Preparation method and application of super matte high hardness co-extruded fabric for wood plastic
Through the combination of modified matting agent and resin, the problems of excessive gloss and insufficient hardness of wood-plastic composite materials are solved, low gloss, high hardness and wear resistance are achieved, the service life of the material is extended, and it is suitable for outdoor environments.
Patent Information
- Application Number
- CN202410547690.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-06
AI Technical Summary
The excessive gloss of existing wood-plastic composite materials affect the decorative effect and insufficient hardness, resulting in a short service life of the material.
Using a modified matting agent, a super matte high hardness co-extruded fabric is designed through chemical modification of silica, aminosilane coupling agent and fluoroalkyl chloride, combined with HDPE and PP resin and plant fibers, to enhance the The bonding strength and wear resistance of the material.
It realizes the low-gloss and self-extinguishing effect of the material, improves hardness and wear resistance, extends service life, and improves the comprehensive performance of the material. It is suitable for outdoor weather-resistant environments.
Smart Images

Figure GDA0005080174760000161
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of an ultra-matte high-hardness co-extruded fabric for wood-plastic materials. The invention belongs to the technical field of functional wood-plastic materials. Background Art
[0002] Wood-plastic composite materials are a type of environmentally friendly composite materials made of polymer materials as the matrix, plant fibers as the filling components, supplemented with other functional additives, and made through melt extrusion, molding and other processes. They are widely used in the fields of building materials, furniture, logistics packaging, etc. In the prior art, a layer of co-extruded fabric is usually co-extruded on the surface of the wood-plastic composite material through the composite material co-extrusion technology to improve the water vapor barrier performance, weather resistance or aging resistance, wear resistance, etc. of the wood-plastic composite material, and strengthen the durable performance of the wood-plastic composite material.
[0003] As the application of wood plastic becomes more and more extensive, the requirements for the functionality of wood plastic are getting higher and higher. In recent years, researchers have coated wood plastic materials with a layer of plastic fabric with different properties through surface coating or co-extrusion coating, making it an outdoor waterproof and anti-corrosion building material with excellent performance and durability. However, the plastic fabric has too high a gloss, which affects the decorative effect of the wood texture on the one hand, and causes glare during outdoor use, which is harmful to human eyes to a certain extent. The improvement of the wood texture often requires the surface of the wood plastic material to be polished and matte. The currently disclosed preparation methods of co-extruded wood plastic fabrics still lack self-matting and polish-free co-extruded wood plastic fabrics.
[0004] In addition, the commonly used co-extruded fabrics of wood-plastic composite materials are mainly polyethylene, which is a thermoplastic material and has the problem of low hardness, which affects the service life of the material. In view of the problems existing in the above co-extruded wood-plastic fabrics, it is urgent to develop a co-extruded fabric with low gloss and high hardness to meet the requirements of wood-plastic materials. Summary of the invention
[0005] The purpose of the present invention is to provide a super matte high hardness co-extruded fabric for wood-plastic and a preparation method thereof, in order to solve the problems of high gloss and low hardness in the prior art wood-plastic composite products, which lead to obvious plastic texture affecting the decorative effect and insufficient surface hardness affecting the material performance. The self-made modified matting agent is designed through molecular structure, which can improve the bonding strength and wear resistance of the composite product while solving the problems of high gloss and low hardness, and effectively prolong the service life of the used material.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] The present invention provides a method for preparing a modified matting agent, comprising the following steps:
[0008] S11, placing silicon dioxide and an aminosilane coupling agent in an alcohol solvent for silylation coupling reaction to obtain an intermediate product I;
[0009] S12, subjecting the intermediate product I to a ring-opening reaction with an epoxide to obtain an intermediate product II; and
[0010] S13, subjecting the intermediate product II to a substitution reaction with a fluoroalkyl acid chloride to obtain a target product, namely a modified matting agent.
[0011] Further, the silicon dioxide is micron-sized silicon dioxide; and
[0012] The usage of the silicon dioxide, aminosilane coupling agent and alcohol solvent is 1g:3.3-5.5g:80mL.
[0013] Furthermore, the intermediate product I and the epoxy olefins are added in a molar ratio of amino group to epoxy group of 1:1.
[0014] Further,
[0015] The intermediate product II and the fluoroalkyl acid chloride are mixed in a molar ratio of secondary amine to acid chloride of 1:0.6-1.
[0016] The invention also provides a modified matting agent prepared by the preparation method.
[0017] The present invention also provides an ultra-matte high-hardness co-extruded fabric for wood-plastic, comprising the following raw materials in parts by weight:
[0018] HDPE 80-90 parts;
[0019] PP 6-10 parts;
[0020] 5-10 parts of plant fiber;
[0021] Cross-linking agent 0.2-1.0 part;
[0022] 3.0-5.0 parts of modified matting agent;
[0023] 2.0-4.0 parts of inorganic filler;
[0024] Compatibilizer 2.0-4.0 parts;
[0025] Antioxidant 0.5-1.0 part;
[0026] Light stabilizer 0.2-0.5 parts;
[0027] Lubricant 0.3-0.6 parts.
[0028] Furthermore, the melt index of the HDPE is 0.9-1.5 g / 10 min.
[0029] Furthermore, the melt index of the PP is 8.0±2.5 g / 10 min.
[0030] Furthermore, the cross-linking agent is an organic peroxide.
[0031] Furthermore, the lubricant is polyamide wax.
[0032] The present invention also provides a method for preparing an ultra-matte high-hardness co-extruded fabric for wood-plastic composites, comprising the following steps:
[0033] S21, mixing, i.e.
[0034] Add the raw materials into the mixer according to the proportion and mix them. After mixing evenly, cool down and discharge the materials for later use; and
[0035] S22, granulation, i.e.
[0036] The mixed raw materials in S1 are placed in an extruder for melt blending, extrusion and granulation to obtain a co-extruded fabric.
[0037] The invention also provides the use of the co-extruded fabric for preparing the super matte high hardness co-extruded wood-plastic composite material.
[0038] The present invention also provides an ultra-matte high-hardness co-extruded wood-plastic composite material, comprising a wood-plastic core material and a surface layer, wherein the surface layer is formed by co-extruding an ultra-matte high-hardness co-extruded surface material for wood-plastic.
[0039] The present invention also provides a method for preparing an ultra-matte high-hardness co-extruded wood-plastic composite material.
[0040] The core material particles and the co-extruded fabric particles are melted by an extruder and then enter the core material cavity and the fabric cavity, and are shaped by a shaping mold, cooled and formed, and cut to a fixed length to obtain the product.
[0041] Beneficial effects of the present invention:
[0042] (1) The present invention provides an ultra-matte high-hardness co-extruded fabric for wood-plastic, containing a homemade modified matting agent, which is an inorganic silica microsphere material wrapped in an organic structure, wherein the organic structure contains F element, carbon-carbon double bonds, hydroxyl groups, and tertiary amine structures. First, the inorganic material wrapped in the organic structure has excellent dispersibility and improved physical properties; second, small-sized silica has a higher refractive index and transmittance, and has a multiple scattering effect; at the same time, its size is small and has diffraction characteristics; it has an excellent matting effect; third, the F element has a low surface energy, which enriches the inorganic microspheres at the material interface and improves the hardness; fourth, the inorganic microspheres are a spatial three-dimensional structure, which contains multi-functional carbon-carbon double bonds, and will form a higher local cross-linking density during the thermal processing process, and the surface will shrink. Due to the difference in shrinkage rate, its matting property is further improved; fifth, the surface forms a higher cross-linking density At the same time, the hardness and wear resistance are effectively improved; at the same time, the difference in shrinkage rate will cause the flatness of the interface to be destroyed, which is beneficial to improve the bonding strength between the core material and the surface during the co-extrusion process; Sixth, polar groups such as hydroxyl groups and tertiary amine structures form "two-to-two compatibility" with plant fibers and compatibilizers, ultimately improving the comprehensive performance of the material; finally, the tertiary amine structure can be used as a free radical scavenger. On the one hand, it can remove free radicals remaining in the cross-linking agent during thermal processing; on the other hand, it can remove free radicals generated by material degradation during long-term use; it has a synergistic anti-aging effect with antioxidants and light stabilizers, which can effectively improve the service life of the material.
[0043] (2) The present invention provides a super matte high hardness co-extruded fabric for wood plastic, with HDPE and PP as the main resins. The difference in crystallinity and molecular weight between HDPE and PP leads to a subtle "roughness" at the interface of the material, which has a self-matting effect.
[0044] (3) The present invention provides an ultra-matte high-hardness co-extruded fabric for wood-plastic composites, which contains plant fibers. The presence of plant fibers in the surface layer helps to further improve the bonding strength between the surface layer and the core material, thereby extending the service life of the material.
[0045] (4) The present invention provides a super matte high hardness co-extruded fabric for wood-plastic and a preparation method thereof. After material modification, formula design optimization, and synergistic effect of various components, it not only has excellent decorative properties, but also has outstanding water boiling resistance and excellent comprehensive performance. It is suitable for outdoor weather-resistant environment. DETAILED DESCRIPTION
[0046] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0047] The purpose of the present invention is to develop a method for preparing a super matte high hardness co-extruded fabric for wood plastic. The idea of realization is to reduce the gloss by utilizing diffuse reflection of light by increasing the surface roughness of the fabric (self-made modified matting agent). On the one hand, the gloss is reduced by adding matting particles; on the other hand, the molecular weight difference between the matrix resins is utilized to achieve the self-matting effect of the co-extruded fabric (formula design). The theoretical basis for realization is: self-made a modified matting agent. Since silicon dioxide is the most commonly used matting agent, firstly, silicon dioxide is used as the basic raw material, chemically modified by aminosilane, and then reacted with epoxy olefins to graft carbon-carbon double bonds to form a local cross-linked structure to enhance the effect and hardness; thirdly, F element is grafted with fluorine-containing acyl chloride to migrate to the interface to enhance the performance. From the perspective of formula design, HDPE (molecular weight 300,000-400,000), PP (molecular weight 80,000-150,000) and plant fibers are blended to achieve the purpose of self-matting by utilizing the difference in molecular weight; in addition, components such as matte fillers are added to utilize the efficacy of each component and the synergistic volatilization effect to achieve the super matte and high hardness effect of the co-extruded fabric. The embodiments of the present invention are as follows:
[0048] The embodiment of the present invention provides a method for preparing a modified matting agent, comprising the following steps:
[0049] S11, adding silicon dioxide and aminosilane coupling agent to an alcohol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 50-80° C. for 2-10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product I;
[0050] The usage ratio of the silicon dioxide, the aminosilane coupling agent and the alcohol solvent is 1g:3.5-5.5g:80mL.
[0051] The silicon dioxide described in the following examples of the present invention has an average particle size of 2.5 μm and a purity of 98.00%, and is purchased from Guangzhou Lingwei Technology Co., Ltd.
[0052] The aminosilane coupling agent may be KH902, KH540, KH550, KH602, or KH792, and preferably KH550.
[0053] The alcohol solvent may be anhydrous methanol, anhydrous ethanol, anhydrous isopropanol, etc., and anhydrous ethanol is preferred.
[0054] S12, adding the intermediate product I and the epoxy olefin to N,N-dimethylformamide A, and stirring magnetically at 40-60° C. for 2-4 hours; after the reaction, cooling to room temperature, filtering, washing with N,N-dimethylformamide B, and drying the insoluble matter under vacuum at 50° C. to constant weight to obtain the intermediate product II;
[0055] The intermediate product I and the epoxy olefins are added in a molar ratio of amino group to epoxy group of 1:1;
[0056] The usage ratio of the epoxy olefins, N,N-dimethylformamide A and N,N-dimethylformamide B is 1 mol:400 mL:500 mL.
[0057] The epoxy olefins may be allyl glycidyl ether, 1,2-epoxy-5-hexene, 1,2-epoxy-7-octene or 1,2-epoxy-9-decene, etc., and preferably allyl glycidyl ether.
[0058] S13, protect from light, dissolve fluoroalkyl chloride and dichloromethane A in a constant pressure dropping funnel, add dropwise to dichloromethane B containing intermediate II and triethylamine, stir magnetically, ice bath, react at 0-5°C for 5-10h; let stand, stir overnight, filter, take the filtrate, wash with saturated salt water and saturated sodium bicarbonate solution 3 times, respectively, wash with deionized water 3 times, separate the liquids, take the oil phase, distill under reduced pressure, and dry in a vacuum oven at 40°C for 24h to obtain the target product, i.e., the modified matting agent;
[0059] The intermediate product II and the fluoroalkyl acyl chloride are mixed in a molar ratio of secondary amine group to acyl chloride of 1:0.6-1;
[0060] The dosage ratio of the fluoroalkyl chloride, dichloromethane A, triethylamine, dichloromethane B, saturated saline, saturated sodium bicarbonate solution, and deionized water is: 0.1 mol: 100 mL: 0.1 mol: 300 mL: 500 mL: 500 mL: 500 mL.
[0061] The fluoroalkyl acid chloride can be heptafluorobutyryl chloride, nonafluoropentanoyl chloride, perfluorooctanoyl chloride or heptadecafluorononanoyl chloride.
[0062] In the present invention, the reaction raw materials in the modified matting agent step S13 contain both secondary amino groups and secondary hydroxyl groups, both of which are active hydrogen atoms and have reactivity with acyl chlorides. In addition, since the molar number of the secondary amino group and the secondary hydroxyl group is the same, and the reaction ratio is higher than the acyl chloride content, the secondary amino group tends to participate in the reaction mainly because the alkalinity of the secondary amino group is stronger.
[0063] In addition, the fluorine content in the modified matting agent step S13 of the present invention exists in a reasonable range. If the fluorine content is low, there is no migration effect to the interface; if the fluorine content is high, the migration effect is obvious, but the interface bonding strength will be reduced.
[0064] The embodiment of the present invention further provides an ultra-matte high-hardness co-extruded fabric for wood-plastic, comprising the following raw materials in parts by weight:
[0065] HDPE 80-90 parts;
[0066] PP 6-10 parts;
[0067] 5-10 parts of plant fiber;
[0068] Cross-linking agent 0.2-1.0 part;
[0069] 3.0-5.0 parts of modified matting agent;
[0070] 2.0-4.0 parts of inorganic filler;
[0071] Compatibilizer 2.0-4.0 parts;
[0072] Antioxidant 0.5-1.0 part;
[0073] Light stabilizer 0.2-0.5 parts;
[0074] Lubricant 0.3-0.6 parts.
[0075] The HDPE has a melt index of 0.9-1.5 g / 10 min, and may be 3300F (Yangzi Petrochemical), TJDL-9475 (Tianjin United), etc. Moreover, the HDPE described in the following embodiments of the present invention is 3300F (Yangzi Petrochemical).
[0076] The melt index of the PP is 8.0±2.5 g / 10 min, and the PP may be FC801M (Shanghai Petrochemical), F800E (Shanghai Petrochemical), etc. Moreover, the PP described in the following embodiments of the present invention is F800E (Shanghai Petrochemical).
[0077] The plant fiber may be wood powder, bamboo powder, straw powder, rice husk powder, peanut shell powder, coconut shell powder or bagasse powder, etc., and preferably straw powder.
[0078] The crosslinking agent is an organic peroxide. In the present invention, HDPE resin is mainly used, which has a high processing temperature, so a crosslinking agent with a high decomposition temperature is selected, and the crosslinking agent can be di-tert-butyl peroxide, diisopropylbenzene peroxide or methyl ethyl ketone peroxide, etc., and di-tert-butyl peroxide is preferred.
[0079] The inorganic filler may be calcium carbonate, talc, barium sulfate, glass powder, etc., and preferably talc;
[0080] The talcum powder described in the following examples of the present invention is 5000 mesh, plastic grade, purchased from Jiangyin Ousenna Chemical Co., Ltd.
[0081] The compatibilizer is ethylene-acrylic acid copolymer, maleic anhydride grafted PE, maleic anhydride grafted ethylene-vinyl acetate copolymer or epoxy grafted PE, etc., and maleic anhydride grafted PE is preferred, which is purchased from Shanghai Langte Import and Export Co., Ltd.
[0082] The antioxidant is a hindered phenol antioxidant, which may be antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, antioxidant 1098, etc., and antioxidant 1098 is preferred.
[0083] The light stabilizer is a hindered amine light stabilizer, which may be UV-770, UV-622, UV-944, UV-3853, UV-292, UV-123, etc., and preferably UV-770.
[0084] The lubricant is polyamide wax, which may be erucamide wax or oleamide wax, etc., and preferably erucamide wax. The embodiment of the present invention also provides a method for preparing an ultra-matte high-hardness co-extruded fabric for wood-plastic composites, comprising the following steps:
[0085] S21, mixing, i.e.
[0086] Add the raw materials into a mixer according to the proportion and mix them. After high-speed mixing at 105-125° C. and 80-150 rpm for 10-20 minutes, cool and discharge the materials after mixing evenly for later use; and
[0087] S22, granulation, i.e.
[0088] The mixed raw materials in S1 are placed in an extruder for melt blending, extrusion and granulation. The barrel temperature is set at 180-200°C and the screw speed is set at 200-300rpm to obtain a co-extruded fabric.
[0089] The embodiment of the present invention further provides an ultra-matte high-hardness co-extruded wood-plastic composite material, comprising a wood-plastic core material and a surface layer, wherein the surface layer is formed by co-extruding an ultra-matte high-hardness co-extruded surface material for wood-plastic.
[0090] The following embodiment of the present invention is a method for preparing a super matte high hardness co-extruded wood-plastic composite material.
[0091] The core material particles and the co-extruded fabric particles are melted by an extruder and then enter the core material cavity and the fabric cavity, and are shaped by a shaping mold, cooled and formed, and cut to a fixed length to obtain the product.
[0092] The mass ratio of the core material particles to the co-extruded surface particles is 0.08:1.
[0093] During the melting process of the core material particles, the barrel temperature of the extruder is 190-200°C;
[0094] The temperature of each zone of the extruder is 190° C. for zone 1, 200° C. for zone 2, and 195° C. for zone 3, and the rotation speed is 50 rpm.
[0095] During the melting process of the co-extruded fabric particles, the barrel temperature of the extruder is controlled to be 230-240°C;
[0096] The temperature of each zone of the extruder is 230° C. in zone 1, 240° C. in zone 2, and 235° C. in zone 3, and the rotation speed is 50 rpm.
[0097] The core material comprises the following raw materials in parts by weight:
[0098] HDPE 50 parts;
[0099] 35 parts of plant fiber (straw powder);
[0100] 15 parts of 5000 mesh talcum powder;
[0101] 1 part of erucamide wax;
[0102] Maleic anhydride grafted PE 5 parts;
[0103] Silane coupling agent KH-792 1 part.
[0104] The method for preparing the core material comprises the following steps:
[0105] The selected raw materials and proportions are added into a mixer, fully mixed at 110°C and 100 rpm for 20 min, cooled and discharged to obtain a premix for the core material; and added into a parallel twin-screw extruder, extruded and granulated at 180°C and 200 rpm to obtain core material particles for later use.
[0106] In order to further understand the present invention, the preparation method of a super matte high hardness co-extruded fabric for wood-plastic provided by the present invention is described in detail below in conjunction with the embodiments, and the protection scope of the present invention is not limited by the following embodiments.
[0107] Example 1
[0108] A method for preparing a modified matting agent comprises the following steps:
[0109] S11, adding silica and silane coupling agent KH550 to anhydrous ethanol, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 70° C. for 4 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I;
[0110] The usage ratio of the silicon dioxide, the silane coupling agent KH550 and the anhydrous ethanol is 1g:4.5g:80mL.
[0111] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH peak exists; 1109cm-1 、801cm -1 :-Si-O- exists.
[0112] S12, adding the intermediate product I and allyl glycidyl ether to N,N-dimethylformamide A, and stirring magnetically at 50° C. for 3 h; after the reaction, cooling to room temperature, filtering, washing with N,N-dimethylformamide B, and drying the insoluble matter under vacuum at 50° C. to constant weight, to obtain the intermediate product II;
[0113] The intermediate product I and allyl glycidyl ether are added in a molar ratio of amino group to epoxy group of 1:1;
[0114] The usage ratio of allyl glycidyl ether, N,N-dimethylformamide A and N,N-dimethylformamide B is 1 mol:400 mL:500 mL.
[0115] Its infrared data is as follows: 3443cm -1 :-OH exists; 1560cm -1 :-NH peak weakened; 1109cm -1 、801cm -1 :-Si-O- exists; 1262cm -1 、927cm -1 、794cm -1 : Epoxy group does not exist; 1628cm -1 :-C=C- exists.
[0116] S13, protect from light, dissolve nonafluorovaleryl chloride and dichloromethane A in a constant pressure dropping funnel, add dropwise to dichloromethane B containing intermediate II and triethylamine, stir magnetically, ice bath, react at 0°C for 10 hours; let stand, stir overnight, filter, take the filtrate, wash with saturated salt water and saturated sodium bicarbonate solution 3 times, wash with deionized water 3 times, separate the liquids, take the oil phase, distill under reduced pressure, and dry in a vacuum oven at 40°C for 24 hours to obtain the target product, i.e., the modified matting agent;
[0117] The intermediate product II and nonafluorovaleryl chloride are mixed in a molar ratio of secondary amine group to acyl chloride of 1:0.85;
[0118] The dosage ratio of the nonafluorovaleryl chloride, dichloromethane A, triethylamine, dichloromethane B, saturated saline, saturated sodium bicarbonate solution, and deionized water is: 0.1 mol: 100 mL: 0.1 mol: 300 mL: 500 mL: 500 mL: 500 mL.
[0119] Its infrared data is as follows: 3443cm -1 :-OH is weakened (slightly); 1560cm -1: -NH peak weakened (significant); 1109cm -1 、801cm -1 :-Si-O- exists; 1628cm -1 :-C=C- exists; 1250cm -1 :-CF exists.
[0120] A super matte high hardness co-extruded fabric for wood plastic, comprising the following raw materials in parts by weight:
[0121] HDPE 85 parts;
[0122] PP 8 parts;
[0123] 7 parts of straw powder;
[0124] 0.6 part of di-tert-butyl peroxide;
[0125] 4.2 parts of modified matting agent;
[0126] 3.0 parts of talcum powder;
[0127] Maleic anhydride grafted PE 3.0 parts;
[0128] Antioxidant 1098 0.8 parts;
[0129] Light stabilizer UV-770 0.3 parts;
[0130] 0.4 parts of erucamide wax.
[0131] A method for preparing an ultra-matte high-hardness co-extruded fabric for wood-plastic composites comprises the following steps:
[0132] S21, mixing, i.e.
[0133] Add the raw materials into a mixer according to the proportion and mix them. Mix them at a high speed of 115° C. and 100 rpm for 15 minutes. After mixing evenly, cool and discharge the materials for later use.
[0134] S22, granulation, i.e.
[0135] The mixed raw materials in S1 were placed in an extruder for melt blending, extrusion and granulation. The barrel temperature was set to 180°C in zone 1, 190°C in zone 2, 200°C in zone 3 and 190°C in zone 4. The screw speed was 250 rpm to obtain a co-extruded fabric.
[0136] Example 2
[0137] The rest is the same as in Example 1, except that:
[0138] A method for preparing a modified matting agent comprises the following steps:
[0139] S11, adding silica and silane coupling agent KH550 to anhydrous ethanol, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 50° C. for 10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I;
[0140] The usage ratio of the silicon dioxide, the silane coupling agent KH550 and the anhydrous ethanol is 1g:3.5g:80mL.
[0141] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists.
[0142] S12, adding the intermediate product I and allyl glycidyl ether to N,N-dimethylformamide A, and stirring magnetically at 40° C. for 4 h; after the reaction, cooling to room temperature, filtering, washing with N,N-dimethylformamide B, and drying the insoluble matter under vacuum at 50° C. to constant weight, to obtain the intermediate product II;
[0143] The intermediate product I and allyl glycidyl ether are added in a molar ratio of amino group to epoxy group of 1:1;
[0144] The usage ratio of allyl glycidyl ether, N,N-dimethylformamide A and N,N-dimethylformamide B is 1 mol:400 mL:500 mL.
[0145] Its infrared data is as follows: 3443cm -1 :-OH exists; 1560cm -1 :-NH peak weakened; 1109cm -1 、801cm -1 :-Si-O- exists; 1262cm -1 、927cm -1 、794cm -1 : Epoxy group does not exist; 1628cm -1 :-C=C- exists.
[0146] S13, protect from light, dissolve nonafluorovaleryl chloride and dichloromethane A in a constant pressure dropping funnel, add dropwise to dichloromethane B containing intermediate II and triethylamine, stir magnetically, ice bath, react at 5°C for 5 hours; let stand, stir overnight, filter, take the filtrate, wash with saturated salt water and saturated sodium bicarbonate solution 3 times, respectively, wash with deionized water 3 times, separate the liquids, take the oil phase, distill under reduced pressure, and dry in a vacuum oven at 40°C for 24 hours to obtain the target product, i.e., the modified matting agent;
[0147] The intermediate product II and nonafluorovaleryl chloride are mixed in a molar ratio of secondary amine group to acyl chloride of 1:0.85;
[0148] The dosage ratio of the nonafluorovaleryl chloride, dichloromethane A, triethylamine, dichloromethane B, saturated saline, saturated sodium bicarbonate solution, and deionized water is: 0.1 mol: 100 mL: 0.1 mol: 300 mL: 500 mL: 500 mL: 500 mL.
[0149] Its infrared data is as follows: 3443cm -1 :-OH is weakened (slightly); 1560cm -1 : -NH peak weakened (significant); 1109cm -1 、801cm -1 :-Si-O- exists; 1628cm -1 :-C=C- exists; 1250cm -1 :-CF exists.
[0150] Example 3
[0151] The rest is the same as in Example 1, except that:
[0152] A method for preparing a modified matting agent comprises the following steps:
[0153] S11, adding silica and silane coupling agent KH550 to anhydrous ethanol, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 80° C. for 2 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I;
[0154] The usage ratio of the silicon dioxide, the silane coupling agent KH550 and the anhydrous ethanol is 1g:5.5g:80mL.
[0155] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists.
[0156] S12, adding the intermediate product I and allyl glycidyl ether to N,N-dimethylformamide A, and stirring magnetically at 60° C. for 2 h; after the reaction, cooling to room temperature, filtering, washing with N,N-dimethylformamide B, and drying the insoluble matter under vacuum at 50° C. to constant weight, to obtain the intermediate product II;
[0157] The intermediate product I and allyl glycidyl ether are added in a molar ratio of amino group to epoxy group of 1:1;
[0158] The usage ratio of allyl glycidyl ether, N,N-dimethylformamide A and N,N-dimethylformamide B is 1 mol:400 mL:500 mL.
[0159] Its infrared data is as follows: 3443cm -1 :-OH exists; 1560cm -1 :-NH peak weakened; 1109cm -1 、801cm -1 :-Si-O- exists; 1262cm -1 、927cm -1 、794cm -1 : Epoxy group does not exist; 1628cm -1 :-C=C- exists.
[0160] S13, protect from light, dissolve nonafluorovaleryl chloride and dichloromethane A in a constant pressure dropping funnel, add dropwise to dichloromethane B containing intermediate II and triethylamine, stir magnetically, ice bath, react at 5°C for 5 hours; let stand, stir overnight, filter, take the filtrate, wash with saturated salt water and saturated sodium bicarbonate solution 3 times, respectively, wash with deionized water 3 times, separate the liquids, take the oil phase, distill under reduced pressure, and dry in a vacuum oven at 40°C for 24 hours to obtain the target product, i.e., the modified matting agent;
[0161] The intermediate product II and nonafluorovaleryl chloride are mixed in a molar ratio of secondary amine group to acyl chloride of 1:0.85;
[0162] The dosage ratio of the nonafluorovaleryl chloride, dichloromethane A, triethylamine, dichloromethane B, saturated saline, saturated sodium bicarbonate solution, and deionized water is: 0.1 mol: 100 mL: 0.1 mol: 300 mL: 500 mL: 500 mL: 500 mL.
[0163] Its infrared data is as follows: 3443cm -1 :-OH is weakened (slightly); 1560cm -1 : -NH peak weakened (significant); 1109cm -1 、801cm -1 :-Si-O- exists; 1628cm -1 :-C=C- exists; 1250cm -1 :-CF exists.
[0164] Example 4
[0165] The rest is the same as in Example 1, except that:
[0166] A method for preparing a modified matting agent, wherein in step S13, nonafluorovaleryl chloride is replaced with heptafluorobutyryl chloride; and the heptafluorobutyryl chloride is added in an amount of 1:1 molar ratio to the secondary amino group in the intermediate product II.
[0167] Example 5
[0168] The rest is the same as in Example 1, except that:
[0169] A method for preparing a modified matting agent, wherein in step S13, nonafluoropentanoyl chloride is replaced with perfluorooctanoyl chloride; and the amount of perfluorooctanoyl chloride is added at a molar ratio of 0.7:1 to the secondary amino group in the intermediate product II.
[0170] Example 6
[0171] The rest is the same as in Example 1, except that:
[0172] A method for preparing a modified matting agent, wherein in step S13, nonafluoropentanoyl chloride is replaced with heptadecafluorononanoyl chloride; and the heptadecafluorononanoyl chloride is added in an amount with a molar ratio of 0.6:1 to the secondary amino group in the intermediate product II.
[0173] Example 7
[0174] The rest is the same as in Example 1, except that:
[0175] A super matte high hardness co-extruded fabric for wood plastic, comprising the following raw materials in parts by weight:
[0176] HDPE 80 parts;
[0177] PP 6 copies;
[0178] 5 parts of straw powder;
[0179] 0.2 parts of di-tert-butyl peroxide;
[0180] 3.0 parts of modified matting agent;
[0181] 2.0 parts of talcum powder;
[0182] Maleic anhydride grafted PE 2.0 parts;
[0183] Antioxidant 1098 0.5 parts;
[0184] Light stabilizer UV-770 0.2 parts;
[0185] 0.3 parts of erucamide wax.
[0186] A method for preparing an ultra-matte high-hardness co-extruded fabric for wood-plastic composites comprises the following steps:
[0187] S21, mixing, i.e.
[0188] Add the raw materials into a mixer according to the proportion and mix them. Mix them at a high speed of 105° C. and 150 rpm for 20 minutes. After mixing evenly, cool and discharge the materials for later use.
[0189] S22, granulation, i.e.
[0190] The mixed raw materials in S1 were placed in an extruder for melt blending, extrusion and granulation. The barrel temperature was set to 180°C in zone 1, 190°C in zone 2, 200°C in zone 3 and 200°C in zone 4, and the screw speed was 200 rpm to obtain a co-extruded fabric.
[0191] Example 8
[0192] The rest is the same as in Example 1, except that:
[0193] A super matte high hardness co-extruded fabric for wood plastic, comprising the following raw materials in parts by weight:
[0194] HDPE 90 parts;
[0195] PP 10 copies;
[0196] 10 parts of straw powder;
[0197] 1.0 part of di-tert-butyl peroxide;
[0198] 5.0 parts of modified matting agent;
[0199] 4.0 parts of talcum powder;
[0200] Maleic anhydride grafted PE 4.0 parts;
[0201] Antioxidant 1098 1.0 part;
[0202] Light stabilizer UV-770 0.5 parts;
[0203] 0.6 parts of erucamide wax.
[0204] A method for preparing an ultra-matte high-hardness co-extruded fabric for wood-plastic composites comprises the following steps:
[0205] S21, mixing, i.e.
[0206] Add the raw materials into a mixer according to the proportion and mix them. Mix them at a high speed of 125° C. and 80 rpm for 10 minutes. After mixing evenly, cool and discharge the materials for later use.
[0207] S22, granulation, i.e.
[0208] The mixed raw materials in S1 were placed in an extruder for melt blending, extrusion and granulation. The barrel temperature was set to 180°C in zone 1, 185°C in zone 2, 190°C in zone 3 and 190°C in zone 4. The screw speed was 300 rpm to obtain a co-extruded fabric.
[0209] Example 9
[0210] The rest is the same as in Example 1, except that:
[0211] A super matte high hardness co-extruded fabric for wood plastic, comprising the following raw materials in parts by weight:
[0212] HDPE 85 parts;
[0213] PP 6 copies;
[0214] 7 parts of straw powder;
[0215] 0.6 part of di-tert-butyl peroxide;
[0216] 4.2 parts of modified matting agent;
[0217] 3.0 parts of talcum powder;
[0218] Maleic anhydride grafted PE 3.0 parts;
[0219] Antioxidant 1098 0.8 parts;
[0220] Light stabilizer UV-770 0.3 parts;
[0221] 0.4 parts of erucamide wax.
[0222] Example 10
[0223] The rest is the same as in Example 1, except that:
[0224] A super matte high hardness co-extruded fabric for wood plastic, comprising the following raw materials in parts by weight:
[0225] HDPE 85 parts;
[0226] PP 10 copies;
[0227] 7 parts of straw powder;
[0228] 0.6 part of di-tert-butyl peroxide;
[0229] 4.2 parts of modified matting agent;
[0230] 3.0 parts of talcum powder;
[0231] Maleic anhydride grafted PE 3.0 parts;
[0232] Antioxidant 1098 0.8 parts;
[0233] Light stabilizer UV-770 0.3 parts;
[0234] 0.4 parts of erucamide wax.
[0235] Embodiment 11
[0236] The rest is the same as in Example 1, except that:
[0237] A super matte high hardness co-extruded fabric for wood plastic, comprising the following raw materials in parts by weight:
[0238] HDPE 85 parts;
[0239] PP 8 parts;
[0240] 7 parts of straw powder;
[0241] 0.6 part of di-tert-butyl peroxide;
[0242] 3.0 parts of modified matting agent;
[0243] 3.0 parts of talcum powder;
[0244] Maleic anhydride grafted PE 3.0 parts;
[0245] Antioxidant 1098 0.8 parts;
[0246] Light stabilizer UV-770 0.3 parts;
[0247] 0.4 parts of erucamide wax.
[0248] Example 12
[0249] The rest is the same as in Example 1, except that:
[0250] An ultra-matte high-hardness co-extruded fabric for wood-plastic composites comprises the following raw materials in parts by weight: 85 parts of HDPE;
[0251] PP 8 parts;
[0252] 7 parts of straw powder;
[0253] 0.6 part of di-tert-butyl peroxide;
[0254] 5.0 parts of modified matting agent;
[0255] 3.0 parts of talcum powder;
[0256] Maleic anhydride grafted PE 3.0 parts;
[0257] Antioxidant 1098 0.8 parts;
[0258] Light stabilizer UV-770 0.3 parts;
[0259] 0.4 parts of erucamide wax.
[0260] The following comparative examples are compared with specific embodiment 1:
[0261] Comparative Example 1
[0262] The rest is the same as in Example 1, except that:
[0263] An ultra-matte high-hardness co-extruded fabric for wood-plastic composites comprises the following raw materials in parts by weight: 85 parts of HDPE;
[0264] PP 8 parts;
[0265] 7 parts of straw powder;
[0266] 0.6 part of di-tert-butyl peroxide;
[0267] 3.0 parts of talcum powder;
[0268] Maleic anhydride grafted PE 3.0 parts;
[0269] Antioxidant 1098 0.8 parts;
[0270] Light stabilizer UV-770 0.3 parts;
[0271] 0.4 parts of erucamide wax.
[0272] Comparative Example 2
[0273] The rest is the same as in Example 1, except that:
[0274] An ultra-matte high-hardness co-extruded fabric for wood-plastic composites comprises the following raw materials in parts by weight: 85 parts of HDPE;
[0275] PP 8 parts;
[0276] 7 parts of straw powder;
[0277] 0.6 part of di-tert-butyl peroxide;
[0278] 4.2 parts of silicon dioxide;
[0279] 3.0 parts of talcum powder;
[0280] Maleic anhydride grafted PE 3.0 parts;
[0281] Antioxidant 1098 0.8 parts;
[0282] Light stabilizer UV-770 0.3 parts;
[0283] 0.4 parts of erucamide wax.
[0284] Comparative Example 3
[0285] The rest is the same as in Example 1, except that:
[0286] The preparation method of a modified matting agent is the same as the intermediate product II in specific embodiment 1.
[0287] Comparative Example 4
[0288] The rest is the same as in Example 1, except that:
[0289] A method for preparing a modified matting agent comprises the following steps:
[0290] S11, adding silica and silane coupling agent KH550 to anhydrous ethanol, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 70° C. for 4 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I;
[0291] The usage ratio of the silicon dioxide, the silane coupling agent KH550 and the anhydrous ethanol is 1g:4.5g:80mL.
[0292] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH peak exists; 1109cm -1 、801cm -1 :-Si-O- exists.
[0293] S12, dissolving nonafluorovaleryl chloride and dichloromethane A in a constant pressure dropping funnel, and dropping into dichloromethane B containing intermediate product I and triethylamine, and reacting for 10 hours under magnetic stirring, ice bath, and 0°C; standing, stirring overnight, filtering, taking the filtrate, washing with saturated saline and saturated sodium bicarbonate solution for 3 times, and then washing with deionized water for 3 times, separating the liquids, taking the oil phase, and distilling under reduced pressure, and drying in a vacuum oven at 40°C for 24 hours to obtain the target product, i.e., the modified matting agent;
[0294] The intermediate product II and nonafluorovaleryl chloride are mixed in a molar ratio of amine group to acyl chloride of 1:0.8;
[0295] The dosage ratio of the nonafluorovaleryl chloride, dichloromethane A, triethylamine, dichloromethane B, saturated saline, saturated sodium bicarbonate solution, and deionized water is: 0.1 mol: 100 mL: 0.1 mol: 300 mL: 500 mL: 500 mL: 500 mL.
[0296] Its infrared data is as follows: 3438cm -1 :-OH exists; 1560cm -1 : -NH peak weakened (significant); 1109cm -1 、801cm-1 :-Si-O- exists; 1250cm -1 :-CF exists.
[0297] Comparative Example 5
[0298] The rest is the same as in Example 1, except that:
[0299] A method for preparing a modified matting agent, wherein the nonafluorovaleryl chloride in step S13 is mixed at a molar ratio of 0.85:1 to the active hydrogen in the intermediate product II;
[0300] The active hydrogen in the intermediate product II is a secondary amino group and a secondary hydroxyl group.
[0301] Comparative Example 6
[0302] The rest is the same as in Example 1, except that:
[0303] An ultra-matte high-hardness co-extruded fabric for wood-plastic composites comprises the following raw materials in parts by weight: 85 parts of HDPE;
[0304] 7 parts of straw powder;
[0305] 0.6 part of di-tert-butyl peroxide;
[0306] 4.2 parts of modified matting agent;
[0307] 3.0 parts of talcum powder;
[0308] Maleic anhydride grafted PE 3.0 parts;
[0309] Antioxidant 1098 0.8 parts;
[0310] Light stabilizer UV-770 0.3 parts;
[0311] 0.4 parts of erucamide wax.
[0312] Comparative Example 7
[0313] The rest is the same as in Example 1, except that:
[0314] An ultra-matte high-hardness co-extruded fabric for wood-plastic composites comprises the following raw materials in parts by weight: 85 parts of HDPE;
[0315] PP 8 parts;
[0316] 0.6 part of di-tert-butyl peroxide;
[0317] 4.2 parts of modified matting agent;
[0318] 3.0 parts of talcum powder;
[0319] Maleic anhydride grafted PE 3.0 parts;
[0320] Antioxidant 1098 0.8 parts;
[0321] Light stabilizer UV-770 0.3 parts;
[0322] 0.4 parts of erucamide wax.
[0323] Comparative Example 8
[0324] The rest is the same as in Example 1, except that:
[0325] An ultra-matte high-hardness co-extruded fabric for wood-plastic composites comprises the following raw materials in parts by weight: 85 parts of HDPE;
[0326] PP 8 parts;
[0327] 7 parts of straw powder;
[0328] 4.2 parts of modified matting agent;
[0329] 3.0 parts of talcum powder;
[0330] Maleic anhydride grafted PE 3.0 parts;
[0331] Antioxidant 1098 0.8 parts;
[0332] Light stabilizer UV-770 0.3 parts;
[0333] 0.4 parts of erucamide wax.
[0334] Comparative Example 9
[0335] The rest is the same as Example 1, except that the erucamide wax is replaced by PE wax.
[0336] The physical properties of the super matte high hardness co-extruded fabrics for wood-plastics of Examples 1-12 of the present invention and Comparative Examples 1-9 were measured respectively, and the results are shown in Table 1.
[0337] Table 1 Physical test performance of each embodiment
[0338]
[0339] First, it can be observed from Examples 1-12 in Table 1 that the super matte high hardness co-extruded fabric for wood-plastic composites of the present invention has excellent low gloss, high hardness, and also has excellent bonding performance with the core material.
[0340] It can be observed from Example 1 and Comparative Example 1 that the super matte high hardness co-extruded fabric for wood-plastic composites of the present invention uses a homemade modified matting agent, which has excellent matting effect, high hardness and high wear resistance, etc.; it can be observed from Example 1 and Comparative Example 2 that the homemade modified matting agent is an inorganic microsphere wrapped in an organic structure, which has excellent dispersibility, thereby greatly improving various properties; it can be observed from Example 1 and Comparative Example 3 that the homemade modified matting agent contains an appropriate amount of F element, which is enriched at the interface to improve the matting effect and wear resistance; it can be observed from Example 1 and Comparative Example 4 that the multi-functional double bonds of the homemade modified matting agent can further improve the matting effect and hardness; at the same time, it can be observed from Example 1 and Comparative Examples 1-4 that the homemade modified matting agent has a certain antioxidant effect; it can be observed from Example 1 and Comparative Example 5 that it contains a large amount of F element, which has certain advantages on surface properties, but it will also reduce the bonding strength with the core material at the interface.
[0341] It can be observed from Example 1 and Comparative Examples 6-7 that the ultra-matte high-hardness co-extruded fabric for wood-plastic composites of the present invention, compared with HDPE, the small molecular weight PP can improve the matte effect and increase the hardness to a certain extent; the role of plant fiber in the fabric can improve the bonding strength with the core material.
[0342] From Example 1 and Comparative Examples 8-9, it can be observed that the improvement of the crosslinking density of the ultra-matte high-hardness co-extruded fabric for wood-plastic composites of the present invention has a positive effect on the physical properties of the material, which is reflected in the improvement of hardness and wear resistance and aging resistance; polyamide wax plays an important role in material performance because PE wax has excellent compatibility in the PE system, and its external lubricating effect is reduced, which affects the surface properties of the product.
[0343] In summary, the super matte high hardness co-extruded fabric for wood-plastic composite material of the present invention has excellent low gloss and high hardness, and also has excellent bonding performance with the core material.
[0344] The test method is as follows:
[0345] (1) Appearance: Visually inspect the surface of the product to see if there are any scratches or graininess.
[0346] (2) Gloss: Tested according to the method described in GB / T 9754-2007.
[0347] (3) Shore hardness: Use a Shore hardness tester to test and read the value.
[0348] (4) Boiling test: Boil in water for 168 hours to verify the surface changes and the cracks and separation between the surface and the core material.
[0349] (5) Abrasion resistance: Tested according to the method described in GB / T 24508-2009.
[0350] (6) Weather resistance: Conduct artificial weathering test for 300 h continuously according to the procedure specified in Table 3A of GB / T 1865-2009.
[0351] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A super matte high hardness co-extruded fabric for wood plastic, characterized in that: Contains the following raw materials in parts by weight: HDPE 80-90 parts; PP 6-10 parts; 5-10 parts of plant fiber; Cross-linking agent 0.2-1.0 part; 3.0-5.0 parts of modified matting agent; 2.0-4.0 parts of inorganic filler; Compatibilizer 2.0-4.0 parts; Antioxidant 0.5-1.0 part; Light stabilizer 0.2-0.5 parts; Lubricant 0.3-0.6 parts; The preparation method of the modified matting agent comprises the following steps: S11, placing silicon dioxide and an aminosilane coupling agent in an alcohol solvent for silylation coupling reaction to obtain an intermediate product I; S12, subjecting the intermediate product I to a ring-opening reaction with an epoxide to obtain an intermediate product II; and S13, subjecting the intermediate product II to a substitution reaction with a fluoroalkyl acyl chloride to obtain a target product, i.e., a modified matting agent; The intermediate product I and the epoxy olefins are added in a molar ratio of amino group to epoxy group of 1:1; The intermediate product II and the fluoroalkyl acyl chloride are mixed in a molar ratio of secondary amine group to acyl chloride group of 1:0.6-1; The cross-linking agent is an organic peroxide; The epoxy olefins are allyl glycidyl ether, 1,2-epoxy-5-hexene, 1,2-epoxy-7-octene or 1,2-epoxy-9-decene; The fluoroalkyl chloride is heptafluorobutyryl chloride, nonafluoropentanoyl chloride, perfluorooctanoyl chloride or heptadecafluorononanoyl chloride.
2. The super matte high hardness co-extruded fabric for wood-plastic composite material according to claim 1, characterized in that: The silicon dioxide is micron-sized silicon dioxide; and The usage of the silicon dioxide, aminosilane coupling agent and alcohol solvent is 1g:3.3-5.5g:80mL.
3. The super matte high hardness co-extruded fabric for wood-plastic composite material according to claim 1, characterized in that: The HDPE has a melt index of 0.9-1.5 g / 10 min.
4. The super matte high hardness co-extruded fabric for wood-plastic composite material according to claim 1, characterized in that: The melt index of the PP is 8.0±2.5 g / 10 min.
5. The super matte high hardness co-extruded fabric for wood-plastic according to claim 1, characterized in that: The lubricant is polyamide wax.
Citation Information
Patent Citations
Super-wear-resistant wood-plastic co-extrusion composite material and preparation method thereof
CN111057385A