A superhydrophobic Raman sensor chip and its fabrication and detection methods

By processing single-crystal silicon wafers with improved etching and magnetron sputtering techniques, combined with zinc oxide solution treatment, a superhydrophobic Raman sensor chip was prepared, solving the problems of complex preparation and insufficient sensitivity in existing technologies, and realizing high-sensitivity and low-cost food detection.

CN118326350BActive Publication Date: 2026-11-10HEZE UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410428514.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-10
Publication Date
2026-11-10
Estimated Expiration
2044-04-10

AI Technical Summary

Technical Problem

Existing SERS substrates are complex to prepare, lack sufficient sensitivity, and are costly, making it difficult to meet the needs of efficient food detection.

Method used

A superhydrophobic Raman sensor chip was fabricated by treating single-crystal silicon wafers with an improved etching solution and magnetron sputtering technique, combined with zinc oxide alkaline solution treatment, and then using nano-silver paste for detection.

Benefits of technology

A Raman sensor chip with high sensitivity, high stability and low cost has been developed, which can detect trace chemical molecules and reduces the complexity and cost of preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118326350B_ABST
    Figure CN118326350B_ABST
Patent Text Reader

Abstract

This invention proposes a superhydrophobic Raman sensor chip and its fabrication and detection methods. Common materials such as silicon, zinc oxide, and silver are used. A modified alkaline etching solution, including potassium hydroxide, deionized water, and propanol, is used to etch a single-crystal silicon wafer. The chip is then treated with magnetron sputtering and an alkaline zinc oxide solution, resulting in a Raman sensor chip with advantages of high sensitivity, high stability, and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of Raman detection technology, and particularly relates to a superhydrophobic Raman sensing chip and its preparation and detection methods. Background Technology

[0002] The statements in this section are merely background information related to the present invention and do not necessarily constitute prior art.

[0003] Surface-enhanced Raman scattering (SERS) is an important technique in the field of food detection. It utilizes the strong localized plasmon resonances generated on the surface of metal nanoparticles or structures to spectrally visualize the chemical bonds of various food additives or harmful substances, enabling the detection of trace or minute amounts of chemical molecules. However, the experimental preparation of existing SERS substrates typically requires precise control over the shape, size, and distribution of the metal nanoparticles or structures. This necessitates a series of complex chemical synthesis and processing steps, increasing the cost and difficulty of preparation, and also resulting in insufficient sensitivity. Summary of the Invention

[0004] To overcome the shortcomings of the prior art, this invention provides a superhydrophobic Raman sensor chip and its preparation and detection methods. Common materials such as silicon, zinc oxide, and silver are used, and a modified alkaline etching solution, including potassium hydroxide, deionized water, and propanol, is used to etch a single-crystal silicon wafer. Based on magnetron sputtering and treatment with an alkaline zinc oxide solution, the prepared Raman sensor chip has the advantages of high sensitivity, high stability, and low cost.

[0005] To achieve the above objectives, a first aspect of the present invention provides a method for fabricating a superhydrophobic Raman sensor chip, comprising:

[0006] Step 1: Etch the single-crystal silicon wafer using an etching solution, then remove it, rinse and dry it; the etching solution includes potassium hydroxide, deionized water and propanol;

[0007] Step 2: The dried single-crystal silicon wafer is processed using magnetron sputtering, and then subjected to...

[0008] Heat, cooling;

[0009] Step 3: Immerse the cooled monocrystalline silicon wafer in an alkaline zinc oxide solution, then rinse, dry, and bake it in sequence.

[0010] A second aspect of the present invention provides a superhydrophobic Raman sensing chip, which is prepared by the superhydrophobic Raman sensing chip preparation method described above.

[0011] A third aspect of the present invention provides a detection method based on a superhydrophobic Raman sensing chip, wherein the Raman sensing chip is prepared using the above-described method for preparing a superhydrophobic Raman sensing chip, comprising:

[0012] The nano-silver paste was uniformly mixed with the solution of the analyte to be tested;

[0013] The uniformly mixed solution was dropped onto the Raman sensor chip, dried, and then detected using a Raman spectrometer.

[0014] The above one or more technical solutions have the following beneficial effects:

[0015] In this invention, commonly used materials such as silicon, zinc oxide, and silver are used. An improved alkaline etching solution, which includes potassium hydroxide, deionized water, and propanol, is used to etch single-crystal silicon wafers. Based on magnetron sputtering and treatment with zinc oxide alkaline solution, the Raman sensor chip prepared has the advantages of high sensitivity, high stability, and low cost.

[0016] Advantages of additional aspects of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description

[0017] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0018] Figure 1 This is a scanning electron microscope (SEM) image of the "textured silicon" structure in Embodiment 1 of the present invention;

[0019] Figure 2 This is a scanning electron microscope (SEM) image of the "textured silicon / zinc oxide nanowire" structure in Embodiment 1 of the present invention;

[0020] Figure 3 The image shows a scanning electron microscope (SEM) image of the Raman sensing chip "textured silicon / zinc oxide nanowires / silver nanoparticles" in Embodiment 3 of the present invention. Figure 1 ;

[0021] Figure 4 The image shows a scanning electron microscope (SEM) image of the Raman sensing chip "textured silicon / zinc oxide nanowires / silver nanoparticles" in Embodiment 3 of the present invention. Figure 2 ;

[0022] Figure 5 The image shows a scanning electron microscope (SEM) image of the Raman sensing chip "textured silicon / zinc oxide nanowires / silver nanoparticles" in Embodiment 3 of the present invention. Figure 3 ;

[0023] Figure 6 The scanning electron microscope (SEM) image of the "textured silicon / zinc oxide nanowires / silver nanoparticles" Raman sensing chip in Embodiment 3 of this invention has a concentration of 10. -7 -10 -11 Raman detection spectrum of Rhodamine 6G molecule M;

[0024] Figure 7 The scanning electron microscope (SEM) image of the "textured silicon / zinc oxide nanowires / silver nanoparticles" Raman sensing chip in Embodiment 3 of this invention has a concentration of 10. -12 -10 -18 Raman detection spectrum of Rhodamine 6G molecule M;

[0025] Figure 8 This is a physical image of the Raman sensor chip made of "textured silicon / zinc oxide nanowires / silver nanoparticles" after being cut according to Embodiment 3 of the present invention;

[0026] Figure 9 The XRD pattern of the "textured silicon / zinc oxide nanowires / silver nanoparticles" Raman sensor chip in Embodiment 3 of the present invention;

[0027] Figure 10 This is an apparent contact angle diagram of the Raman sensor chip made of "textured silicon / zinc oxide nanowires / silver nanoparticles" in Embodiment 3 of the present invention. Detailed Implementation

[0028] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0029] It should be noted that the terminology used herein is for the purpose of describing particular implementations only and is not intended to limit the exemplary implementations of the present invention.

[0030] Where there is no conflict, the embodiments and features in the embodiments of the present invention can be combined with each other.

[0031] Example 1

[0032] This embodiment discloses a method for fabricating a superhydrophobic Raman sensor chip, including:

[0033] Step 1: Etch the single-crystal silicon wafer using an etching solution, then remove it, rinse and dry it; the etching solution includes potassium hydroxide, deionized water and propanol;

[0034] Step 2: The dried single-crystal silicon wafer is processed by magnetron sputtering, followed by heating and cooling;

[0035] Step 3: Immerse the cooled monocrystalline silicon wafer in an alkaline zinc oxide solution, then rinse, dry, and bake with an infrared lamp.

[0036] The Raman sensor chip prepared by the improved alkaline etching method in this embodiment has the advantages of high sensitivity, high stability and low cost.

[0037] Specifically, before step 1 in this embodiment, the method further includes: using a resistivity of 1 -10 ~1 -12 The surface contaminants were removed by ultrasonic treatment with acetone, isopropanol, ethanol, and deionized water for 15 minutes in sequence, and then the monocrystalline silicon wafer was dried in a vacuum drying oven at 60 degrees Celsius.

[0038] In step 1, the etching solution is prepared by adding potassium hydroxide to a mixed solution of deionized water and isopropanol and stirring thoroughly until completely dissolved to obtain the etching solution.

[0039] In step 1, the dried monocrystalline silicon wafer from step 1 is immersed in the prepared etching solution and etched at 85 degrees Celsius for 100 minutes. Then it is taken out and rinsed with a large amount of deionized water. Subsequently, the monocrystalline silicon wafer is placed in a vacuum drying oven at 60 degrees Celsius to dry.

[0040] In step 2, the dried single-crystal silicon wafer from step 1 is placed on a magnetron sputtering apparatus, the vacuum level is adjusted to 3 Pa, and the sputtering rate is adjusted to... The sputtering target is a zinc oxide target with a purity of 99%, and the sputtering time is 300 seconds.

[0041] Then, the monocrystalline silicon wafers that have undergone magnetron sputtering are placed in a muffle furnace and heated at 400 degrees Celsius for 2 hours.

[0042] In step 3, after the silicon wafer cools down, place it in a saturated zinc oxide alkaline solution. After 30 minutes, remove the silicon wafer, rinse it with plenty of deionized water, and dry it with nitrogen. Then place the silicon wafer under an infrared lamp with the power adjusted to 80 watts and the distance adjusted to 15 cm, and bake for 6 hours.

[0043] The preparation of the zinc oxide alkaline solution specifically includes: adding sodium hydroxide to deionized water, adding zinc oxide powder, and slowly stirring the above solution at room temperature to obtain the zinc oxide alkaline solution.

[0044] As an optional embodiment, 1-10 pieces, approximately 3×3cm in size, are used. 2 Taking the single-crystal silicon processed in step 1 as an example, the preparation of the corresponding etching solution is as follows: add 30 grams of potassium hydroxide to a mixed solution containing 800 ml of deionized water and 100 ml of isopropanol, and stir thoroughly until completely dissolved.

[0045] Ten silicon wafers, after being dried in step 1, were simultaneously immersed in an etching solution and etched at 85 degrees Celsius for 100 minutes. They were then removed and rinsed with plenty of deionized water, and subsequently dried in a vacuum drying oven at 60 degrees Celsius.

[0046] The dried single-crystal silicon wafer from step 1 was placed on a magnetron sputtering apparatus. The vacuum level was adjusted to 3 Pa, and the sputtering rate was adjusted to [value missing]. The sputtering target is a zinc oxide target with a purity of 99%, and the sputtering time is 300 seconds.

[0047] The single-crystal silicon wafers, after being magnetron sputtered, were then placed in a muffle furnace and heated at 400 degrees Celsius for 2 hours. After cooling, the wafers were placed in a saturated zinc oxide alkaline solution for 30 minutes. The wafers were then removed, rinsed thoroughly with plenty of deionized water, and dried with nitrogen. Finally, the wafers were placed under an infrared lamp with a power of 80 watts and a distance of 15 cm and baked for 6 hours.

[0048] The preparation of the zinc oxide alkaline solution specifically includes: adding 80g of sodium hydroxide and 20g of zinc oxide powder to 1L of deionized water, and slowly stirring the solution at room temperature.

[0049] As an optional embodiment, two units approximately 3×3cm in size are used. 2 Taking the single-crystal silicon processed in step 1 as an example, the preparation of the corresponding etching solution is as follows: add 60 grams of potassium hydroxide to a mixed solution containing 1600 ml of deionized water and 200 ml of isopropanol, and stir thoroughly until completely dissolved.

[0050] The silicon wafers dried in step 1 are simultaneously immersed in the etching solution and etched at 85 degrees Celsius for 100 minutes. They are then removed and rinsed with plenty of deionized water. Subsequently, the silicon wafers are dried in a vacuum drying oven at 60 degrees Celsius.

[0051] The dried single-crystal silicon wafer from step 1 was placed on a magnetron sputtering apparatus. The vacuum level was adjusted to 3 Pa, and the sputtering rate was adjusted to [value missing]. The sputtering target is a zinc oxide target with a purity of 99%, and the sputtering time is 300 seconds.

[0052] The single-crystal silicon wafers, after being magnetron sputtered, were then placed in a muffle furnace and heated at 400 degrees Celsius for 2 hours. After cooling, the wafers were placed in a saturated zinc oxide alkaline solution for 30 minutes. The wafers were then removed, rinsed thoroughly with plenty of deionized water, and dried with nitrogen. Finally, the wafers were placed under an infrared lamp with a power of 80 watts and a distance of 15 cm and baked for 6 hours.

[0053] The preparation of the zinc oxide alkaline solution specifically includes: adding 160g of sodium hydroxide and 40g of zinc oxide powder to 2L of deionized water, and slowly stirring the solution at room temperature.

[0054] Similarly, depending on the size of the chip being prepared, the specific values ​​used in the above steps can be increased proportionally according to the formula.

[0055] like Figure 1 The image shown is a scanning electron microscope (SEM) image of the "textured silicon" structure; as shown... Figure 2 The image shown is a scanning electron microscope (SEM) image of the "textured silicon / zinc oxide nanowire" structure.

[0056] Example 2

[0057] The purpose of this embodiment is to provide a superhydrophobic Raman sensing chip, which is prepared using a superhydrophobic Raman sensing chip preparation method described in Embodiment 1.

[0058] Example 3

[0059] The purpose of this embodiment is to provide a detection method based on a superhydrophobic Raman sensor chip. The Raman sensor chip is fabricated using a superhydrophobic Raman sensor chip fabrication method described in Embodiment 1, and includes:

[0060] The nano-silver paste was uniformly mixed with the solution of the analyte to be tested;

[0061] The uniformly mixed solution was dropped onto the Raman sensor chip, dried, and then detected using a Raman spectrometer.

[0062] Specifically, the usage method of the "textured silicon / zinc oxide nanowires / silver nanoparticles" chip is as follows: During detection, take 0.25 mL of silver paste solution and mix it with alcohol or aqueous solution containing the target analyte at a volume ratio of 1:1. Sonicate for 5 minutes to ensure homogeneity. Then, take 10 μL of the mixture and drop it onto the surface of the prepared Raman sensor chip, and dry it in an oven at 45 degrees Celsius. After the sample is completely dry, it can be detected using any brand of Raman spectrometer. It is recommended to take 10 data points and average them.

[0063] The preparation of the nano-silver paste specifically includes: adding 1.30 mL of ethylene glycol to a round-bottom flask, heating it to 140–150°C in an oil bath, then adding 0.2 g (0.2 ± 0.02 g) of polyvinylpyrrolidone (PVP), with an average molecular weight of 5000–1300000; after the PPVP in the solution is completely dissolved, adding 0.05 g (0.05 ± 0.005 g) of silver nitrate, and heating at 150°C for 1 hour. Subsequently, the resulting solution is allowed to cool naturally and transferred to a centrifuge tube, centrifuged at 8000 rpm for 5 minutes; the supernatant is removed, ethanol is added, and the mixture is ultrasonically dispersed and centrifuged again; this process is repeated three times, with the final ultrasonic dispersion followed by sealing.

[0064] like Figure 3 -like Figure 10 As shown, the method of this invention improves the sensitivity of the Raman sensor chip substrate: the lowest detection limit for Rhodamine 6G molecules is approximately 1 × 10⁻⁶. -18 M; The limit of detection for malachite green and melamine molecules is approximately 1 × 10⁻⁶. - 15 M all reached the single-molecule level.

[0065] The method of this invention improves the quantization performance of Raman sensor chips: for Rhodamine 6G molecules, when the concentration is 1×10⁻⁶, -6 M to 1×10 -12 In the M interval, the linear regression coefficient is approximately 0.96; for malachite green and melamine molecules, when the concentration is 1×10 - 7 M to 1×10 -15 For the M interval, the linear regression coefficients were 0.96 and 0.98, respectively.

[0066] The method of this invention improves the stability of Raman sensor chips: for Rhodamine 6G molecules, when the concentration is 1×10 -6 At time M, the relative standard deviations of detection between different batches of substrates and between different detection sites on the same substrate were 6.36% and 6.92%, respectively.

[0067] The method of this invention reduces the cost of SERS chips: specifically for chips with a size of 3×3cm. 2 The cost of each chip is approximately 5 yuan.

[0068] While the specific embodiments of the present invention have been described above in conjunction with the accompanying drawings, this is not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art without creative effort based on the technical solutions of the present invention are still within the scope of protection of the present invention.

Claims

1. A method for fabricating a Raman sensor chip based on superhydrophobicity, characterized in that, include: Step 1: Etch the single-crystal silicon wafer using an etching solution, then remove it, rinse, and dry it. The etching solution comprises potassium hydroxide, deionized water, and propanol; Step 2: The dried single-crystal silicon wafer is processed by magnetron sputtering, followed by heating and cooling; Step 3: Immerse the cooled monocrystalline silicon wafer in a saturated zinc oxide alkaline solution for 30 minutes, then rinse, dry, and bake under an infrared lamp. The zinc oxide alkaline solution is prepared by adding 80g of sodium hydroxide and 20g of zinc oxide powder to 1L of deionized water and stirring slowly at room temperature; or by adding 160g of sodium hydroxide and 40g of zinc oxide powder to 2L of deionized water and stirring slowly at room temperature. In step 1, the preparation of the etching solution specifically involves adding potassium hydroxide to a mixed solution containing deionized water and isopropanol, and stirring thoroughly until completely dissolved to obtain the etching solution. In step 2, magnetron sputtering is used for processing. Specifically, the vacuum level of the magnetron sputtering device is adjusted to 3 Pa, the sputtering rate is adjusted to 1 Å / s-3 Å / s, the sputtering target is a zinc oxide target with a purity of 99%, and the sputtering time is 300 seconds. In step 3, the silicon wafer is rinsed with deionized water and dried with nitrogen gas; then the silicon wafer is baked under an infrared lamp.

2. The method for fabricating a superhydrophobic Raman sensor chip as described in claim 1, characterized in that, Before step 1, the process includes: sequentially using acetone, isopropanol, ethanol, and deionized water to ultrasonically remove contaminants from the surface of the monocrystalline silicon wafer, followed by drying.

3. A Raman sensing chip based on superhydrophobicity, characterized in that, The chip was prepared using the superhydrophobic Raman sensor chip fabrication method as described in any one of claims 1-2.

4. A detection method based on a superhydrophobic Raman sensor chip, wherein the Raman sensor chip is prepared using the superhydrophobic Raman sensor chip fabrication method as described in any one of claims 1-2, characterized in that, include: The nano-silver paste was uniformly mixed with the solution of the analyte to be tested; The uniformly mixed solution was dropped onto the Raman sensor chip, dried, and then detected using a Raman spectrometer.

5. The detection method based on a superhydrophobic Raman sensor chip as described in claim 4, characterized in that, include: The preparation of the nano-silver paste specifically includes: Ethylene glycol was heated using an oil bath heating method, then polyvinylpyrrolidone was added. After complete dissolution, silver nitrate was added, followed by heating, cooling, and centrifugation.

6. The detection method based on a superhydrophobic Raman sensor chip as described in claim 5, characterized in that, After centrifugation, remove the supernatant from the solution, add ethanol, sonicate to disperse evenly, centrifuge again, and repeat several times.

Citation Information

Patent Citations

  • Preparation method of flexible semitransparent surface enhanced Raman substrate and application

    CN112014371A

  • Silver nano-sol-based surface enhanced Raman rapid detection of natural anthraquinone dye in silk

    CN113933284A