adjusted to 75°C, and the mixture is stirred for 4 hours. Then 180 grams of modified cellulose is added, and the mixture is stirred for 30 minutes. Then 120 grams of magnesium hydroxide, 345 grams of aluminum hydroxide, and 100 grams of antimony trioxide are added as flame retardant fillers, and the mixture is stirred for 2 hours. The mixture is stirred but the circulation function of the oil bath heating device is turned off, and the mixture is cooled naturally to room temperature. Then 10.5 grams of leveling agent BYK307 and 22 grams of defoaming agent BYK024 are added, and the mixture is stirred at high speed for 1 hour, and then the stirring is stopped. The mixture is discharged after standing for 2 hours.
[0067] In a third aspect, the present invention provides a bio-based flame retardant coating, which is obtained by coating the above-mentioned bio-based flame retardant coating on a substrate and drying it.
[0068] Embodiment 2: The present invention provides a method for preparing a bio-based flame retardant coating, which is used to prepare the above-mentioned bio-based flame retardant coating, comprising the following steps:
[0069] (1) The acrylic resin and the brominated styrene butadiene rubber resin are mixed and stirred under heating and stirring conditions. The stirring time is 1 h to 10 h and the heating temperature is 50°C to 80°C. The acrylic resin has a glass transition temperature of 10°C, and the oily brominated styrene butadiene rubber resin has a solid content of 45% and a viscosity of 10,000 centipoise.
[0070] (2) Add functional fillers, including modified cellulose and flame retardant fillers. During the addition of modified cellulose and flame retardant fillers, high-speed heating and stirring are performed at a heating temperature of 50°C to 80°C. The modified cellulose dry powder is dispersed in pure water and tested with a Malvern particle size analyzer. Its particle size distribution D50 is 15 microns. After cellulose is modified, its surface has good hydrophobicity. The flame retardant filler needs to pass through a 325-mesh screen to ensure that the flame retardant coating prepared later has fewer defects.
[0071] (3) Add paint additives while stirring, then let it sit for several hours before packaging.
[0072] Specifically, in this embodiment, 90 grams of acrylic emulsion and 540 grams of brominated styrene butadiene rubber emulsion were added to the mixing tank of the basket grinder, and an external heat-conducting oil bath device was connected to adjust the oil bath temperature to 75°C, and stirring was continued for 4 hours. Then 220 grams of modified cellulose was added, and stirring was continued for 30 minutes. Then 120 grams of magnesium hydroxide, 260 grams of aluminum hydroxide and 140 grams of antimony trioxide were added, and stirring was continued for 2 hours. Stirring was continued but the circulation function of the oil bath heating device was turned off, and the stirring tank was naturally cooled to room temperature. Then 16 grams of leveling agent BYK307 and 20.5 grams of defoaming agent BYK024 were added, and high-speed stirring was continued for 1 hour, and then stirring was stopped. After standing for 2 hours, the material was discharged.
[0073] Comparative Example 1: In this comparative example, 200 grams of acrylic emulsion and 150 grams of brominated styrene butadiene rubber emulsion were added to the mixing tank of the basket grinder, and the mixture was heated by an external heat-conducting oil bath device. The oil bath temperature was adjusted to 75°C and the mixture was stirred for 4 hours. 240 grams of magnesium hydroxide and 150 grams of antimony trioxide were added as flame retardant fillers, and the mixture was stirred for 2 hours. The mixture was stirred but the circulation function of the oil bath heating device was turned off, and the mixture was cooled naturally to room temperature. 19 grams of leveling agent BYK307 and 18 grams of defoaming agent BYK024 were added, and the mixture was stirred at high speed for 1 hour, then the stirring was stopped, and the mixture was discharged after standing for 2 hours.
[0074] Comparative Example 2: In this comparative example, 550 g of brominated styrene butadiene rubber latex, 240 g of antimony trioxide and 420 g of aluminum hydroxide as flame retardant filler were added to a mixing tank of a basket mill, and stirring was continued for 2 hours. 10 g of leveling agent BYK307 and 9 g of defoamer BYK024 were added, and high-speed stirring was continued for 1 hour, and then stirring was stopped and the material was discharged after standing for 2 hours.
[0075] The four samples in the above-mentioned Examples 1-2 and Comparative Examples 1-2 were tested and the results are as follows:
[0076] The coatings of the four samples in the above-mentioned Examples 1-2 and Comparative Examples 1-2 were uniformly scraped on a self-made cement gypsum substrate, which was 3 cm thick, flat on the surface, and polished with 100-mesh sandpaper. The coating thickness was 200 μm by scraping method, and the coating was evaporated and dried at room temperature (25°C) for 48 hours, and then dried at 110 degrees for 2 hours. The dried coated substrate was cut into a 15 cm x 15 cm substrate block, and the edges were sealed for protection.
[0077] The contents not described in detail in this specification belong to the prior art known to the professional and technical personnel in this field. In the description of the present invention, unless otherwise specified, "multiple" means two or more. Although the present invention is described in detail with reference to the aforementioned embodiments, it is still possible for the technical personnel in this field to modify the technical solutions recorded in the aforementioned embodiments, or to replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A bio-based flame retardant coating, characterized in that: The following raw materials are included in weight percentage: Acrylic resin 5%~50% Brominated styrene butadiene rubber resin 5%~50% Modified cellulose 5%~30% Flame retardant filler 10%~50% Additives 1%~5%, The flame retardant filler is a mixture of antimony compounds and metal hydroxides; The molecular structure of the acrylic resin has a side chain, and the side chain contains a -NR1R2 structure, wherein R1 is a hydrogen atom, and R2 is composed of an alkane containing 1 to 6 carbon atoms; The modified cellulose is prepared by modifying cellulose with a silane coupling agent, and a certain number of epoxy groups are grafted onto the macromolecular chain segments of the modified cellulose.
2. The bio-based flame retardant coating according to claim 1, characterized in that: The antimony compound is antimony trioxide; And / or, the metal hydroxide is at least one of aluminum hydroxide or magnesium hydroxide.
3. The bio-based flame retardant coating according to claim 1, characterized in that: The acrylic resin is any one of an oil-soluble resin or an emulsion; And / or, the brominated styrene butadiene rubber resin is any one of an oily resin or an emulsion.
4. The bio-based flame retardant coating according to claim 1, characterized in that: The additives include defoamers and leveling agents: The leveling agent is an organic silicon auxiliary agent; And / or, the defoaming agent is a silicone additive.
5. The bio-based flame retardant coating according to claim 1, characterized in that: The cellulose is a natural plant extract, and the plant sources include grass plants and woody plants.
6. A method for preparing a bio-based flame retardant coating, for preparing the bio-based flame retardant coating according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Mixing and grinding the acrylic resin and brominated styrene-butadiene rubber resin under heating and stirring conditions, wherein the stirring time is 1 h to 10 h and the heating temperature is 50°C to 80°C; (2) adding functional fillers, including modified cellulose and flame retardant fillers, and heating and stirring at high speed during the addition of modified cellulose and flame retardant fillers, with the heating temperature being 50°C to 80°C; (3) Add paint additives while stirring, then let it sit for several hours before packaging.
7. The method for preparing the bio-based flame retardant coating according to claim 6, characterized in that: In step (1), a basket sand mill is used to mix and grind the acrylic resin and the brominated styrene butadiene rubber resin.
8. A bio-based flame retardant coating, which is obtained by coating the bio-based flame retardant coating according to any one of claims 1 to 5 on a substrate and drying the coating.