A rubber homogeneous permeable floor with a glittering particle structure
Through the process of coating pearlescent powder and using non-vulcanized natural rubber particles, the problems of floor glitter effect and exhaust gas emissions are solved, achieving the goal of maintaining the glitter effect and improving material elasticity in rubber homogeneous and transparent floors, and improving the functionality of the product. and environmental friendliness.
Patent Information
- Application Number
- CN202410766070.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-14
Smart Images

Figure CN118327244B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flooring, and more particularly to a rubber homogeneous and permeable flooring with a glittering particle structure. Background Art
[0002] In the existing floor production technology, pearlescent powder is often directly added to the floor formula as a pigment additive to enhance the product appearance. It usually includes mixing various types of pearlescent powder directly into the raw materials. After being processed by an extruder, it is pressed into sheets by two rollers and then crushed by a crusher to form irregular particles. These particles are then added to environmentally friendly rubber floor materials to enhance the visual effect of the floor. However, this conventional production method has significant loss of pearlescent effect and uneven distribution efficiency problems and quality defects, resulting in unsatisfactory sparkle effect of the final product.
[0003] At the same time, in order to obtain the required elasticity and wear resistance, natural rubber particles need to be added to the rubber floor. However, since the non-vulcanized natural rubber particles are very sticky, they will clump after a short period of standing and cannot be added to the non-vulcanized elastic rubber floor. The vulcanized natural rubber particles have formed a cross-linked structure through the chemical reaction triggered by heating. The hardness of the particles cannot be processed and molded again, which will cause the material to crack. The current rubber floor production process has a small batch and phased production method, which not only has a large color difference, but also generates a wide variety of waste gases during the high-temperature vulcanization process, including flue gas, various sulfur oxides, sulfides such as hydrogen sulfide, thiols, hydrocarbons and indole waste gases. If these waste gases are not effectively collected and treated, they will have a significant impact on the environment. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a rubber homogeneous permeable floor with a shiny particle structure, so as to improve the pearlescent effect of the shiny particles in the homogeneous permeable floor and reduce exhaust gas emissions and treatment through non-vulcanized rubber.
[0005] The above technical purpose of the present invention is achieved through the following technical scheme: a rubber homogeneous permeable floor with a glittering particle structure, comprising a floor body, the floor body comprising a plurality of mixed granules, the mixed granules are provided with a plurality of glittering particles and non-vulcanized natural rubber particles, the glittering particles comprise pearlescent powder and transparent thermoplastic elastomer, the outer surface of the pearlescent powder is provided with a coating, the coating is a liquid lubricant, the liquid lubricant is 1% stearic acid, the pearlescent powder is mixed with a raw material mixture after being coated with the coating, and the pearlescent powder is embedded in the raw material mixed particles formed by the raw material mixture after molding, the raw material mixture comprises the following raw materials in weight proportion: 93-97% thermoplastic elastomer, 0.4-0.6% anti-ultraviolet agent, 0.3-0.8% antioxidant and auxiliary additives.
[0006] The present invention also discloses a rubber homogeneous permeable floor with a glittering particle structure, comprising a floor body, wherein the floor body comprises a plurality of mixed granular materials, wherein the mixed granular materials are provided with a plurality of glittering particles and non-vulcanized natural rubber particles, wherein the glittering particles comprise pearlescent powder and a transparent thermoplastic elastomer, wherein a coating is provided on the outer surface of the pearlescent powder, wherein the coating is used to coat the pearlescent powder by adding the pearlescent powder after the raw material mixture has completed a plurality of shearing operations, wherein the raw material mixture comprises the following raw materials in weight proportion: 93-97% thermoplastic elastomer, 0.4-0.6% anti-ultraviolet agent, 0.3-0.8% antioxidant and auxiliary additives.
[0007] The present invention is further configured as follows: the non-vulcanized natural rubber particles include a thermoplastic elastomer and a filler, the thermoplastic elastomer includes TPU or TPE, and the filler includes kaolin or calcium carbonate.
[0008] The present invention is further configured as follows: the processing equipment of the glitter particles comprises a twin-screw extruder, a barrel of the twin-screw extruder is provided with a plurality of shearing modules, the twin-screw extruder is provided with a vacuum port, and a pearl powder adding mechanism is provided at the front end of the vacuum port.
[0009] The present invention is further configured as follows: the processing steps of the flash particles are as follows:
[0010] Step 1: First, 93-97% of thermoplastic elastomer, 0.4-0.6% of anti-ultraviolet agent, 0.3-0.8% of antioxidant and auxiliary additives are put into a high-speed mixer for blending, and the mixture is fully mixed, and then dried after being discharged to obtain a raw material mixture;
[0011] Step 2: Add the raw material mixture to the feeding port of the twin-screw extruder, melt blend, and pass the raw material mixture through the shearing module at the front end of the vacuum port of the twin-screw extruder. Then, add the pearlescent powder from the pearlescent powder adding mechanism, mix it with the molten raw material mixture, and pass through the shearing module set in the conveying section of the twin-screw extruder.
[0012] Step 3: Through weight loss weighing or adjusting the extrusion speed ratio to draw the wire, extrude the granules and then dry them to obtain the glitter particles.
[0013] The present invention is further configured as follows: the aspect ratio of the twin-screw extruder is greater than 34:1, the number of times the pearlescent powder passes through the shearing module is less than the number of times the raw material mixture passes through the shearing module, and the difference is at least 1.
[0014] The present invention is further configured as follows: the manufacturing process steps of the non-vulcanized natural rubber particles are as follows:
[0015] Step 1, putting the following raw materials in weight proportion: 10-16% thermoplastic elastomer, 5-12% silicon dioxide, 4-8% rutile titanium dioxide and 28-35% kaolin or calcium carbonate into a high-speed mixer and mixing them evenly to obtain a non-vulcanized natural rubber mixture;
[0016] Step 2: Cool the non-sulfurized natural rubber mixture and put it into an internal mixer, add 30-40% natural rubber blocks from the feeding port of the internal mixer for internal mixing, and after the internal mixing is completed, put it into an open mixer to obtain rubber compound.
[0017] Step 3, using a tablet press to press the rubber compound into sheets, and then using a crusher to crush the sheets into non-vulcanized natural rubber particles;
[0018] Step 4: Pour 1-3% by weight of kaolin or calcium carbonate into the non-vulcanized natural rubber particles and stir slowly.
[0019] The present invention is further configured as follows: the processing steps of the mixed granular material are as follows:
[0020] Step 1, 35-70% of thermoplastic elastomer, 0-10% of SEBS+white oil, 2-5% of pigment, 0-2% of compatibilizer, 0.6-1% of antioxidant, 0.6-1.2% of anti-ultraviolet agent, 0.5-1% of processing stabilizer, 3-15% of non-halogen composite combustion aid, 10-25% of non-halogen inorganic flame retardant, 0-30% of filler, 0-5% of non-vulcanized natural rubber particles and 0-25% of self-recycled material are put into a high-speed mixer and mixed evenly, and stirred and cooled in a low-speed mixer to obtain a mixture;
[0021] Step 2: adding the mixture into a twin-screw extruder for melt blending, and plasticizing and extruding the mixture to obtain a rope material;
[0022] Step 3: Place the rope material on a two-roller mill to press it into a sheet, and then crush it into particles by a crusher;
[0023] Step 4: Put the particles into a horizontal mixer and mix them to obtain mixed particles.
[0024] The present invention is further configured as follows: the processing steps of the rubber homogeneous permeable floor with a glittering particle structure are as follows:
[0025] Step 1: Evenly mix the mixed granules and 0.5-3% of flash particles to obtain broken particles;
[0026] Step 2: Lay the base cloth under the spreading equipment, add the mixed crushed particles into the spreading equipment, and evenly spread the crushed particles;
[0027] Step 3: sending the base cloth covered with the crushed particles into the oven channel, heating and baking, and then rolling it into a sheet through a low-temperature pressing roller to obtain a pressed layer;
[0028] Step 4: Apply UV coating on the surface of the laminated layer, anneal in a drying oven, separate the floor body and the base fabric, and roll it up.
[0029] In summary, the present invention has the following beneficial effects:
[0030] Through the improvement of the process of shiny pearlescent powder, the production of shiny particles in rubber homogeneous permeable flooring with shiny particle structure has been realized. Through the formula and process, non-vulcanized natural rubber particles have been added to the rubber homogeneous permeable flooring to achieve better elasticity effect. The waste gas generated during the high-temperature vulcanization reaction has been reduced in the process. The finished flooring can be recycled and reused to achieve circular renewable resources. In addition, the rubber color difference control effect of the non-vulcanized natural rubber process is also significantly better than that of traditional rubber control, effectively maintaining consistent color performance. Through material selection and process improvement, not only the functionality and environmental friendliness of the rubber homogeneous permeable flooring have been improved, but also the visual effect of the product has been optimized. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a structural schematic diagram of the present invention;
[0032] Figure 2 A schematic diagram of the process flow for producing glitter particles when the coating is a raw material mixture;
[0033] Figure 3 The process flow chart of non-vulcanized natural rubber particles;
[0034] Figure 4 The process flow chart of mixed granules;
[0035] Figure 5 This is a process flow chart of a rubber homogeneous permeable floor with a glittering particle structure;
[0036] Figure 6 This is the finished product rendering of the rubber homogeneous permeable floor with a shiny particle structure.
[0037] In the figure: 1. Floor body; 2. Glitter particles; 3. Twin-screw extruder; 31. Vacuum port. DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments, and all other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making creative work are within the scope of protection of the present invention.
[0039] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0040] like Figure 1 and Figure 6 As shown, the rubber homogeneous permeable floor with a flashing particle structure includes a floor body 1, which is formed by a plurality of mixed granules, wherein a plurality of flashing particles 2 and non-vulcanized natural rubber particles are arranged in the mixed granules, the flashing particles 2 include pearl powder and transparent thermoplastic elastomer, the raw material of the pearl powder is synthetic fluorphlogopite coated with silicon dioxide, titanium dioxide and tin dioxide, the selected pearl powder has a better flashing effect, the thermoplastic elastomer includes transparent TPU or TPE, the non-vulcanized natural rubber particles include thermoplastic elastomer and filler, the filler includes kaolin or calcium carbonate, and the flashing particles 2 are The formula is 96% thermoplastic elastomer, 3% pearl powder, 0.5% antioxidant, and 0.5% light stabilizer. The microstructure of the pearl powder is flaky, which can reflect and refract light to produce a multi-level reflection effect. When light shines on the surface of the pearl powder, light at different angles will be reflected and transmitted differently, forming a visual flash effect. In order to slow down the flash loss of the pearl powder during the processing and reduce the weakening degree of the flash effect, a coating is provided on the outer surface of the pearl powder. The pearl powder coated with the coating still has a high pearl efficiency after processing, and has a good flash effect after forming the floor body 1.
[0041] Example 1
[0042] The coating on the outer surface of the pearl powder is a liquid lubricant, which is 1% stearic acid. Stearic acid is a long-chain fatty acid composed of a carbon chain of 18 carbon atoms and a terminal carboxyl group (-COOH). This structure gives stearic acid good hydrophobicity and the ability to form a protective film on the surface of the pearl powder. This protective film acts as a lubricant, reduces the direct contact of the pearl powder, and reduces the damage caused by shear force. 1% stearic acid is added to the pearl powder, and the mixture is stirred at a slow speed of 60 revolutions per minute for 5 minutes at 85°C. After being coated with the coating, the pearl powder is mixed with the raw material mixture and added into an extruder with weak shearing, and granulated by a water drawing production process to obtain translucent glittering particles 2 with good glittering effect. The raw material mixture includes 96% thermoplastic elastomer, 0.5% anti-ultraviolet agent, 0.5% antioxidant and auxiliary additives. After coating, the pearl powder has a good shearing effect, is not easy to crush, and retains the glittering effect of the pearl powder.
[0043] Example 2
[0044] like Figure 2As shown, the coating on the outer surface of the pearlescent powder is a raw material mixture, and the coating is carried out by adding pearlescent powder to the raw material mixture after completing several shearing operations to coat the pearlescent powder, so as to form translucent glittering particles 2. The processing equipment of the glittering particles 2 includes a twin-screw extruder 3, a shearing module is arranged in the barrel of the twin-screw extruder 3, the twin-screw extruder 3 is provided with a vacuum port 31, a pearlescent powder adding mechanism is arranged at the front end of the vacuum port 31, and the rear end of the vacuum port 31 is the conveying section of the twin-screw extruder 3, the number of shearing modules at the front end of the vacuum port 31 is greater than or equal to 2 sections, and the conveying section is provided with 0-1 section shearing modules.
[0045] The processing steps of the flash particles 2 are as follows:
[0046] Step 1: First, 96% of thermoplastic elastomer, 0.5% of anti-ultraviolet agent, 0.5% of antioxidant and auxiliary additives are put into a high-speed mixer for blending, and the mixture is fully mixed, and then dried after being discharged to obtain a raw material mixture;
[0047] Step 2: Add the raw material mixture to the feeding port of the twin-screw extruder 3, melt blend, and the raw material mixture passes through the shearing module at the front end of the vacuum port 31 of the twin-screw extruder 3, and then add 3% pearlescent powder from the pearlescent powder adding mechanism, mix with the molten raw material mixture, and pass through the shearing module set in the conveying section of the twin-screw extruder 3;
[0048] Step 3: The glitter particles 2 are obtained by weight loss weighing or adjusting the extrusion speed ratio to draw the wire, extruding the granules and then drying them.
[0049] The pearl powder adding mechanism is arranged at the end of the twin-screw extruder 3 and at the front end of the vacuum port 31, so that the raw material mixture can completely pass through the shear module, while reducing the number of times the pearl powder passes through the shear module. The twin-screw extruder 3 with a length-to-diameter ratio of 34:1 or more is used to plasticize the raw material mixture through the barrel temperature and weaken the shearing. The pearl powder is melted and mixed with the raw material mixture that has passed through the shear module at the front end of the vacuum port 31 of the twin-screw extruder 3. After mixing, the molten raw material mixture wraps the pearl powder, and after extrusion granulation, it is dried to obtain translucent glittering particles 2 with better glittering effect.
[0050] Example 3
[0051] like Figure 3 As shown, the manufacturing process steps of non-vulcanized natural rubber particles are as follows:
[0052] Step 1: Put the following raw materials in weight proportion: 15% thermoplastic elastomer, 10% silicon dioxide, 8% rutile titanium dioxide and 32% kaolin or calcium carbonate into a high-speed mixer and mix them evenly to obtain a non-vulcanized natural rubber mixture;
[0053] Step 2, cooling the non-vulcanized natural rubber mixture and putting it into an internal mixer, adding 35% natural rubber blocks from the feeding port of the internal mixer for internal mixing, and after the internal mixing is completed, putting it into an open mixer to obtain rubber compound;
[0054] Step 3, using a tablet press to press the rubber compound into sheets, and then using a crusher to crush the sheets into non-vulcanized natural rubber particles;
[0055] Step 4: Pour 1-3% by weight of kaolin or calcium carbonate into the non-vulcanized natural rubber particles and stir slowly.
[0056] Through this process, non-vulcanized natural rubber particles with low viscosity are obtained. After crushing, the non-vulcanized natural rubber particles are cooled and isolated by a small amount of kaolin or calcium carbonate to reduce the degree of adhesion, facilitate subsequent processing and molding, and reduce the waste gas generated during the high-temperature vulcanization reaction during the process.
[0057] Example 4
[0058] like Figure 2 and Figure 4 As shown, the processing steps of mixed granules are as follows:
[0059] Step 1: put 45% thermoplastic elastomer, 5% SEBS+white oil, 3% pigment, 1% compatibilizer, 0.6% antioxidant, 0.6% anti-ultraviolet agent, 0.8% processing stabilizer, 10% non-halogen composite combustion aid, 15% non-halogen inorganic flame retardant, 10% filler, 3% non-vulcanized natural rubber particles and 6% self-recycled material into a high-speed mixer and mix well, stir and cool in a low-speed mixer to obtain a mixture;
[0060] Step 2: conveying the mixture to a twin-screw extruder 3 for melt blending, and plasticizing and extruding the mixture to obtain a rope material;
[0061] Step 3: Place the rope material on a two-roller mill to press it into sheets of different colors, and then crush it into particles of different colors by a crusher;
[0062] Step 4: Put particles of different colors into a horizontal mixer and mix them to obtain mixed particles.
[0063] Use large mixing equipment to break the mixture into particles of different colors, so that the mixing volume is more than 4.8T at a time, and different pot extraction ratios are mixed again to improve the color consistency of the entire batch of pellets, making the color of the produced products more consistent, thereby reducing rubber color difference defects.
[0064] Example 5
[0065] like Figure 1 and 5 As shown, the processing steps of the rubber homogeneous permeable floor with a flashing particle structure are as follows:
[0066] Step 1: Evenly mix the mixed granules and 3% of the flash granules 2 to obtain broken granules;
[0067] Step 2: Lay the base cloth under the spreading equipment, add the mixed crushed particles into the spreading equipment, and evenly spread the crushed particles;
[0068] Step 3: sending the base cloth covered with the crushed particles into the oven channel, heating and baking, and then rolling it into a sheet through a low-temperature pressing roller to obtain a pressed layer;
[0069] Step 4: Apply UV coating on the surface of the pressed layer, carry out annealing in a drying oven, separate the floor body 1 and the base fabric, and roll them up.
[0070] like Figure 1-Figure 6 As shown, mixed granules of different colors are pressed into gradient colors and then crushed, so that a drawing pattern is formed on the surface of the floor body 1 that is finally produced. Transparent flashing particles 2 that still have a good flashing effect after fusion can be seen on the surface of the floor body 1. Non-vulcanized natural rubber particles are added to the environmentally friendly rubber homogeneous permeable floor through formula and process, which improves the elastic effect of the floor body 1, realizes the production of flashing particles 2 in the rubber homogeneous permeable floor with a flashing particle structure, and reduces the waste gas generated during the high-temperature vulcanization reaction.
[0071] Performance Test:
[0072] Table 1 is the specification of the rubber homogeneous permeable floor with a flashing particle structure:
[0073] Table 1
[0074]
[0075]
[0076] The following is a test of the halogen content of the rubber homogeneous permeable floor with a flashing particle structure. The test method is based on EN14582:2016. The IC analysis results are shown in Table 2:
[0077] Table 2
[0078] Test items unit MDL 001 Fluorine (F) mg / kg 20 ND Chlorine (Cl) mg / kg 50 ND Bromine (Br) mg / kg 50 ND Iodine(I) mg / kg 50 ND
[0079] As can be seen from Table 2, the rubber homogeneous permeable floor with a glittering particle structure does not contain halogen, is environmentally friendly, safe for human health, and durable.
[0080] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
[0081] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A rubber homogeneous permeable floor with a glittering particle structure, comprising a floor body (1), characterized in that: The floor body (1) comprises a plurality of mixed granules, wherein a plurality of glittering particles (2) and non-vulcanized natural rubber particles are arranged in the mixed granules, wherein the glittering particles (2) comprise pearlescent powder and transparent thermoplastic elastomer, wherein the outer surface of the pearlescent powder is provided with a coating, wherein the coating is a liquid lubricant, wherein the liquid lubricant is 1% stearic acid, and after being coated with the coating, the pearlescent powder is mixed with a raw material mixture, and after molding, the pearlescent powder is embedded in the raw material mixed particles formed by the raw material mixture, wherein the raw material mixture comprises the following raw materials in weight proportion: 93-97% thermoplastic elastomer, 0.4-0.6% anti-ultraviolet agent, 0.3-0.8% antioxidant and auxiliary additives.
2. A rubber homogeneous permeable floor with a glittering particle structure, comprising a floor body (1), characterized in that: The floor body (1) comprises a plurality of mixed granules, wherein a plurality of glittering particles (2) and non-vulcanized natural rubber particles are arranged in the mixed granules, wherein the glittering particles (2) comprise pearlescent powder and transparent thermoplastic elastomer, wherein the outer surface of the pearlescent powder is provided with a coating, wherein the coating is applied to the pearlescent powder by adding the pearlescent powder after the raw material mixture has completed a plurality of shearing operations, wherein the raw material mixture comprises the following raw materials in weight proportion: 93-97% thermoplastic elastomer, 0.4-0.6% anti-ultraviolet agent, 0.3-0.8% antioxidant and auxiliary additives.
3. The rubber homogeneous permeable floor with a glittering particle structure according to claim 1 or 2, characterized in that: The non-vulcanized natural rubber particles include a thermoplastic elastomer and a filler, wherein the thermoplastic elastomer includes TPU or TPE, and the filler includes kaolin or calcium carbonate.
4. The rubber homogeneous permeable floor with a glittering particle structure according to claim 3, characterized in that: The processing equipment of the glitter particles (2) comprises a twin-screw extruder (3), a barrel of the twin-screw extruder (3) is provided with a plurality of shearing modules, the twin-screw extruder (3) is provided with a vacuum port (31), and a pearl powder adding mechanism is provided at the front end of the vacuum port (31).
5. The rubber homogeneous permeable floor with a glittering particle structure according to claim 4, characterized in that: The processing steps of the glitter particles (2) are as follows: Step 1: First, 93-97% of thermoplastic elastomer, 0.4-0.6% of anti-ultraviolet agent, 0.3-0.8% of antioxidant and auxiliary additives are put into a high-speed mixer for blending, and the mixture is fully mixed, and then dried after being discharged to obtain a raw material mixture; Step 2: Add the raw material mixture to the feeding port of the twin-screw extruder (3), melt blend, and pass the raw material mixture through the shearing module at the front end of the vacuum port (31) of the twin-screw extruder (3). Then, add 1-3% pearl powder from the pearl powder adding mechanism, mix with the molten raw material mixture, and pass through the shearing module provided in the conveying section of the twin-screw extruder (3); Step 3: weigh by weight loss or adjust the extrusion speed ratio to draw the wire, extrude the granules and then dry them to obtain the glitter particles (2).
6. The rubber homogeneous permeable floor with a glittering particle structure according to claim 5, characterized in that: The length-to-diameter ratio of the twin-screw extruder (3) is greater than 34:1, and the number of times the pearlescent powder passes through the shearing module is less than the number of times the raw material mixture passes through the shearing module, and the difference is at least 1.
7. The rubber homogeneous permeable floor with a glittering particle structure according to any one of claims 4 to 6, characterized in that: The manufacturing process steps of the non-vulcanized natural rubber particles are as follows: Step 1, putting the following raw materials in weight proportion: 10-16% thermoplastic elastomer, 5-12% silicon dioxide, 4-8% rutile titanium dioxide and 28-35% kaolin or calcium carbonate into a high-speed mixer and mixing them evenly to obtain a non-vulcanized natural rubber mixture; Step 2: Cool the non-vulcanized natural rubber mixture and put it into an internal mixer, add 30-40% natural rubber blocks from the feeding port of the internal mixer for internal mixing, and after the internal mixing is completed, put it into an open mixer to obtain rubber compound; Step 3, using a tablet press to press the rubber compound into sheets, and then using a crusher to crush the sheets into non-vulcanized natural rubber particles; Step 4: Pour 1-3% by weight of kaolin or calcium carbonate into the non-vulcanized natural rubber particles and stir slowly.
8. The rubber homogeneous permeable floor with a glittering particle structure according to claim 7, characterized in that: The processing steps of the mixed granules are as follows: Step 1, 35-70% of thermoplastic elastomer, 0-10% of SEBS+white oil, 2-5% of pigment, 0-2% of compatibilizer, 0.6-1% of antioxidant, 0.6-1.2% of anti-ultraviolet agent, 0.5-1% of processing stabilizer, 3-15% of non-halogen composite combustion aid, 10-25% of non-halogen inorganic flame retardant, 0-30% of filler, 0-5% of non-vulcanized natural rubber particles and 0-25% of self-recycled material are put into a high-speed mixer and mixed evenly, and stirred and cooled in a low-speed mixer to obtain a mixture; Step 2: adding the mixture into a twin-screw extruder (3) for melt blending, and plasticizing and extruding the mixture to obtain a rope material; Step 3: Place the rope material on a two-roller mill to press it into a sheet, and then crush it into particles by a crusher; Step 4: Put the particles into a horizontal mixer and mix them to obtain mixed particles.
9. The rubber homogeneous permeable floor with a glittering particle structure according to claim 8, characterized in that: The processing steps of the rubber homogeneous permeable floor with a flashing particle structure are as follows Step 1, mixing the mixed granules and 0.5-3% of the flash particles (2) uniformly to obtain broken particles; Step 2: Lay the base cloth under the spreading equipment, add the mixed crushed particles into the spreading equipment, and evenly spread the crushed particles; Step 3: sending the base cloth covered with the crushed particles into the oven channel, heating and baking, and then rolling it into a sheet through a low-temperature pressing roller to obtain a pressed layer; Step 4: Apply UV coating on the surface of the pressed layer, and after annealing in a drying oven, separate the floor body (1) and the base fabric, and roll them up.