Road paving material and preparation method thereof
By introducing crack self-healing particles into pavement materials and filling cracks with acetone-dissolved polystyrene solution wrapped in epoxy resin, the problem of insufficient crack resistance of thermosetting materials is solved and the service life of the material is significantly increased.
Patent Information
- Application Number
- CN202410493406.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-23
AI Technical Summary
Existing thermosetting pavement materials lack self-healing ability after minor cracks caused by load or deformation, resulting in insufficient crack resistance and affecting service life.
Crack self-healing particles are introduced into pavement paving materials. The particles contain an acetone-dissolved polystyrene solution wrapped in epoxy resin. The elongation at break of the particle shell is lower than that of the epoxy adhesive, ensuring self-healing when cracks occur. The solution can fill and repair cracks.
Significantly improves the service life of road paving materials. Through the effective filling and repair of crack self-healing particles, further damage to cracks is avoided and the crack resistance of the material is enhanced.
Smart Images

Figure CN118359398B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of road paving, and in particular to a road paving material and a preparation method thereof. Background Art
[0002] In the late 1980s, asphalt concrete pavement began to become the main structural form of road paving. However, after years of application, it was found that it had disadvantages such as poor temperature stability, poor water resistance, and easy aging. Especially in scenarios such as steel bridge decks that have high requirements for paving materials, its service life is relatively low. The key reason is that asphalt is a low molecular weight thermoplastic material, and its intrinsic performance is greatly affected by external environment such as temperature.
[0003] In order to improve the comprehensive performance of the paving material system, since 2000, scientific researchers have replaced traditional asphalt with epoxy-modified asphalt and pure epoxy thermosetting materials, making them the preferred choice for high-performance road and bridge deck paving materials, significantly improving the durability of paving materials.
[0004] However, compared with asphalt-based thermoplastic materials, epoxy-based thermosetting paving materials have the following problems: after the paving materials produce fine cracks due to load or deformation, the thermosetting materials do not have the ability of asphalt-based materials to self-heal fine cracks at a certain temperature. As a result, the road paving materials have great deficiencies in crack resistance, which affects the service life of the paving materials.
[0005] Based on this, the present application creates a road paving material and a preparation method thereof, which adds crack self-repairing particles to the thermosetting paving material. When the paving material begins to crack somewhere, the self-repairing solution stored in the crack self-repairing particles can fill the cracks to prevent further damage to the cracks, thereby significantly improving the service life of the paving material. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a road paving material, which adds crack self-repairing particles on the basis of thermosetting paving materials. When the paving material begins to crack somewhere, the self-repairing solution stored in the crack self-repairing particles can fill the cracks to avoid further damage to the cracks, thereby significantly improving the service life of the paving material and overcoming the shortcomings of existing paving materials.
[0007] In order to solve the above technical problems, the present invention provides a road paving material, including mineral aggregate, epoxy adhesive and crack self-repairing particles, the crack self-repairing particles include an outer shell and a self-repairing solution wrapped by the outer shell, and the outer shell is made of an epoxy resin material whose elongation at break after curing is less than the elongation at break of the epoxy adhesive in the road paving material after curing.
[0008] As a further improvement, the self-repairing solution is a polystyrene solution dissolved in acetone.
[0009] Further improvement, the preparation method of the crack self-repairing particles comprises the following steps:
[0010] (1) Take a diameter of 7-9 mm and an apparent density of 25-30 kg / cm 3 of polystyrene foam particles;
[0011] (2) using a coating machine to uniformly coat the outer shell on the surface of the polystyrene foam particles with epoxy resin to obtain a coated outer shell, and then curing the outer shell;
[0012] (3) injecting acetone into the cured coating shell to fully dissolve the polystyrene foam in the acetone to form a self-repairing solution, and sealing the injection port with epoxy resin for the shell. After curing at room temperature, the crack self-repairing particles are obtained.
[0013] As a further improvement, the thickness of the coating shell formed by the epoxy resin of the shell is 0.5-1.0 mm.
[0014] As a further improvement, the epoxy adhesive and the epoxy resin for the shell are both two-component room temperature curing epoxy resins, the elongation at break of the epoxy adhesive after curing is ≥8%, and the elongation at break of the epoxy resin for the shell after curing is ≤3%.
[0015] As a further improvement, the mineral aggregate comprises basalt aggregate A with a particle size of 5-10 mm and basalt aggregate B with a particle size of 10-20 mm, and the mass ratio of aggregate A to aggregate B is 1:1.
[0016] As a further improvement, the epoxy adhesive accounts for 8-10% of the mass of the mineral aggregate, and the crack self-repairing particles account for 3-5% of the mass of the mineral aggregate.
[0017] As a further improvement, the preparation method of the road paving material is: mixing the crack self-repairing particles and mineral aggregates at room temperature for 1-2 minutes, then adding a uniformly mixed epoxy adhesive, and then mixing for 3-5 minutes to obtain the road paving material.
[0018] As another improvement of the present invention, the present invention provides a method for preparing the above-mentioned road paving material, the method comprising the following steps:
[0019] S1. Take a diameter of 7-9mm and an apparent density of 25-30kg / cm 3The polystyrene foam particles are coated with epoxy resin on the surface of the polystyrene foam particles by a coating machine to obtain a coated shell with a thickness of 0.5-1.0 mm, and then cured; acetone is injected into the cured coated shell to fully dissolve the polystyrene foam to form a self-repairing solution, and the injection port is sealed with epoxy resin for the shell, and after curing at room temperature, the crack self-repairing particles are obtained;
[0020] S2. The obtained crack self-repairing particles are mixed with mineral aggregates at room temperature, and epoxy adhesive is added after mixing for 1-2 minutes, and then mixed for another 3-5 minutes to obtain the road paving material.
[0021] Further improvement, the mineral aggregate includes basalt aggregate A with a particle size of 5-10mm and basalt aggregate B with a particle size of 10-20mm, the mass ratio of aggregate A to aggregate B is 1:1, the epoxy adhesive adopts a two-component room-temperature curing epoxy resin, the elongation at break after curing is ≥8%, and the epoxy adhesive accounts for 8-10% of the mass of the mineral aggregate; the epoxy resin for the outer shell adopts a two-component room-temperature curing epoxy resin, the elongation at break after curing is ≤3%, and the crack self-repairing particles account for 3-5% of the mass of the mineral aggregate.
[0022] After adopting such a design, the present invention has at least the following advantages:
[0023] The pavement paving material of the present invention is prepared by mixing crack self-repairing particles, mineral aggregates and epoxy adhesive and fully curing them to form a consolidated body in which crack self-repairing particles are uniformly dispersed in the curing system. When the deformation of the epoxy resin exceeds its elongation at break due to external stress at a certain place, the epoxy adhesive at that place cracks. Since the elongation at break of the epoxy resin coated on the surface of the crack self-repairing particles is significantly lower than the elongation at break of the epoxy adhesive body, the outer shell of the crack self-repairing particles at that place will inevitably crack first, thereby allowing the self-repairing solution stored in the particles to be released. When the solvent therein evaporates, the effective components fill the cracks, making it impossible for media such as water to pass through the place and cause more serious damage, thereby significantly improving the service life of the paving material.
[0024] The preparation method of the crack self-repairing particles and road paving materials of the present invention is simple and convenient, which can not only meet the mechanical mixing strength requirements in the preparation process of the road paving materials, but also ensure timely rupture when cracks appear on the road surface, thereby achieving the requirement of rapid repair of the road surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The above is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0026] Figure 1 It is a schematic diagram of the preparation process of the crack self-repairing particles of the present invention. DETAILED DESCRIPTION
[0027] The exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0028] Example 1
[0029] (I) Preparation of crack self-repairing particles
[0030] (1) Refer to the attached Figure 1 As shown, the diameter is 9mm and the apparent density is 25kg / cm 3 Polystyrene foam particles 1;
[0031] (2) The coating machine temperature is set to 45° C., the nozzle temperature is set to 50° C., the rotation speed is set to 22 rpm, and the spraying peristaltic pump frequency is set to 4 Hz. By controlling the above parameters, the outer shell is evenly coated with epoxy resin on the surface of the above polystyrene foam particles to form particles with an average outer diameter of 10 mm, that is, at this time, the average thickness of the outer shell 2 is 0.5 mm;
[0032] Among them, the resin used is Sinopec Phoenix brand E51, the curing agent is JH-5160 curing agent of Jiadida New Materials Co., Ltd., and the mass ratio of E51 to JH-5160 is 100:48.
[0033] The elongation at break of the shell after it was completely cured with epoxy resin was tested and the result was 2.4%.
[0034] (3) curing the coated particles at 50° C. for 48 h;
[0035] (4) using a syringe with a nominal capacity of 0.5 mL and a needle diameter of 0.3 mm to draw 0.30 mL of acetone 3 and inject it into the interior of the wrapped shell 2 to fully dissolve the polystyrene foam to form a self-healing solution 4;
[0036] (5) Remove the syringe, dip the above shell into epoxy resin to seal the injection port, and cure at room temperature for 72 hours to complete the preparation of the crack self-repairing particle 1.
[0037] (II) Preparation of epoxy adhesive
[0038] In the epoxy adhesive, the resin is Sinopec Phoenix E51, the curing agent is JH-5150 curing agent of Jiadida New Materials Co., Ltd., and the active diluent is JA-712 of Jiadida New Materials Co., Ltd. Moreover, E51: JH-5150: JA-712 = 100: 50: 10 (mass ratio).
[0039] The elongation at break of the epoxy adhesive after complete curing was tested, and the result was 10.5%.
[0040] (III) Preparation of road paving materials
[0041] The quality ratio of each raw material is as follows:
[0042] Basalt aggregate A (particle size 5-10mm): 50 parts
[0043] Basalt aggregate B (particle size 10-20mm): 50 parts
[0044] Crack self-repair particles: 3 pieces
[0045] Epoxy adhesive: 8 parts
[0046] The preparation steps are as follows: add the above-mentioned crack self-repairing particles 1 and mineral aggregates into a mixing container according to a proportion, and mechanically mix for 1 minute; then, mix the epoxy adhesive evenly according to the proportion, add it into the mixing container, and mechanically mix for 3 minutes to obtain the road paving material 1.
[0047] Example 2
[0048] (I) Preparation of crack self-repairing particles
[0049] (1) Select a diameter of 7 mm and an apparent density of 30 kg / cm 3 of polystyrene foam particles;
[0050] (2) The coating machine temperature is set to 50° C., the nozzle temperature is set to 55° C., the rotation speed is set to 18 rpm, and the spraying peristaltic pump frequency is set to 4 Hz. By controlling the above parameters, the outer shell is evenly coated with epoxy resin on the surface of the above polystyrene foam particles to form particles with an average outer diameter of 9 mm, that is, at this time, the average thickness of the outer shell 2 is 1.0 mm;
[0051] Among them, the resin used is Sinopec Phoenix brand E51, the curing agent is JH-5160 curing agent of Jiadida New Materials Co., Ltd., and the mass ratio of E51 to JH-5160 is 100:48.
[0052] The elongation at break of the shell after it was completely cured with epoxy resin was tested and the result was 2.8%.
[0053] (3) curing the coated particles at 50° C. for 48 h;
[0054] (4) using a syringe with a nominal capacity of 0.5 mL and a needle diameter of 0.3 mm to draw 0.16 mL of acetone and inject it into the interior of the package shell to fully dissolve the polystyrene foam to form a self-healing solution;
[0055] (5) Remove the syringe, apply the epoxy adhesive to seal the injection port, and cure at room temperature for 72 hours to complete the preparation of the crack self-repairing particles 2.
[0056] (II) Preparation of epoxy adhesive
[0057] In the epoxy adhesive, the resin is Sinopec Phoenix E51, the curing agent is JH-5150 curing agent of Jiadida New Materials Co., Ltd., and the active diluent is JA-712 of Jiadida New Materials Co., Ltd. Moreover, E51: JH-5150: JA-712 = 100: 50: 10 (mass ratio).
[0058] The elongation at break of the epoxy adhesive after complete curing was tested, and the result was 9.6%.
[0059] (III) Preparation of road paving materials
[0060] The quality ratio of each raw material is as follows:
[0061] Basalt aggregate A (particle size 5-10mm): 50 parts
[0062] Basalt aggregate B (particle size 10-20mm): 50 parts
[0063] Crack self-repair particles: 5 pieces
[0064] Epoxy adhesive: 10 parts
[0065] The preparation steps are as follows: add the above-mentioned crack self-repairing particles 2 and mineral aggregates into a mixing container according to a proportion, and mechanically mix for 2 minutes; then, mix the epoxy adhesive evenly according to the proportion, add it into the mixing container, and mechanically mix for 5 minutes to obtain the road paving material 2.
[0066] Comparative Example 1
[0067] (I) Preparation of coated particles:
[0068] (1) Select a diameter of 9 mm and an apparent density of 25 kg / cm 3 of polystyrene foam particles;
[0069] (2) The coating machine temperature was set to 45° C., the nozzle temperature was set to 50° C., the rotation speed was set to 22 rpm, and the spraying peristaltic pump frequency was set to 4 Hz. By controlling the above parameters, the outer shell was evenly coated on the surface of the above polystyrene foam particles with epoxy resin to form particles with an average outer diameter of 10 mm, that is, the average thickness of the outer shell was 0.5 mm at this time;
[0070] Among them, the resin used is Sinopec Phoenix brand E51, the curing agent is JH-5160 curing agent of Jiadida New Materials Co., Ltd., and the mass ratio of E51 to JH-5160 is 100:48.
[0071] The elongation at break of the shell after it was completely cured with epoxy resin was tested and the result was 2.1%.
[0072] (3) The coated particles were post-cured at 50° C. for 48 h to complete the preparation of coated particles 1.
[0073] (II) Preparation of epoxy adhesive
[0074] In the epoxy adhesive, the resin is Sinopec Phoenix E51, the curing agent is JH-5150 curing agent of Jiadida New Materials Co., Ltd., and the active diluent is JA-712 of Jiadida New Materials Co., Ltd. Moreover, E51: JH-5150: JA-712 = 100: 50: 10 (mass ratio).
[0075] The elongation at break of the epoxy adhesive after complete curing was tested, and the result was 8.9%.
[0076] (III) Preparation of road paving materials
[0077] The quality ratio of each raw material is as follows:
[0078] Basalt aggregate A (particle size 5-10mm): 50 parts,
[0079] Basalt aggregate B (particle size 10-20mm): 50 parts
[0080] Coated particles: 3 parts
[0081] Epoxy adhesive: 8 parts
[0082] The preparation steps are as follows: add the above-mentioned coated particles 1 and mineral aggregates into a mixing container according to a ratio, and mechanically mix for 1 minute; then, mix the epoxy adhesive according to a ratio and add it into the mixing container, and mechanically mix for 3 minutes to obtain the road paving material 3.
[0083] Comparative Example 2
[0084] (I) Preparation of coated particles:
[0085] (1) Select a diameter of 7 mm and an apparent density of 30 kg / cm 3 of polystyrene foam particles;
[0086] (2) The coating machine temperature was set to 50° C., the nozzle temperature was set to 55° C., the rotation speed was set to 18 rpm, and the spraying peristaltic pump frequency was set to 4 Hz. By controlling the above parameters, the outer shell was evenly coated on the surface of the above polystyrene foam particles with epoxy resin to form particles with an average outer diameter of 9 mm, that is, the average thickness of the outer shell was 1.0 mm at this time;
[0087] Among them, the resin used is Sinopec Phoenix brand E51, the curing agent is JH-5160 curing agent of Jiadida New Materials Co., Ltd., and the mass ratio of E51 to JH-5160 is 100:48.
[0088] The elongation at break of the shell after it was completely cured with epoxy resin was tested and the result was 2.7%.
[0089] (3) The coated particles are cured at 50°C for 48 hours to complete the preparation of coated particles 2. (II) Preparation of epoxy adhesive
[0090] In the epoxy adhesive, the resin is Sinopec Phoenix E51, the curing agent is JH-5150 curing agent of Jiadida New Materials Co., Ltd., and the active diluent is JA-712 of Jiadida New Materials Co., Ltd. Moreover, E51: JH-5150: JA-712 = 100: 50: 10 (mass ratio).
[0091] The elongation at break of the epoxy adhesive after complete curing was tested, and the result was 9.8%.
[0092] (III) Preparation of road paving materials
[0093] The quality ratio of each raw material is as follows:
[0094] Basalt aggregate A (particle size 5-10mm): 50 parts
[0095] Basalt aggregate B (particle size 10-20mm): 50 parts
[0096] Coated particles: 5 parts
[0097] Epoxy adhesive: 10 parts
[0098] The preparation steps are as follows: add the above-mentioned coated particles 2 and mineral aggregates into a mixing container according to a proportion, and mechanically mix for 2 minutes; then, mix the epoxy adhesive evenly according to the proportion, add it into the mixing container, and mechanically mix for 5 minutes to obtain the road paving material 4.
[0099] Comparative Example 3
[0100] (I) Preparation of coated particles:
[0101] (1) Select a diameter of 9 mm and an apparent density of 30 kg / cm 3 of polystyrene foam particles;
[0102] (2) The coating machine temperature is set to 45°C, the nozzle temperature is set to 50°C, the rotation speed is set to 22 rpm, and the spray peristaltic pump frequency is set to 4 Hz. By controlling the above parameters, the outer shell is evenly wrapped on the surface of the above polystyrene foam particles with epoxy resin to form particles with an average outer diameter of 10 mm, that is, the average thickness of the outer shell is 0.5 mm at this time.
[0103] Among them, the resin is Sinopec Phoenix brand E51, the curing agent is JH-5140 curing agent of Jiadida New Materials Co., Ltd., and the active diluent is JA-712 of Jiadida New Materials Co., Ltd., and E51:JH-5140:JA-712=100:40:20 (mass ratio).
[0104] The elongation at break of the shell after it was completely cured with epoxy resin was tested and the result was 18.7%.
[0105] (3) curing the coated particles at 50° C. for 48 h;
[0106] (4) using a syringe with a nominal capacity of 0.5 mL and a needle diameter of 0.3 mm to draw 0.30 mL of acetone and inject it into the interior of the package shell to fully dissolve the polystyrene foam to form a self-healing solution;
[0107] (5) Remove the syringe, apply the epoxy adhesive to seal the injection port, and cure at room temperature for 72 hours to complete the preparation of coated particles 3.
[0108] (II) Preparation of epoxy adhesive
[0109] In the epoxy adhesive, the resin is Sinopec Phoenix E51, the curing agent is JH-5150 curing agent of Jiadida New Materials Co., Ltd., and the active diluent is JA-712 of Jiadida New Materials Co., Ltd. Moreover, E51: JH-5150: JA-712 = 100: 50: 10 (mass ratio).
[0110] The elongation at break of the epoxy adhesive after complete curing was tested, and the result was 8.8%.
[0111] (III) Preparation of road paving materials
[0112] The quality ratio of each raw material is as follows:
[0113] Basalt aggregate A (particle size 5-10mm): 50 parts
[0114] Basalt aggregate B (particle size 10-20mm): 50 parts
[0115] Coated particles: 5 parts
[0116] Epoxy adhesive: 10 parts
[0117] The preparation steps are as follows: add the above-mentioned coated particles 3 and mineral aggregates into a mixing container according to a proportion, and mechanically mix for 2 minutes; then, mix the epoxy adhesive according to a proportion and add it into the mixing container, and mechanically mix for 5 minutes to obtain the road paving material 5.
[0118] Water permeability test
[0119] The above-mentioned pavement materials 1-5 were formed separately, cured at room temperature for 14 days, and 250mm×30mm×35mm prismatic beams were prepared according to Item 1.3 of T 0728-2000 in JTG E20-2011. Different strain tests were carried out at -10℃ using a creep tester (the strain ε was set to 1000με, 2000με, 3000με... until failure). After reaching the above strains, the loading was stopped and the test beams were removed. A 20mm diameter permeable test funnel was bonded to the upper surface of the loaded beam with sealant, placed at room temperature for 48 hours to confirm that the sealant was well sealed, and pure water was injected. It was placed at room temperature for another 24 hours, and the water level drop scale was recorded. The permeability test verified whether the microcracks caused by strain inside each test beam were effectively repaired. The results are shown in Table 1 below.
[0120] Table 1 Experimental results of examples and comparative examples
[0121]
[0122] From the results in Table 1 above, it can be seen that the test beams obtained from the pavement paving materials 1-5 obtained from Examples 1-2 and Comparative Examples 1-3 have a failure bending strain range of 4000-5000 με, so water permeability tests after loading strains of 1000 με, 2000 με and 3000 με were performed. The lower the water permeability value in the water permeability test, the better the sealing of the base, that is, the cracks are well sealed and effectively repaired.
[0123] From the above results, it can be seen that the water permeability of the test beams obtained in Examples 1 and 2 is very low, and is far lower than the water permeability of the test beams obtained in Comparative Examples 1-3, especially at 2000με and 3000με, the gap is even greater, indicating that the microcracks are effectively repaired by the crack self-repairing particles, indicating that the crack self-repairing particles in the pavement materials 1 and 2 can crack when the epoxy resin has tiny cracks, and the shell of the crack self-repairing particles at the crack can be cracked, and the self-repairing solution naturally flows out to the crack, achieving effective filling and repair of the crack. Although there are coated particles in the test beams obtained in Comparative Examples 1 and 2, there is no self-repairing solution, so the function of crack repair cannot be achieved. Although the test beam obtained in Comparative Example 3 has coated particles wrapped with self-repairing solution, due to the excessive elasticity of the shell of the coated particles, when the resin in the paving material cracks, the shell of the coated particles produces elastic deformation, and has not yet reached the cracking state, so the self-repairing solution cannot flow out effectively, and thus the effect of automatically repairing cracks cannot be achieved.
[0124] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Those skilled in the art may make some simple modifications, equivalent changes or modifications using the technical contents disclosed above, which all fall within the protection scope of the present invention.
Claims
1. A road paving material, characterized in that: It comprises mineral aggregate, epoxy adhesive and crack self-repairing particles, wherein the crack self-repairing particles comprise a shell and a self-repairing solution wrapped by the shell, wherein the shell is made of an epoxy resin material having a fracture elongation after curing that is less than the fracture elongation of the epoxy adhesive in the road paving material after curing, and the self-repairing solution is a polystyrene solution dissolved in acetone; The preparation method of the crack self-repairing particles comprises the following steps: (1) Take a diameter of 7-9 mm and an apparent density of 25-30 kg / cm 3 of polystyrene foam particles; (2) using a coating machine to uniformly coat the outer shell on the surface of the polystyrene foam particles with epoxy resin to obtain a coated outer shell, and then curing the outer shell; (3) injecting acetone into the cured coating shell to fully dissolve the polystyrene foam in the acetone to form a self-repairing solution, and sealing the injection port with epoxy resin for the shell. After curing at room temperature, the crack self-repairing particles are obtained.
2. The road paving material according to claim 1, characterized in that: The thickness of the coating shell formed by epoxy resin of the shell is 0.5-1.0mm.
3. The road paving material according to claim 1, characterized in that: The epoxy adhesive and the epoxy resin for the shell are both two-component room temperature curing epoxy resins. The elongation at break of the epoxy adhesive after curing is ≥8%, and the elongation at break of the epoxy resin for the shell after curing is ≤3%.
4. The road paving material according to claim 3, characterized in that: The mineral aggregates include basalt aggregate A with a particle size of 5-10 mm and basalt aggregate B with a particle size of 10-20 mm, and the mass ratio of aggregate A to aggregate B is 1:
1.
5. The road paving material according to claim 4, characterized in that: The epoxy adhesive accounts for 8-10% of the mass of the mineral aggregate, and the crack self-repairing particles account for 3-5% of the mass of the mineral aggregate.
6. The road paving material according to claim 5, characterized in that: The preparation method of the road paving material is: mixing the crack self-repairing particles and mineral aggregates at room temperature for 1-2 minutes, then adding epoxy adhesive, and mixing for another 3-5 minutes to obtain the road paving material.
7. A method for preparing the road paving material according to claim 1, characterized in that: The method comprises the following steps: S1. Take a diameter of 7-9mm and an apparent density of 25-30kg / cm 3 The polystyrene foam particles are coated with epoxy resin by a coating machine to uniformly coat the surface of the polystyrene foam particles to obtain a coated shell with a thickness of 0.5-1.0 mm, and then cured; Injecting acetone into the cured coating shell to fully dissolve the polystyrene foam to form a self-repairing solution, and sealing the injection port with epoxy resin for the shell. After curing at room temperature, the crack self-repairing particles are obtained; S2. The obtained crack self-repairing particles are mixed with mineral aggregates at room temperature, and epoxy adhesive is added after mixing for 1-2 minutes, and then mixed for another 3-5 minutes to obtain the road paving material.
8. The method for preparing a road paving material according to claim 7, characterized in that: The mineral aggregate includes basalt aggregate A with a particle size of 5-10 mm and basalt aggregate B with a particle size of 10-20 mm, the mass ratio of aggregate A to aggregate B is 1:1, the epoxy adhesive adopts a two-component room-temperature curing epoxy resin, the elongation at break after curing is ≥8%, and the epoxy adhesive accounts for 8-10% of the mass of the mineral aggregate; the epoxy resin for the shell adopts a two-component room-temperature curing epoxy resin, the elongation at break after curing is ≤3%, and the crack self-repairing particles account for 3-5% of the mass of the mineral aggregate.
Citation Information
Patent Citations
Epoxy-resin concrete repairing material, preparation method and usage method
CN104402303A
Road surface pavement material and road surface pavement material preparation method
CN110593051A